High-wear-resistant oil-resistant fireproof coating and preparation method thereof

By using polyurethane resin, silicon micropowder, aluminum hydroxide and other components in high wear-resistant oil-resistant fire-resistant coatings, combined with nanosilicon dioxide and self-healing microcapsules, the coating is insufficient adhesion and flexibility in high temperature or humid environments. The problem of this paper achieves better wear, oil and fire resistance, and extends the coating life.

CN118978853APending Publication Date: 2024-11-19SICHUAN FIRE RES INST OF MEM

Patent Information

Application Number
CN202411307542.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

High wear-resistant oil-resistant fire-resistant coatings reduce adhesion in high temperature or humid environments, resulting in peeling or cracking of the coating, insufficient flexibility, easy to produce cracks, affecting long-term protection effect.

Method used

Polyurethane resin or epoxy resin is used as the matrix, silicon micropowder, alumina or silicon carbide is used as wear-resistant filler, aluminum hydroxide, magnesium hydroxide or expanded graphite is used as fire retardant, fluoride or fluorosiloxane modified polymer provides oil resistance Elastic modifiers improve flexibility, nanosilica or nanoalumina acts as adhesion promoters, self-healing microcapsules achieve automatic repair, additives regulate rheology, and ensure uniformity and stability through low-speed stirring and high-speed dispersion. sex.

Benefits of technology

It significantly improves the adhesion and flexibility of the coating, prevents cracks, extends the service life of the coating, provides excellent wear, oil and fire resistance, and ensures safe performance under high temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978853A_ABST
    Figure CN118978853A_ABST
Patent Text Reader

Abstract

The invention provides a high-wear-resistance, oil-resistance and fire-retardant coating and a preparation method thereof, and relates to the field of high-wear-resistance, oil-resistance and fire-retardant coatings. The high-wear-resistant oil-resistant fireproof coating comprises 30-50% of polyurethane resin or epoxy resin serving as a base material and providing excellent chemical corrosion resistance and mechanical strength, and 15-25% of silica powder, aluminum oxide or silicon carbide serving as a wear-resistant filler and improving the wear resistance of a coating and prolonging the service life of the coating. According to the invention, the problem that the coating is peeled off or cracked due to insufficient adhesive force of the existing coating in a high-temperature or humid environment is successfully solved, and the nano silicon dioxide or nano aluminum oxide is introduced as an adhesive force accelerant, so that the coating forms a nano-scale adhesive layer on a smooth or difficult-to-adhere surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of highly wear-resistant, oil-resistant and fire-resistant coatings, and in particular to a highly wear-resistant, oil-resistant and fire-resistant coating and a preparation method thereof. Background Art

[0002] High wear-resistant, oil-resistant and fire-resistant coating is a coating material that can provide wear-resistant, oil-resistant and fire-resistant properties. It is often used on surfaces that require oil-resistant and fire-resistant protection, such as industrial equipment, petrochemical equipment, ships, and buildings. Its main components include polymer matrix, wear-resistant filler, fire retardant and oil barrier agent.

[0003] The preparation method generally includes the following steps: Select a suitable base resin as required, then add wear-resistant fillers to give the coating excellent wear resistance. At the same time, add fire retardants and oil-resistant materials to improve the fire resistance and oil resistance of the coating. Disperse the mixed raw materials evenly to ensure that the fillers, resins and additives are fully combined. Use a sand mill or high-speed stirring equipment for grinding to achieve good fluidity and dispersibility of the coating. The coating can be applied to the surface to be protected by spraying, brushing or dipping, and then naturally cured or heated to form a hard coating, providing excellent wear resistance, oil resistance and fire resistance.

[0004] Although highly wear-resistant, oil-resistant and fire-retardant coatings have demonstrated excellent performance in multiple application scenarios, there are still some deficiencies in the system. In high temperature or humid environments, the adhesion of the coating will be reduced, resulting in peeling or cracking of the coating. The coating is not flexible enough and is prone to cracks on some surfaces with deformation requirements, affecting its long-term protective effect. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a highly wear-resistant, oil-resistant and fire-retardant coating and a preparation method thereof, which solves the problem that the adhesion of the coating may be reduced, resulting in peeling or cracking of the coating; and solves the problem that the coating is not sufficiently flexible and cracks are easily generated on some surfaces with deformation requirements.

