Preparation method of anticorrosive coating based on modified acrylic resin

Through the chemical modification and cross-linking reaction of modified polyacrylic resin and activated nano α-Al2O3, combined with azobisisobutyronitrile catalyzed double bond reaction, the problem of insufficient wear resistance and corrosion resistance of existing coatings is solved, and the problem of insufficient wear resistance and corrosion resistance of existing coatings is achieved. High-performance coatings that are wear-resistant, corrosion-resistant, UV-resistant and oxidative-resistant.

CN118978862AActive Publication Date: 2024-11-19JIANGMEN CAIGE ENVIRONMENTAL PROTECTION TECH IND

Patent Information

Application Number
CN202411225994.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-19
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

The wear resistance and corrosion resistance of existing acrylic resin coatings need to be improved, and the bonding force between nanoparticles and matrix resin is insufficient, resulting in the coating being easily peeled off during friction, poor bonding strength and wear resistance, and corrosion resistance. Inadequate ability.

Method used

Modified polyacrylic resin and activated nano α-Al2O3 are used to form corrosion-resistant and wear-resistant interpolymers through chemical modification and cross-linking reaction, combining azobisisobutyronitrile catalyzed double bond reaction to enhance the durability and chemical bonding of the coating. , using fluorinated allyl groups to reduce surface energy, 2-(2'-hydroxy-3',5'-di-tert-butylbenzotriazole provides UV resistance, S-(2-trimethoxysilylethyl ) Ethylsulfonate enhances antioxidant capacity.

Benefits of technology

It significantly improves the wear resistance, corrosion resistance, UV resistance and oxidation resistance of the coating, enhances the bonding force between the coating and the substrate, and forms a durable and high-performance anti-corrosion coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005024569790000021
    Figure BDA0005024569790000021
  • Figure BDA0005024569790000031
    Figure BDA0005024569790000031
  • Figure BDA0005024569790000041
    Figure BDA0005024569790000041
Patent Text Reader

Abstract

The invention discloses a preparation method of an anticorrosive coating based on modified acrylic resin, belongs to the technical field of coating processing, and aims to solve the technical problem that the wear resistance and corrosion resistance of an acrylic resin coating in the prior art need to be further improved. The preparation method comprises the following steps: preparing modified polyacrylic resin, carrying out anti-ultraviolet treatment on the modified polyacrylic resin to obtain a copolymer, preparing nano alpha-Al2O3, modifying the nano alpha-Al2O3, preparing a dispersion liquid, mixing the dispersion liquid and the copolymer for addition to obtain an anticorrosive coating, preparing a washing coating, and spraying and curing to obtain the anticorrosive coating. The water-based polyacrylic resin coating with excellent wear resistance, high binding force, high hardness, oxidation resistance and ultraviolet resistance is prepared by preparing modified acrylic resin and further modifying the modified acrylic resin to obtain a co-polymer and reacting the co-polymer with a dispersion liquid modified and prepared by nano alpha-Al2O3.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coating processing, and in particular to a method for preparing an anticorrosive coating based on modified acrylic resin. Background Art

[0002] Acrylic resin is a kind of polymer material made from acrylic acid and its ester monomers through free radical polymerization. It is widely used in coatings, adhesives and textiles. In terms of chemical synthesis, acrylic resin uses acrylic acid and its esters as basic monomers, forms polymer chains through polymerization reactions initiated by free radical initiators, and introduces different comonomers to adjust the mechanical properties, weather resistance and chemical stability of the resin.

[0003] In addition, the application of nanotechnology and high-performance fillers has further enhanced the hardness, wear resistance and chemical resistance of acrylic resins, making acrylic resin coatings widely used in the construction, automotive and electronics industries, becoming an indispensable and important material for modern industry.

[0004] In the prior art, patent application CN2021105536585 discloses a wear-resistant, high-adhesion super-hydrophobic coating and a preparation method thereof, wherein the coating adopts a solution polymerization process to prepare an epoxy-modified polyacrylate solution, and an aminosilane coupling agent and a fluorine-containing silane coupling agent are used to surface-treat micronized silica and nano-silica, respectively, to obtain amino-modified micronized silica and fluorine-modified nano-silica, and epoxy-modified polyacrylate, amino-modified micronized silica / epoxy-modified polyacrylate and fluorine-modified nano-silica / epoxy-modified polyacrylate coatings are sequentially coated on the surface of the substrate, and a super-hydrophobic coating is obtained after curing and cross-linking;

[0005] This method uses a layered coating method to obtain the coating. By simply compounding several coatings, it is difficult for the coatings to achieve a mutually reinforcing effect. In addition, the document only uses a silane coupling agent to modify the surface of the nanoparticles. The bonding strength between the obtained nanomaterials and the matrix resin needs to be improved. The nanoparticles are easy to fall off during the friction process. The bonding strength and wear resistance of the coating are poor. In addition, the matrix resin is only epoxidized, and its corrosion resistance needs to be further improved.

[0006] In view of the technical defects in this aspect, a solution is now proposed. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing an anti-corrosion coating based on a modified acrylic resin, so as to solve the technical problem that the wear resistance and corrosion resistance of the acrylic resin coating in the prior art need to be further improved.

[0008] The purpose of the present invention can be achieved by the following technical scheme: A method for preparing an anticorrosive coating based on a modified acrylic resin, comprising the following steps:

[0009] S1, adding modified polyacrylic acid resin, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-benzotriazole, triethylamine and dimethyl sulfoxide into a reaction kettle, raising the temperature of the reaction kettle to 155-175° C., keeping the temperature for reaction for 1-3 hours, and post-treating to obtain a copolymer;

[0010] The copolymer synthesis equation is:

[0011]

[0012] Principle of copolymer synthesis reaction: Under weak alkaline conditions, the hydroxyl group (-OH) of 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-benzotriazole and the epoxy group in the modified polyacrylic acid resin undergo a ring-opening reaction, and 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-benzotriazole and the modified polyacrylic acid resin are polymerized through ether bonds, and the anti-UV group is modified on the outside of the modified polyacrylic acid resin and a hydroxyl group is introduced to prepare a copolymer.

[0013] S2, adding activated nano-α-Al2O3, S-(2-trimethoxysilylethyl)ethanesulfonate, isocyanate methyltrimethoxysilane, N,N-dimethylformamide and triethylamine into a reaction kettle, reacting at room temperature for 2-4 hours to obtain alkylated nano-α-Al2O3;

[0014] Reaction equation:

[0015]

[0016] Reaction principle: Under weak alkaline conditions, the ethoxy (-OCH2CH3) groups of S-(2-trimethoxysilylethyl) ethanesulfonate and isocyanate methyltrimethoxysilane will be hydrolyzed and react with the active oxygen-containing groups on the surface of modified nano-α-Al2O3 to form silicon-oxygen bonds, thereby achieving cross-linking between particles and preparing alkylated nano-α-Al2O3.

[0017] S3, adding the copolymer and the dispersion into a reactor, raising the temperature of the reactor to 160-180°C, keeping the temperature and stirring for 1-2h, and post-treating to obtain a modified copolymer;

[0018] Modified copolymer synthesis reaction equation:

[0019]

[0020] Principle of the modified copolymer synthesis reaction: Under heating conditions, the hydroxyl group (-OH) in the copolymer will react with the isocyanate group (-NCO) in the activated nanomaterial, and the nanomaterial will be modified on the copolymer through urethane bonding to prepare a thermoplastic coating.

[0021] S4, preparing an anticorrosive coating using the modified copolymer, deionized water, dimethyl sulfoxide and an auxiliary agent;

[0022] S5. Use a spray gun to spray the anti-corrosion coating on the substrate to form an anti-corrosion coating with a thickness of 15-20 mm on the surface of the substrate.

[0023] Furthermore, in step S1, the preparation method of the modified polyacrylic acid resin comprises the following steps:

[0024] A1, add glycidyl methacrylate, allyl fluoride, 9,10-epoxy-1,5-cyclododecadiene and N,N-dimethylformamide into a reaction kettle, and stir at room temperature for 15-20 minutes to obtain a reaction precursor solution;

[0025] A2. Add the reaction precursor liquid and azobisisobutyronitrile into the reactor, increase the temperature of the reactor to 80-100° C., keep the temperature for 2-4 hours, and perform post-treatment to obtain a modified acrylic resin.

[0026] Modified acrylic resin synthesis reaction equation:

[0027]

[0028] Principle of the synthetic reaction of modified acrylic resin: Under the action of azobisisobutyronitrile, the double bonds of glycidyl methacrylate, allyl fluoride, and 9,10-epoxy-1,5-cyclododecadiene undergo free radical polymerization to form a copolymer.

[0029] Furthermore, in step A1, the amount ratio of glycidyl methacrylate, allyl fluoride, 9,10-epoxy-1,5-cyclododecadiene and N,N-dimethylformamide is 3-5g:1-2g:6-8g:40-50mL, and the stirring rate is 120-180rpm; in step A2, the amount ratio of the reaction precursor liquid and azobisisobutyronitrile is 40-50mL:0.5-0.8g, and the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added to a rotary evaporator with a water bath temperature of 60-80°C, and distilled under reduced pressure until no liquid is produced to obtain a modified acrylic resin.

[0030] Furthermore, in step S1, the amount ratio of modified polyacrylic acid resin, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-benzotriazole, triethylamine and dimethyl sulfoxide is 3-5g:1-2g:0.2-0.5g:20-25mL, and the post-treatment includes: after the reactor is cooled to room temperature, the reaction solution is added to a rotary evaporator with a water bath temperature of 60-100°C, and distilled under reduced pressure until no liquid is extracted to obtain a copolymer.

[0031] Furthermore, in step S2, the preparation method of activated nano α-Al2O3 comprises the following steps:

[0032] B1. Add 0.05-0.15 mol / L aluminum nitrate solution into the reaction kettle, and adjust the pH value of the solution system to 8.5-9.5 with saturated ammonia water while stirring at room temperature to obtain a reaction precursor solution;

[0033] B2. Add the reaction precursor solution into a magnetic stirrer, stir at room temperature for 6-8 hours, let it stand for 24 hours after stirring, and post-treat to obtain a gel;

[0034] Reaction principle: Under weak alkaline conditions, aluminum ions (Al 3+ ) will react with the hydroxide ions (OH - ) react to form aluminum hydroxide colloid, which is composed of extremely small clusters and aggregates and can form a stable dispersed system in the solution. Shear force is introduced during stirring, which reduces the distance between the colloid particles and weakens the repulsive effect between the charges, thereby promoting the coagulation and aggregation between the colloid particles and forming a larger colloid structure.

[0035] B3. Crush the gel, sieve it to obtain gel powder, and then post-treat it to obtain activated nano-α-Al2O3.

[0036] Reaction principle: In the initial stage, the aluminum hydroxide in the colloidal powder will undergo a dehydration reaction at about 200°C and convert into aluminum oxide. This process is achieved by releasing water molecules. As the temperature continues to rise to above 400°C, the crystal phase of aluminum oxide begins to change, and the most stable crystal phase α-Al2O3 is generated at about 600°C. The temperature increase at this stage is conducive to the rearrangement of crystals and the crystal growth of particles.