[0006] To achieve the above purpose, the present invention is implemented by the following technical scheme: a highly wear-resistant, oil-resistant and fire-retardant coating, comprising:

[0007] Polyurethane resin or epoxy resin: 30-50%, as the matrix material, providing excellent chemical corrosion resistance and mechanical strength;

[0008] Silicon powder, alumina or silicon carbide: 15-25%, as wear-resistant filler to improve the wear resistance of the coating and extend its service life;

[0009] Aluminum hydroxide, magnesium hydroxide or expanded graphite: 10-20%, as fire retardant, with fire retardant function, can form an isolation layer when exposed to high temperature;

[0010] Fluoride or fluorosilicone modified polymer: 5-15%, providing strong oil resistance, preventing grease penetration, and maintaining the stability of the coating;

[0011] Elastic modifier: 5-10%, used to improve the flexibility and crack resistance of the coating, so that the coating remains intact when subjected to stress or temperature changes;

[0012] Nano-silicon dioxide or nano-alumina: 1-5%, as a nano-scale adhesion promoter, it can improve the adhesion of the coating on smooth or difficult-to-attach surfaces by forming a nano-scale interfacial bonding layer;

[0013] Self-healing microcapsules: 1-3%, used for the automatic repair function of the coating. When it is subjected to microcracks or wear, it can release sealants to repair cracks and extend the life of the coating;

[0014] Additives: 1-5%, adjust the rheology of the coating and ensure the uniformity and stability of construction.

[0015] Preferably, the elastic modifier is polybutadiene, ethylene-propylene rubber or nano rubber particles, and the additive is a leveling agent, a dispersant or a defoaming agent.

[0016] Preferably, the nano rubber particles have a particle size of 20-50 nanometers, forming a nano-scale composite structure with the matrix resin to improve the impact resistance and fatigue resistance of the coating. The wear-resistant filler is silicon carbide, and its particle diameter is 10-30 microns, which can effectively improve the wear resistance and thermal stability of the coating under high temperature or high friction environment.

[0017] A method for preparing a highly wear-resistant, oil-resistant and fire-retardant coating comprises the following steps:

[0018] a. Preparation of base resin: Weigh 30-50% of polyurethane resin or epoxy resin as base material to ensure the mechanical strength and chemical corrosion resistance of the coating;

[0019] b. Preparation of wear-resistant filler: Select 15-25% silicon powder, alumina or silicon carbide as wear-resistant filler to improve the wear resistance of the coating and extend the service life of the coating;

[0020] c. Addition of fire retardant: Add 10-20% of aluminum hydroxide, magnesium hydroxide or expanded graphite as a fire retardant to make the coating have fire retardant function and can form an isolation layer under high temperature conditions;

[0021] d. Addition of oil-resistant ingredients: Add 5-15% of fluoride or fluorosilicone modified polymer to provide oil resistance to the coating and prevent grease penetration and damage;

[0022] e. Addition of elastic modifier: Add 5-10% of polybutadiene, ethylene-propylene rubber or nano rubber particles to improve the flexibility and crack resistance of the coating, ensuring that it remains intact when subjected to stress or temperature changes;

[0023] f. Addition of nano-adhesion promoter: Adding 1-5% of nano-silicon dioxide or nano-alumina as an adhesion promoter can improve the adhesion between the coating and the substrate, especially on smooth or difficult-to-attach surfaces;

[0024] g. Introduction of self-healing microcapsules: By introducing 1-3% of self-healing microcapsules, the coating can release sealants to repair cracks when it is micro-cracked or worn, thus extending the life of the coating;

[0025] h. Addition of additives: Add 1-5% additives, including leveling agent, dispersant, defoamer, to adjust the construction performance of the coating and ensure the uniformity and stability of the coating;

[0026] i. Low-speed stirring: Stir all the components in step ah at room temperature at a low speed of 300-500 rpm for 30 minutes to ensure that all components are evenly mixed;

[0027] j. High-speed dispersion: Use a high-speed disperser to disperse the mixture at 2000-3000 rpm for 20-30 minutes to ensure that the filler is fully dispersed in the matrix resin;

[0028] k. Preliminary curing: The dispersed coating is heated at 60-80°C for preliminary curing for 1-2 hours to preliminarily cure the mechanical properties of the coating;

[0029] 1. Cooling and storage: Allow the initially cured paint to cool naturally to room temperature and then package and store for use or direct construction.