[0037] At high temperatures, the alumina particles gradually grow into nano-α-Al2O3 through the rearrangement of crystals and the combination of particles. Under high temperature conditions, water vapor (H2O) can dissociate into hydroxide ions (OH - ) and hydrogen ions (H + ), dissociated hydroxide ions (OH -) can react with the surface of nano-alumina, and water vapor can react with aluminum ions and oxygen vacancies on the surface to form hydroxyl groups.

[0038] Further, in step B1, the stirring rate is 120-180 rpm; in step B2, the stirring rate is 240-360 rpm, and the post-treatment includes: after standing, filtering to obtain a gel; in step B3, the post-treatment includes: after the gel powder is moved to a tubular heating furnace, the tubular heating furnace is heated to 1100±10°C at a rate of 10°C / min, kept warm for 6-8h, naturally cooled to 300-600°C, and heated at 0.1-0.5m 3 Water vapor is introduced at a rate of / h, and after keeping warm for 4-6 hours, it is naturally cooled to obtain activated nano α-Al2O3.

[0039] Furthermore, in step S2, the amount ratio of activated nano α-Al2O3, S-(2-trimethoxysilylethyl)ethanesulfonate, isocyanate methyltrimethoxysilane, N,N-dimethylformamide and triethylamine is 5-8g:3-5g:3-5g:40-50mL:0.5-1g, and the post-treatment includes: after the reaction is completed, collecting the filter cake by suction filtration, placing the filter cake in a drying oven at a temperature of 80°C and vacuum drying it until the filter cake has a constant weight, thereby obtaining alkylated nano α-Al2O3.

[0040] Furthermore, in step S3, the amount ratio of the copolymer and the dispersion is 3-5g:15-20mL, the stirring rate is 60-80rpm, and the dispersion is prepared by mixing alkylated nano-α-Al2O3, dimethyl sulfoxide, deionized water, polyvinyl pyrrolidone and sodium dodecylbenzene sulfonate in an amount ratio of 15-20g:50mL:150mL:2-5g:1-3g. The post-treatment includes: after the reactor is cooled to room temperature, the reaction solution is added to a rotary evaporator with a water bath temperature of 80-100°C, and reduced pressure distillation is performed until no liquid is extracted to obtain a modified copolymer.

[0041] Further, in step S4, the amount ratio of the modified copolymer, deionized water, dimethyl sulfoxide and auxiliary agent is 5-8g:10-15mL:5-10mL:0.5-0.6g; the auxiliary agent includes the following components in parts by weight: 5-20 parts of dispersant, 3-10 parts of stabilizer, 10-30 parts of filler, 5-10 parts of leveling agent and 5-10 parts of anti-sticking agent, the dispersant is one or more of polyvinyl alcohol, sodium polyacrylate, and polyvinyl ether, the stabilizer is one or more of polyoxyethylene ether, dodecyl polyoxyethylene ether and fatty alcohol polyoxyethylene ether, the filler is one or more of silicon dioxide powder, calcium carbonate powder and aluminum oxide powder, the leveling agent is one or more of polydimethylsiloxane, polymethylsiloxane and polyvinyl siloxane, and the anti-sticking agent is one or more of polyvinyl alcohol, polyethylene glycol and polypropylene glycol.

[0042] Further, in step S4, the spraying operation is as follows: in step S4, the spraying operation is as follows: select a spray gun with a nozzle diameter of 1.2-1.4 mm, a spraying pressure of 40-50 psi, a distance of 20-30 cm between the spray gun and the substrate, a spray gun movement speed of 40-60 cm / min, a coating thickness of 15-20 mm, and after spraying, place the material in an oven at a temperature of 20-25°C and a relative humidity of 30-50% to dry for 2-4 hours, and after drying, cure at room temperature for 24 hours to obtain a material with a surface coated with a modified acrylic resin coating.

[0043] The present invention has the following beneficial effects:

[0044] 1. In the process of preparing an anti-corrosion coating based on modified acrylic resin, the present invention first uses glycidyl acrylate, allyl fluoride, and 9,10-epoxy-1,5-cyclododecadiene to synthesize a multifunctional modified polyacrylate through free radical polymerization, and then the modified acrylic resin is surface-modified to obtain a copolymer; nano α-Al2O3 is prepared to provide support for the coating, and then its surface is modified to obtain an activated nano material, and a dispersion is further prepared; finally, the copolymer and the dispersion are synergistically coordinated through chemical reactions to obtain a corrosion-resistant, wear-resistant, UV-resistant and antioxidant water-based coating based on modified acrylic resin.

[0045] 2. In the process of preparing the copolymer of the present invention, azobisisobutyronitrile is used to catalyze the cleavage of double bonds of glycidyl methacrylate, allyl fluoride, and 9,10-epoxy-1,5-cyclododecadiene to produce a free radical addition reaction. The double bonds of glycidyl methacrylate provide reaction activity and epoxy groups at the same time, and cooperate with the epoxy groups of 9,10-epoxy-1,5-cyclododecadiene to form a strong chemical bond with the surface of the substrate, thereby enhancing the durability, stability and corrosion resistance of the material. At the same time, the cyclic multi-double bond structure of 9,10-epoxy-1,5-cyclododecadiene optimizes the spatial structure of the polyacrylic resin while enhancing the rigidity of the modified acrylic resin. ; The fluorine group of the fluorinated allyl group provides excellent chemical resistance and corrosion resistance while reducing the surface energy of the coating; further, the epoxy group in the modified polyacrylic resin undergoes a ring-opening reaction with the hydroxyl group of 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-benzotriazole to form a copolymer, and 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-benzotriazole provides UV resistance to the copolymer, while the internal benzene ring cooperates with the cyclic structure of 9,10-epoxy-1,5-cyclododecadiene to enhance the rigidity of the copolymer, and the hydroxyl group produced by the ring-opening reaction also provides a basis for subsequent reactions, ultimately obtaining a corrosion-resistant and UV-resistant copolymer.