[0030] Preferably, the nano-silicon dioxide has a particle size of 10-50 nanometers and acts as an adhesion promoter to significantly improve the adhesion performance of the coating.

[0031] Preferably, the self-healing microcapsules contain a low-temperature polymer sealant for effectively repairing cracks under low-temperature conditions, and the initial curing treatment can be adjusted to 90° C. according to construction requirements to accelerate the curing process.

[0032] Preferably, the dispersion process uses a bead mill to ensure the refinement and uniform dispersion of the filler. The fire retardant is expanded graphite, which forms a heat insulation layer through volume expansion under high temperature conditions, thereby improving the fire retardant performance of the coating.

[0033] Preferably, a photothermal responsive material is added to the coating, which can change its structure to form an additional protective layer when exposed to high temperature, and the dispersant is a polymer dispersant, which is used to improve the compatibility of the filler and the matrix resin.

[0034] The present invention provides a highly wear-resistant, oil-resistant and fire-resistant coating and a preparation method thereof. It has the following beneficial effects:

[0035] The present invention successfully solves the problem that the existing coatings have insufficient adhesion in high temperature or humid environments, resulting in peeling or cracking of the coating. By introducing nano-silicon dioxide or nano-alumina as an adhesion promoter, the coating forms a nano-scale bonding layer on a smooth or difficult-to-adhere surface, which greatly improves its adhesion. Polybutadiene, ethylene-propylene rubber or nano-rubber particles are added to the coating as an elastic modifier to enhance the flexibility of the coating, so that it can maintain structural stability when subjected to force or temperature changes, effectively prevent the generation of cracks, and extend the service life of the coating.

[0036] The present invention introduces self-healing microcapsules into the coating, so that the coating can automatically repair itself when it is subjected to microcracks or wear, thereby significantly improving the durability of the coating. Silicon micropowder, aluminum oxide or silicon carbide is used as wear-resistant filler, so that the coating still exhibits excellent wear resistance in high friction and high temperature environments. By adding fluoride or fluorosilicone modified polymer, the coating is given excellent oil resistance. The added fire retardant such as expanded graphite provides the coating with excellent fire retardant function, ensuring its safety performance under high temperature conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0038] The technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] like Figure 1 As shown, an embodiment of the present invention provides a highly wear-resistant, oil-resistant and fire-retardant coating, comprising:

[0040] Polyurethane resin or epoxy resin: 30-50%, as the matrix material, providing excellent chemical corrosion resistance and mechanical strength.

[0041] Silicon powder, alumina or silicon carbide: 15-25%, as wear-resistant filler to improve the wear resistance of the coating and extend its service life.

[0042] Aluminum hydroxide, magnesium hydroxide or expanded graphite: 10-20%, as fire retardants, with fire retardant functions, and can form an isolation layer when exposed to high temperatures.

[0043] Fluoride or fluorosilicone modified polymer: 5-15%, provide strong oil resistance, prevent grease penetration, and maintain the stability of the coating.

[0044] Elasticity modifier: 5-10%, used to improve the flexibility and crack resistance of the coating, so that the coating remains intact when subjected to force or temperature changes. The elasticity modifier is polybutadiene, ethylene-propylene rubber or nano rubber particles. The additives are leveling agents, dispersants, and defoaming agents. The nano rubber particles have a particle size of 20-50 nanometers and form a nano-scale composite structure with the matrix resin to improve the impact resistance and fatigue resistance of the coating. The wear-resistant filler is silicon carbide with a particle diameter of 10-30 microns, which can effectively improve the wear resistance and thermal stability of the coating under high temperature or high friction environments.

[0045] Nano-silicon dioxide or nano-alumina: 1-5%, as a nano-scale adhesion promoter, it can improve the adhesion of the coating on smooth or difficult-to-attach surfaces by forming a nano-scale interfacial bonding layer.

[0046] Self-healing microcapsules: 1-3%, used for the automatic repair function of the coating. When it is subjected to microcracks or wear, it can release sealants to repair cracks and extend the life of the coating.

[0047] Additives: 1-5%, adjust the rheology of the coating and ensure the uniformity and stability of construction.

[0048] A method for preparing a highly wear-resistant, oil-resistant and fire-retardant coating comprises the following steps:

[0049] a. Preparation of base resin: Weigh 30-50% of polyurethane resin or epoxy resin as the base material to ensure the mechanical strength and chemical corrosion resistance of the coating.

[0050] b. Preparation of wear-resistant fillers: Select 15-25% of silicon powder, alumina or silicon carbide as wear-resistant fillers to improve the wear resistance of the coating and extend the service life of the coating.

[0051] c. Addition of fire retardant: Add 10-20% aluminum hydroxide, magnesium hydroxide or expanded graphite as fire retardant to make the coating have fire retardant function and form an isolation layer under high temperature conditions. The fire retardant is expanded graphite, which forms a heat insulation layer by volume expansion under high temperature conditions, thereby improving the fire retardant performance of the coating. Photothermal responsive materials are added to the coating, which can change its structure to form an additional protective layer when exposed to high temperature. The dispersant is a polymer dispersant, which is used to improve the compatibility of the filler and the matrix resin.

[0052] d. Addition of oil-resistant ingredients: Add 5-15% of fluoride or fluorosilicone modified polymer to provide the coating with oil resistance and prevent grease penetration and damage.

[0053] e. Addition of elastic modifier: Add 5-10% of polybutadiene, ethylene-propylene rubber or nano rubber particles to improve the flexibility and crack resistance of the coating, ensuring that it remains intact when subjected to stress or temperature changes.

[0054] f. Addition of nano-adhesion promoter: Adding 1-5% of nano-silicon dioxide or nano-alumina as an adhesion promoter can improve the adhesion between the coating and the substrate, especially on smooth or difficult-to-attach surfaces. The particle size of nano-silicon dioxide is 10-50 nanometers. As an adhesion promoter, it significantly improves the adhesion performance of the coating.

[0055] g. Introduction of self-healing microcapsules: By introducing 1-3% of self-healing microcapsules, the coating can release sealants to repair cracks when it is micro-cracked or worn, thereby extending the life of the coating. The self-healing microcapsules contain low-temperature polymer sealants, which are used to effectively repair cracks under low temperature conditions. The initial curing treatment can be adjusted to 90°C according to construction requirements to speed up the curing process.

[0056] h. Addition of additives: Add 1-5% of additives, including leveling agent, dispersant, defoamer, to adjust the construction performance of the coating and ensure the uniformity and stability of the coating.

[0057] i. Low-speed stirring: Stir all the components in step ah at low speed at room temperature, with a stirring speed of 300-500 rpm for 30 minutes to ensure that all components are evenly mixed.

[0058] j. High-speed dispersion: Use a high-speed disperser to disperse the mixture at 2000-3000 rpm for 20-30 minutes to ensure that the filler is fully dispersed in the matrix resin. Bead milling equipment is used in the dispersion process to ensure the refinement and uniform dispersion of the filler.

[0059] k. Preliminary curing: Heat the dispersed coating at 60-80°C for preliminary curing for 1-2 hours to initially cure the mechanical properties of the coating.

[0060] 1. Cooling and storage: Allow the initially cured paint to cool naturally to room temperature and then package and store for use or direct construction.

[0061] Table 1: Data comparison table

[0062]

[0063]

[0064] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A highly wear-resistant, oil-resistant and fire-retardant coating, characterized in that: include: Polyurethane resin or epoxy resin: 30-50%, as matrix material; Silicon powder, alumina or silicon carbide: 15-25%, as wear-resistant filler; Aluminum hydroxide, magnesium hydroxide or expanded graphite: 10-20%, as fire retardant, with fire retardant function; Fluoride or fluorosilicone modified polymer: 5-15%, providing strong oil resistance and preventing grease penetration; Elastic modifier: 5-10%, used to improve the flexibility and crack resistance of the coating, so that the coating remains intact when subjected to stress or temperature changes; Nano-silicon dioxide or nano-alumina: 1-5%, as a nano-scale adhesion promoter, can form a nano-scale interface bonding layer; Self-healing microcapsules: 1-3%, used for the automatic repair function of the coating, which can release sealants to repair cracks when subjected to microcracks or wear; Additive: 1-5%, to adjust the rheology of the coating.

2. A highly wear-resistant, oil-resistant and fire-retardant coating according to claim 1, characterized in that: The elastic modifier is polybutadiene, ethylene-propylene rubber or nano rubber particles, and the additive is a leveling agent, a dispersant and a defoaming agent.

3. A highly wear-resistant, oil-resistant and fire-retardant coating according to claim 1, characterized in that: The nano rubber particles have a particle size of 20-50 nanometers and form a nano-scale composite structure with the matrix resin. The wear-resistant filler is silicon carbide, and the particle diameter is 10-30 micrometers.