[0046] 3. In the process of preparing the dispersion liquid, the present invention firstly stirs an aluminum nitrate solution under alkaline conditions to produce a colloid, and then calcines the colloid at a high temperature to obtain an activated nano α-Al2O3 material with a surface rich in hydroxyl groups; the nano α-Al2O3 is a metal oxide, and its structure is a hexagonal close-packed body, the lattice energy is large, and it has excellent physical and chemical properties. The material has strong intermolecular cohesion, dense structure, perfect crystals, and the ability to resist various chemical changes, which can provide the coating with chemical stability and corrosion resistance while also enhancing its wear resistance; further, the ethoxy group of S-(2-trimethoxysilylethyl)ethanesulfonate and isocyanatemethyltrimethoxysilane is used in a weak base to Under the condition of high temperature, the modified nano-α-Al2O3 reacts with the hydroxyl group on the surface of the modified nano-α-Al2O3. The alkylation reaction further improves the binding ability of the nano-α-Al2O3 and the copolymer. The thio group of S-(2-trimethoxysilylethyl)ethanesulfonate further improves the antioxidant capacity of the coating. The isocyanate group of isocyanatemethyltrimethoxysilane also provides active groups for further reactions. Finally, a surfactant and the surface-modified nano-α-Al2O3 are used to prepare a dispersion. The surfactant reduces the agglomeration of nano-α-Al2O3 and provides favorable conditions for its binding with the copolymer. Finally, a synergistic combination with the copolymer is obtained to improve the wear resistance and antioxidant capacity of the coating. DETAILED DESCRIPTION

[0047] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] Example 1

[0049] This embodiment provides a method for preparing a modified acrylic resin anticorrosive coating, comprising the following steps:

[0050] S1. Preparation of copolymer

[0051] Weigh 60.3 g of glycidyl methacrylate, 20.1 g of allyl fluoride, 90.3 g of 9,10-epoxy-1,5-cyclododecadiene and 850.3 mL of N,N-dimethylformamide, add them into a reaction kettle, stir at room temperature for 15 min at a stirring rate of 120 rpm to obtain a reaction precursor solution;

[0052] 800 mL of reaction precursor solution and 12.1 g of azobisisobutyronitrile were weighed and added to a reactor. The temperature of the reactor was raised to 80° C. and the reaction was kept warm for 2 h. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 60° C. and distilled under reduced pressure until no liquid was produced, to obtain 152.1 g of modified polyacrylic acid resin;

[0053] 150.0 g of modified polyacrylic acid resin, 50.2 g of 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-benzotriazole, 25.0 g of triethylamine and 1.2 L of dimethyl sulfoxide were added to a reactor, the temperature of the reactor was raised to 155°C, and the reaction was kept warm for 1 hour. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 60°C, and distilled under reduced pressure until no liquid was produced, to obtain 195.7 g of a copolymer.

[0054] S2. Preparation of alkylated nano-α-Al2O3

[0055] 5 L of 0.05 mol / L aluminum nitrate solution was added to the reaction kettle, and the pH of the solution system was adjusted to 8.5 with saturated ammonia water while stirring at room temperature, and the stirring rate was 120 rpm to obtain a reaction precursor solution;

[0056] The reaction precursor solution was added into a magnetic stirrer, stirred at room temperature for 6 h at a stirring rate of 240 rpm, and allowed to stand for 24 h after the stirring was completed. After the standing was completed, the gel was filtered to obtain a gel;

[0057] The gel was crushed and sieved to obtain gel powder. The gel powder was moved to a tubular heating furnace and nitrogen was introduced for protection. The tubular heating furnace was heated to 1090°C at a rate of 10°C / min, kept warm for 6 hours, cooled naturally to 300°C, and heated at 0.1m 3 Water vapor was introduced at a rate of / h, and after keeping warm for 4h, it was naturally cooled to obtain 25.3g of activated nano-α-Al2O3;

[0058] 24.0 g activated nano α-Al2O3, 19.2 g S-(2-trimethoxysilylethyl) ethanesulfonate, 19.2 g isocyanate methyltrimethoxysilane, 195.3 mL N,N-dimethylformamide and 3.6 g triethylamine were added to the reactor and reacted at room temperature for 2 h. After the reaction was completed, the filter cake was collected by filtration and placed in a drying oven at 80°C for vacuum drying until the filter cake had a constant weight, to obtain 60.1 g alkylated nano α-Al2O3.

[0059] S3. Preparation of modified copolymer

[0060] Weigh 50.0 g of alkylated nano-α-Al2O3, 138.3 mL of dimethyl sulfoxide, 416.6 mL of deionized water, 8.3 g of polyvinyl pyrrolidone and 4.2 g of sodium dodecylbenzene sulfonate and mix to prepare a dispersion;

[0061] 150 g of copolymer and 450 mL of dispersion were weighed and added to the reactor. The temperature of the reactor was raised to 160°C and stirred for 1 hour at a stirring rate of 60 rpm. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 80°C and distilled under reduced pressure until no liquid was extracted to obtain 173.5 g of modified copolymer.