4. A method for preparing a highly wear-resistant, oil-resistant and fire-retardant coating, characterized in that: The following steps are involved: a. Preparation of base resin: Weigh 30-50% of polyurethane resin or epoxy resin as base material to ensure the mechanical strength and chemical corrosion resistance of the coating; b. Preparation of wear-resistant filler: Select 15-25% silicon powder, alumina or silicon carbide as wear-resistant filler to improve the wear resistance of the coating and extend the service life of the coating; c. Addition of fire retardant: Add 10-20% of aluminum hydroxide, magnesium hydroxide or expanded graphite as a fire retardant to make the coating have fire retardant function and can form an isolation layer under high temperature conditions; d. Addition of oil-resistant ingredients: Add 5-15% of fluoride or fluorosilicone modified polymer to provide oil resistance to the coating and prevent grease penetration and damage; e. Addition of elastic modifier: Add 5-10% of polybutadiene, ethylene-propylene rubber or nano rubber particles to improve the flexibility and crack resistance of the coating, ensuring that it remains intact when subjected to stress or temperature changes; f. Addition of nano-adhesion promoter: Adding 1-5% of nano-silicon dioxide or nano-alumina as an adhesion promoter can improve the adhesion between the coating and the substrate, especially on smooth or difficult-to-attach surfaces; g. Introduction of self-healing microcapsules: By introducing 1-3% of self-healing microcapsules, the coating can release sealants to repair cracks when it is micro-cracked or worn, thus extending the life of the coating; h. Addition of additives: Add 1-5% additives, including leveling agent, dispersant, defoamer, to adjust the construction performance of the coating and ensure the uniformity and stability of the coating; i. Low-speed stirring: Stir all the components in step ah at room temperature at a low speed of 300-500 rpm for 30 minutes to ensure that all components are evenly mixed; j. High-speed dispersion: Use a high-speed disperser to disperse the mixture at 2000-3000 rpm for 20-30 minutes to ensure that the filler is fully dispersed in the matrix resin; k. Preliminary curing: The dispersed coating is heated at 60-80°C for preliminary curing for 1-2 hours to preliminarily cure the mechanical properties of the coating; 1. Cooling and storage: Allow the initially cured paint to cool naturally to room temperature and then package and store for use or direct construction.

5. The method for preparing a highly wear-resistant, oil-resistant and fire-retardant coating according to claim 4, characterized in that: The nano silicon dioxide has a particle size of 10-50 nanometers and acts as an adhesion promoter to significantly improve the adhesion performance of the coating.

6. The method for preparing a highly wear-resistant, oil-resistant and fire-retardant coating according to claim 4, characterized in that: The self-healing microcapsules contain a low-temperature polymer sealant for effectively repairing cracks under low-temperature conditions, and the initial curing treatment can be adjusted to 90° C. according to construction requirements.

7. The method for preparing a highly wear-resistant, oil-resistant and fire-retardant coating according to claim 4, characterized in that: The dispersion process uses a bead mill to ensure the refinement and uniform dispersion of the filler. The fire retardant is expanded graphite, which forms a heat insulation layer through volume expansion under high temperature conditions.

8. The method for preparing a highly wear-resistant, oil-resistant and fire-retardant coating according to claim 4, characterized in that: The photothermal responsive material is added to the coating, which can change its structure to form an additional protective layer when exposed to high temperature. The dispersant is a polymer dispersant, which is used to improve the compatibility of the filler and the matrix resin.

Citation Information

Patent Citations

  • Flexible epoxy intumescence fire-retardant coating and preparation method thereof

    CN105238221A

  • Fireproof coating for self-repairing type steel structure and preparation method thereof

    CN106221346A

  • Antifouling flame retardant coating and construction method thereof

    CN110387186A

  • Flame-retardant anticorrosive coating material for outdoor power equipment, and preparation method thereof

    CN110819201A

  • Degradable zinc-lithium alloy surface coating and preparation method and application thereof

    CN113855853A

Cited By

  • Light-cured putty and preparation method thereof

    CN121182257A

  • A photocuring putty and a preparation method thereof

    CN121182257B

  • Wear-resistant protective coating for cable sheath as well as preparation method and application of wear-resistant protective coating

    CN121249251A

  • Composite slurry, preparation method therefor, and use thereof

    WO2026137957A1