[0062] S4. Preparation of water-washable coating spray substrate

[0063] 432.4 mL of water-based coating was prepared by mixing 3.6 g of sodium polyacrylate, 3.6 g of polyoxyethylene ether, 3.2 g of silicon dioxide powder, 3.5 g of polydimethylsiloxane and 3.5 g of polyvinyl alcohol, 150.0 g of modified copolymer, 300.0 mL of deionized water and 150.0 mL of dimethyl sulfoxide;

[0064] Select a spray gun with a nozzle diameter of 1.2 mm, a spraying pressure of 50 psi, a distance of 30 cm between the spray gun and the substrate, a spray gun movement speed of 40 cm / min, and a coating thickness of 20 mm. After spraying, place the material in an oven at a temperature of 20°C and a relative humidity of 50% to dry for 2 hours. After drying, cure it at room temperature for 24 hours to obtain a material with a surface coated with a modified acrylic resin coating.

[0065] Example 2

[0066] This embodiment provides a method for preparing a modified acrylic resin anticorrosive coating, comprising the following steps:

[0067] S1. Preparation of copolymer

[0068] Weigh 60.8 g of glycidyl methacrylate, 22.8 g of allyl fluoride, 106.4 g of 9,10-epoxy-1,5-cyclododecadiene and 748.3 mL of N,N-dimethylformamide, add them into a reaction kettle, stir at room temperature for 20 min at a stirring rate of 120 rpm to obtain a reaction precursor solution;

[0069] 600 mL of reaction precursor solution and 11.9 g of azobisisobutyronitrile were weighed and added to a reactor. The temperature of the reactor was raised to 100° C. and the reaction was kept warm for 3 h. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 80° C. and distilled under reduced pressure until no liquid was produced, to obtain 183.5 g of modified polyacrylic acid resin;

[0070] 150.0 g of modified polyacrylic acid resin, 75.2 g of 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-benzotriazole, 25.0 g of triethylamine and 1.1 L of dimethyl sulfoxide were added to the reactor, the temperature of the reactor was raised to 175°C, and the reaction was kept warm for 3 hours. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 100°C, and distilled under reduced pressure until no liquid was produced, to obtain 211.3 g of copolymer.

[0071] S2. Preparation of alkylated nano-α-Al2O3

[0072] 5 L of 0.10 mol / L aluminum nitrate solution was added to the reaction kettle, and the pH of the solution system was adjusted to 8.5 with saturated ammonia water while stirring at room temperature, and the stirring rate was 160 rpm to obtain a reaction precursor solution;

[0073] The reaction precursor solution was added into a magnetic stirrer, stirred at room temperature for 6 h at a stirring rate of 360 rpm, and allowed to stand for 24 h after the stirring was completed. After the standing was completed, the gel was filtered to obtain a gel;

[0074] The gel was crushed and sieved to obtain gel powder. The gel powder was moved to a tubular heating furnace and nitrogen was introduced for protection. The tubular heating furnace was heated to 1110°C at a rate of 10°C / min, kept warm for 8 hours, cooled naturally to 600°C, and heated at 0.5m 3 Water vapor was introduced at a rate of / h, and after keeping warm for 6h, it was naturally cooled to obtain 48.5g activated nano-α-Al2O3;

[0075] 36.0 g activated nano α-Al2O3, 26.7 g S-(2-trimethoxysilylethyl) ethanesulfonate, 25.9 g isocyanate methyltrimethoxysilane, 180.2 mL N,N-dimethylformamide and 4.8 g triethylamine were added to the reactor and reacted at room temperature for 4 hours. After the reaction was completed, the filter cake was collected by filtration and placed in a drying oven at 80°C for vacuum drying until the filter cake had a constant weight, to obtain 79.3 g alkylated nano α-Al2O3.

[0076] S3. Preparation of modified copolymer

[0077] Weigh 50.0 g of alkylated nano-α-Al2O3, 126.3 mL of dimethyl sulfoxide, 378.9 mL of deionized water, 12.5 g of polyvinyl pyrrolidone and 2.6 g of sodium dodecylbenzene sulfonate and mix to prepare a dispersion;

[0078] 150 g of copolymer and 450 mL of dispersion were weighed and added to the reactor. The temperature of the reactor was raised to 180°C and stirred for 2 h at a stirring rate of 80 rpm. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 80°C and distilled under reduced pressure until no liquid was extracted to obtain 183.9 g of modified copolymer.

[0079] S4. Preparation of water-washable coating spray substrate

[0080] 431.5 mL of water-based coating was prepared by mixing 6.0 g of sodium polyacrylate, 3.0 g of polyoxyethylene ether, 3.0 g of silicon dioxide powder, 3.0 g of polydimethylsiloxane and 3.0 g of polyvinyl alcohol, 150.0 g of modified copolymer, 300.0 mL of deionized water and 150.0 mL of dimethyl sulfoxide.

[0081] Select a spray gun with a nozzle diameter of 1.2 mm, a spraying pressure of 50 psi, a distance of 30 cm between the spray gun and the substrate, a spray gun movement speed of 40 cm / min, and a coating thickness of 20 mm. After spraying, place the material in an oven at a temperature of 20°C and a relative humidity of 50% to dry for 2 hours. After drying, cure it at room temperature for 24 hours to obtain a material with a surface coated with a modified acrylic resin coating.

[0082] Example 3

[0083] This embodiment provides a method for preparing a modified acrylic resin anticorrosive coating, comprising the following steps:

[0084] S1. Preparation of copolymer

[0085] Weigh 60.0 g of glycidyl methacrylate, 20.0 g of allyl fluoride, 101.2 g of 9,10-epoxy-1,5-cyclododecadiene and 601.2 mL of N,N-dimethylformamide, add them into a reaction kettle, stir at room temperature for 15 min at a stirring rate of 120 rpm to obtain a reaction precursor solution;

[0086] 500 mL of reaction precursor solution and 9.9 g of azobisisobutyronitrile were weighed and added to a reactor. The temperature of the reactor was raised to 80° C. and the reaction was kept warm for 2 h. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 70° C. and distilled under reduced pressure until no liquid was produced, to obtain 169.3.1 g of modified polyacrylic acid resin;

[0087] 150.0 g of modified polyacrylic acid resin, 74.2 g of 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-benzotriazole, 22.5 g of triethylamine and 1.2 L of dimethyl sulfoxide were added to a reactor, the temperature of the reactor was raised to 165°C, and the reaction was kept warm for 1 hour. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 100°C, and distilled under reduced pressure until no liquid was produced, to obtain 213.5 g of a copolymer.

[0088] S2. Preparation of alkylated nano-α-Al2O3

[0089] 5L of 0.15mol / L aluminum nitrate solution was added to the reaction kettle, and the pH of the solution system was adjusted to 9 with saturated ammonia water while stirring at room temperature, and the stirring rate was 150rpm to obtain a reaction precursor solution;

[0090] The reaction precursor solution was added into a magnetic stirrer, stirred at room temperature for 7 hours at a stirring rate of 280 rpm, and allowed to stand for 24 hours after the stirring was completed. After the standing was completed, the gel was filtered to obtain a gel;

[0091] The gel was crushed and sieved to obtain gel powder. The gel powder was moved to a tubular heating furnace and nitrogen was introduced for protection. The tubular heating furnace was heated to 1110°C at a rate of 10°C / min, kept warm for 7 hours, cooled naturally to 450°C, and heated at 0.3m 3 Water vapor was introduced at a rate of / h, and after keeping warm for 5h, it was naturally cooled to obtain 68.3g activated nano-α-Al2O3;

[0092] 48.0 g activated nano α-Al2O3, 36.0 g S-(2-trimethoxysilylethyl) ethanesulfonate, 36.0 g isocyanate methyltrimethoxysilane, 360.0 mL N,N-dimethylformamide and 6.0 g triethylamine were added to the reactor and reacted at room temperature for 3 hours. After the reaction was completed, the filter cake was collected by filtration and placed in a drying oven at 80°C for vacuum drying until the filter cake had a constant weight, to obtain 105.3 g alkylated nano α-Al2O3.

[0093] S3. Preparation of modified copolymer

[0094] Weigh 50.0 g of alkylated nano-α-Al2O3, 138.8 mL of dimethyl sulfoxide, 416.7 mL of deionized water, 6.67 g of polyvinyl pyrrolidone and 5.0 g of sodium dodecylbenzene sulfonate and mix to prepare a dispersion;

[0095] 150 g of copolymer and 450 mL of dispersion were weighed and added to the reactor. The temperature of the reactor was raised to 160°C and stirred for 3 hours at a stirring rate of 80 rpm. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 100°C and distilled under reduced pressure until no liquid was extracted to obtain 169.3 g of modified copolymer.

[0096] S4. Preparation of water-washable coating spray substrate

[0097] 433.2 mL of water-based coating was prepared by mixing 4.5 g of sodium polyacrylate, 3.0 g of polyoxyethylene ether, 6.0 g of silicon dioxide powder, 3.0 g of polydimethylsiloxane and 1.5 g of polyvinyl alcohol, 150.0 g of modified copolymer, 300.0 mL of deionized water and 150.0 mL of dimethyl sulfoxide;

[0098] Select a spray gun with a nozzle diameter of 1.3 mm, a spraying pressure of 50 psi, a distance of 30 cm between the spray gun and the substrate, a spray gun movement speed of 40 cm / min, and a coating thickness of 18 mm. After spraying, place the material in an oven at a temperature of 20°C and a relative humidity of 50% to dry for 3 hours. After drying, cure it at room temperature for 24 hours to obtain a material with a surface coated with a modified acrylic resin coating.

[0099] Comparative Example 1

[0100] The difference between this comparative example and Example 3 is that in step S1, an equal amount of polyacrylic acid resin is used to replace the modified polyacrylic acid resin.

[0101] Comparative Example 2

[0102] The difference between this comparative example and Example 3 is that in step S2, an equal amount of nano zinc oxide powder is used to replace the activated nano α-Al2O3.

[0103] Comparative Example 3

[0104] The difference between this comparative example and Example 3 is that in step S2, an equal amount of activated nano α-Al2O3 is used to replace the alkylated nano α-Al2O3.

[0105] Comparative Example 4

[0106] The difference between this comparative example and Example 3 is that in step S4, an equivalent amount of polyacrylic acid resin with a molecular weight of 3654.23 is used to replace the modified copolymer.

[0107] Performance Test:

[0108] The UV resistance, wear resistance, corrosion resistance, adhesion and antioxidant capacity of the materials coated with modified acrylic resin coatings prepared in Examples 1-3 and Comparative Examples 1-4 were tested. The adhesion grade of the coating was determined according to the standard GB / T31586.2-2015 "Evaluation and acceptance criteria for adhesion / cohesion (destructive strength) of protective coating systems for anti-corrosion protective coatings of steel structures Part 2: Cross-hatch test and cross-hatch test" for adhesion resistance; the wear resistance was determined according to the standard YY / T 0988.15-2016 "Surgical implant coatings Part 15: Test method for wear resistance of metal thermal spray coatings" for wear resistance; the corrosion resistance was tested according to the standard JB / T 6073-1992 "Laboratory full immersion corrosion test for metal coverings" for corrosion resistance; the antioxidant capacity was tested according to the standard JB / T 10458-2004 "Technical conditions for high temperature oxidation resistant coatings for mechanical equipment"; the materials coated with modified acrylic resin coatings prepared in Example 3 and Comparative Examples 1-4 were subjected to ultraviolet corrosion with reference to the standard GB / T 23987-2009 "Artificial weathering exposure of paint and varnish coatings, exposure to fluorescent ultraviolet rays and water", and the wear resistance, corrosion resistance, hardness, adhesion and antioxidant capacity of the materials were tested for the second time. The specific test data are shown in Table 1-2:

[0109] Table 1-Performance test data of the sample

[0110]

[0111]

[0112] Table 2-Performance test data of samples after ultraviolet radiation

[0113]

[0114] Data Analysis:

[0115] A comparative analysis of the data in Table 1 shows that the scratch test structure grade of the modified acrylic resin anti-corrosion coating prepared by the present invention reaches level 0, the mass loss after 100 cycles of wear is 3.5 mg, the complete immersion corrosion rate is 0.21%, and the coating has no powdering, bubbles, shedding, or bottom exposure after high-temperature oxidation treatment at 120°C; by comparing the data of Example 3, Comparative Example 1, Comparative Example 2, and Comparative Example 3, it can be seen that the copolymer and the dispersion prepared by the present invention cooperate with each other to improve the bonding force, wear resistance, and corrosion resistance of the coating and the base material; by comparing the data of Example 3 and Comparative Example 4, it can be seen that the bonding force, wear resistance, and corrosion resistance of the modified acrylic resin anti-corrosion coating prepared by the present invention are significantly improved compared with ordinary polyacrylic acid coatings; in summary, in the process of preparing an anti-corrosion coating based on a modified acrylic resin, the present invention prepares a copolymer, prepares nano α-Al2O3, and modifies the nano α-Al2O3 to prepare a dispersion, and finally obtains an anti-corrosion coating with excellent wear resistance, high bonding force, and antioxidant properties.

[0116] By comparing the data in Table 2 above, it can be found that the anti-corrosion coating obtained by cross-linking the anti-ultraviolet groups in Example 3 after ultraviolet radiation still has a cross-scratch test structure grade of 0, a mass loss of 6.7 mg after 100 cycles of wear, a complete immersion corrosion rate of 0.32%, and no powdering, bubbles, shedding, or bottom exposure of the coating after 120°C high-temperature oxidation treatment. On the other hand, in Comparative Examples 1 and 4, the coatings finally obtained without cross-linking the anti-ultraviolet groups in the polyacrylic resin have significantly decreased in various properties after ultraviolet radiation, while in Comparative Examples 2 and 3, since the anti-ultraviolet groups are cross-linked in the coatings, the various properties of these two items have not been significantly decreased. In summary, the anti-corrosion coating based on modified acrylic resin after internal cross-linking of anti-ultraviolet groups has the advantages of excellent wear resistance, high bonding strength, and antioxidant performance, while the anti-ultraviolet performance is also significantly improved.

[0117] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

[0118] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0119] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing an anticorrosive coating based on a modified acrylic resin, characterized in that: The following steps are involved: S1, adding modified polyacrylic acid resin, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-benzotriazole, triethylamine and dimethyl sulfoxide into a reaction kettle, raising the temperature of the reaction kettle to 155-175° C., keeping the temperature for reaction for 1-3 hours, and post-treating to obtain a copolymer; S2, adding activated nano-α-Al2O3, S-(2-trimethoxysilylethyl)ethanesulfonate, isocyanate methyltrimethoxysilane, N,N-dimethylformamide and triethylamine into a reaction kettle, reacting at room temperature for 2-4 hours to obtain alkylated nano-α-Al2O3; S3, adding the copolymer and the dispersion into a reactor, raising the temperature of the reactor to 160-180° C., keeping the temperature and stirring for 1-2 hours, and post-treating to obtain a modified copolymer; S4, preparing an anticorrosive coating using the modified copolymer, deionized water, dimethyl sulfoxide and an auxiliary agent; S5. Use a spray gun to spray the anti-corrosion coating on the substrate to form an anti-corrosion coating with a thickness of 15-20 mm on the surface of the substrate.

2. The method for preparing a modified acrylic resin anticorrosive coating according to claim 1, characterized in that: In step S1, the preparation method of the modified polyacrylic acid resin comprises the following steps: A1, add glycidyl methacrylate, allyl fluoride, 9,10-epoxy-1,5-cyclododecadiene and N,N-dimethylformamide into a reaction kettle, and stir at room temperature for 15-20 minutes to obtain a reaction precursor solution; A2. Add the reaction precursor liquid and azobisisobutyronitrile into the reactor, increase the temperature of the reactor to 80-100° C., keep the temperature for 2-4 hours, and post-treat to obtain the modified acrylic resin.

3. The method for preparing a modified acrylic resin anticorrosive coating according to claim 2, characterized in that: In step A1, the amount ratio of glycidyl methacrylate, allyl fluoride, 9,10-epoxy-1,5-cyclododecadiene and N,N-dimethylformamide is 3-5g:1-2g:6-8g:40-50mL, and the stirring rate is 120-180rpm; in step A2, the amount ratio of reaction precursor liquid and azobisisobutyronitrile is 40-50mL:0.5-0.8g, and post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added to a rotary evaporator with a water bath temperature of 60-80°C, and reduced pressure distillation is performed until no liquid is produced to obtain a modified acrylic resin.

4. The method for preparing a modified acrylic resin anticorrosive coating according to claim 1, characterized in that: In step S1, the amount ratio of modified polyacrylic acid resin, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-benzotriazole, triethylamine and dimethyl sulfoxide is 3-5g:1-2g:0.2-0.5g:20-25mL, and the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added to a rotary evaporator with a water bath temperature of 60-100°C, and the reduced pressure distillation is carried out until no liquid is extracted to obtain a copolymer.

5. The method for preparing a modified acrylic resin anticorrosive coating according to claim 4, characterized in that: In step S2, the preparation method of activated nano α-Al2O3 comprises the following steps: B1. Add 0.05-0.15 mol / L aluminum nitrate solution into the reaction kettle, and adjust the pH value of the solution system to 8.5-9.5 with saturated ammonia water while stirring at room temperature to obtain a reaction precursor solution; B2. Add the reaction precursor solution into a magnetic stirrer, stir at room temperature for 6-8 hours, let it stand for 24 hours after stirring, and post-treat to obtain a gel; B3. Crush the gel, sieve it to obtain gel powder, and then post-treat it to obtain activated nano-α-Al2O3.

6. The method for preparing a modified acrylic resin anticorrosive coating according to claim 5, characterized in that: In step B1, the stirring rate is 120-180 rpm; In step B2, the stirring rate is 240-360 rpm, and the post-treatment includes: after standing, filtering to obtain a gel; in step B3, the post-treatment includes: after the gel powder is moved to a tubular heating furnace, the tubular heating furnace is heated to 1100±10°C at a rate of 10°C / min, kept warm for 6-8h, naturally cooled to 300-600°C, and heated at 0.1-0.5m 3 Water vapor is introduced at a rate of / h, and after keeping warm for 4-6 hours, it is naturally cooled to obtain activated nano α-Al2O3.

7. The method for preparing a modified acrylic resin anticorrosive coating according to claim 4, characterized in that: In step S2, the amount ratio of activated nano α-Al2O3, S-(2-trimethoxysilylethyl)ethanesulfonate, isocyanate methyltrimethoxysilane, N,N-dimethylformamide and triethylamine is 5-8g:3-5g:3-5g:40-50mL:0.5-1g, and the post-treatment includes: after the reaction is completed, collecting the filter cake by suction filtration, placing the filter cake in a drying oven at a temperature of 80°C and vacuum drying it until the filter cake has a constant weight, thereby obtaining alkylated nano α-Al2O3.

8. The method for preparing a modified acrylic resin anticorrosive coating according to claim 1, characterized in that: In step S3, the amount ratio of the copolymer and the dispersion is 3-5g:15-20mL, the stirring rate is 60-80rpm, and the dispersion is prepared by mixing alkylated nano-α-Al2O3, dimethyl sulfoxide, deionized water, polyvinyl pyrrolidone and sodium dodecylbenzene sulfonate in an amount ratio of 15-20g:50mL:150mL:2-5g:1-3g. The post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added to a rotary evaporator with a water bath temperature of 80-100°C, and reduced pressure distillation is performed until no liquid is extracted to obtain a modified copolymer.

9. The method for preparing a modified acrylic resin anticorrosive coating according to claim 1, characterized in that: In step S4, the amount ratio of the modified copolymer, deionized water, dimethyl sulfoxide and auxiliary agent is 5-8g:10-15mL:5-10mL:0.5-0.6g; the auxiliary agent includes the following components in parts by weight: 5-20 parts of dispersant, 3-10 parts of stabilizer, 10-30 parts of filler, 5-10 parts of leveling agent and 5-10 parts of anti-sticking agent, the dispersant is one or more of polyvinyl alcohol, sodium polyacrylate, and polyvinyl ether, the stabilizer is one or more of polyoxyethylene ether, dodecyl polyoxyethylene ether and fatty alcohol polyoxyethylene ether, the filler is one or more of silicon dioxide powder, calcium carbonate powder and aluminum oxide powder, the leveling agent is one or more of polydimethylsiloxane, polymethylsiloxane and polyvinyl siloxane, and the anti-sticking agent is one or more of polyvinyl alcohol, polyethylene glycol and polypropylene glycol.

10. The method for preparing a modified acrylic resin anticorrosive coating according to claim 9, characterized in that: In step S4, the spraying operation is as follows: select a spray gun with a nozzle diameter of 1.2-1.4 mm, a spraying pressure of 40-50 psi, a distance of 20-30 cm between the spray gun and the substrate, a spray gun movement speed of 40-60 cm / min, a coating thickness of 15-20 mm, and after spraying, place the material in an oven at a temperature of 20-25°C and a relative humidity of 30-50% to dry for 2-4 hours. After drying, cure at room temperature for 24 hours to obtain a material with a surface coated with a modified acrylic resin coating.

Citation Information

Patent Citations

  • Coating composition

    CN101448909A

  • Waterproof breathable membrane

    CN110746688A

  • Water-based ceramic coating and preparation method thereof

    CN112094514A

  • Hybrid functionalized fluoropolymers for lithium ion batteries

    CN114402467A

  • High-wear-resistance anti-ultraviolet film and preparation method thereof

    CN118546407A

Cited By

  • Anti-aging acrylic resin waterproof coating and preparation method thereof

    CN119842278A