Multifunctional hydrogel for promoting nerve repair and diabetes wound healing and application thereof
By developing functional hydrogels with keratin and zinc ion-based and loading coral lactone, the problems of incomplete filling, lack of antibacterial function and insufficient biocompatibility in diabetic wound treatment were solved, and the efficiency of diabetic wounds was achieved Healing and nerve regeneration.
Patent Information
- Application Number
- CN202411131275.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-17
- Publication Date
- 2024-11-22
AI Technical Summary
Existing hydrogel dressings have problems with incomplete filling, limited joint movement and lack of antibacterial function in the treatment of diabetes wounds, and the limited active chemical groups of functional hydrogels lead to poor biocompatibility and therapeutic effects. , especially for neural repair and diabetic wound healing, lack of effective materials.
A natural protein-based functional hydrogel was developed, prepared by dual dynamic cross-linking reactions of keratin, protocatechaldehyde and zinc ions through thiol-aldehyde addition and catechol-zinc coordination, combined with loading Coral lactone forms ker-PA/Zn hydrogel, with excellent injection properties, skin adhesion, self-healing and antibacterial ability.
This hydrogel significantly promotes skin nerve regeneration, angiogenesis and tissue remodeling in a diabetic mouse model, improving wound healing rates, especially through the synergistic effects of zinc ions and coralactone, showing that in diabetic wound treatment huge potential in.
Smart Images

Figure CN118987241A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrogels, in particular to a multifunctional hydrogel for promoting nerve repair and diabetic wound healing and application thereof. Background Art
[0002] Diabetic wounds are a major complication of diabetes and are associated with increased morbidity, high incidence, and socioeconomic burden [1]. Clinical studies have shown that peripheral neuropathy, inflammatory dysfunction, decreased angiogenesis, and uncontrolled bacterial infection are associated with the pathogenesis of diabetic wounds and lead to impaired or even non-healing states of diabetic wounds [2-4]. Therefore, due to the complexity of diabetic wounds, there is an urgent need to develop comprehensive treatment strategies.
[0003] Wound dressings have great application prospects in the treatment of diabetic wounds, among which hydrogels are considered to be an ideal dressing due to their good biocompatibility and strong ability to deliver therapeutic agents [5]. However, traditional hydrogel dressings have some limitations, such as incomplete filling of irregular wound beds, limited joint motion, and lack of antibacterial function. In view of this, hydrogel dressings with ideal adhesion, mechanical and antibacterial capabilities provide good candidates for clinical practice of diabetic wounds [6]. However, due to the limited active chemical groups of functional hydrogels, complex synthetic procedures are usually required to develop functional hydrogels, especially those derived from natural polymers, which in turn impairs the inherent biocompatibility of hydrogel dressings.
[0004] To achieve superior therapeutic effects, various therapeutics including endogenous cells, extracellular vesicles, therapeutic nanoparticles, and chemotherapeutic drugs have been loaded into hydrogels to endow the dressings with anti-inflammatory, angiogenic, or epithelialization functions[7-9]. Neurodegeneration is closely related to impaired wound healing in diabetic patients, and the development of wound dressings with skin nerve regeneration is in its infancy due to the lack of innervation-related therapies or material design approaches
[10] .
[0005] However, there are no reports on a multifunctional hydrogel that promotes nerve repair and diabetic wound healing and its application. Summary of the invention
[0006] The purpose of the present invention is to provide a multifunctional hydrogel and its application for promoting nerve repair and diabetic wound healing in view of the deficiencies in the prior art.
[0007] In a first aspect, the present invention provides a natural protein-based functional hydrogel, which includes keratin, protocatechuic aldehyde and zinc ions. The hydrogel is based on keratin, with protocatechuic aldehyde and zinc ions as building units, and is prepared by a dual dynamic cross-linking reaction of thiol-aldehyde addition and catechol-zinc ion coordination.
[0008] As a preferred example, the keratin is a natural protein rich in cysteine.
[0009] In a second aspect, the present invention provides a ker-PA / Zn hydrogel loaded with choriocarpa lactone, wherein the ker-PA / Zn hydrogel loaded with choriocarpa lactone comprises choriocarpa lactone, F127 / F68 and a hydrogel.
[0010] As a preferred example, the ker-PA / Zn hydrogel loaded with choriocarbapenem lactone is a keriocarbapenem lactone encapsulated in F127 / F68 mixed micelles and loaded into the hydrogel.
[0011] In a third aspect, the present invention provides the use of hydrogel in preparing a drug for promoting nerve repair or diabetic wound healing.
[0012] In a fourth aspect, the present invention provides the use of ker-PA / Zn hydrogel loaded with corallinalool in the preparation of a drug for promoting nerve repair or diabetic wound healing.
[0013] The present invention has the advantages that skin nerve regeneration in diabetic wounds remains a challenge in current clinical treatment. The present invention uses keratin as the only matrix, protocatechuic aldehyde (PA) and zinc ions as building blocks, and develops a natural protein-based functional hydrogel through a dual dynamic cross-linking reaction of thiol-aldehyde addition and catechol-zinc ion coordination. The unique structural design gives the hydrogel excellent injectability, skin adhesion, self-healing and antibacterial ability, and biocompatibility. In addition, the hydrogel also acts as a drug carrier for loading and sustained release of choriocarpa lactone (PP), a natural compound extracted from the traditional Chinese medicine Angelica dahurica. Our results show that PP-loaded hydrogels can promote skin nerve regeneration, angiogenesis, and tissue remodeling in full-thickness wounds of two diabetic mice induced by db / db and streptozotocin, especially through the synergistic effect of zinc ions and PP, showing great potential in the treatment of diabetic wounds. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 .Schematic diagram of the construction mechanism of keratin-based functional hydrogel and its physical and biological functions in diabetic wound healing.
[0015] Figure 2Preparation and evaluation of ker-PA / Zn hydrogels. (A) UV-visible spectra of PA and PA / Zn complexes, and photographs of PA / Zn complex solutions. (B) Digital and SEM photographs of ker-PA / Zn hydrogels. Scale bar = 200 μm. (C) Average pore size measured based on SEM images. (D) Equilibrium swelling ratio of ker-PA / Zn hydrogels. (E) Pictures of hydrogels adhered to bent finger joints. (F) Pictures of hydrogels adhered to various materials. (G) Pictures of hydrogels compressed and stretched by fingers. (H) Strain sweeps of hydrogels. (I) Rheological properties of hydrogels. (J) Shear thinning test of hydrogels, and pictures of hydrogels injected into water through a 26-gauge syringe needle. (K) Rheological behavior of hydrogels under alternating strain cycles. (L) Pictures of the self-healing ability of hydrogels. Data are presented as mean ± SD. NS indicates no significant difference; *P<0.05, **P<0.01, ****P<0.0001.
[0016] Figure 3 Drug release, antibacterial ability and biocompatibility of hydrogels. (A) Release curve of PP from hydrogels. (B) Hemolysis test of hydrogels. PBS and deionized water were set as negative and positive controls, respectively. (C) Antibacterial activity against Staphylococcus aureus was evaluated by inhibition zone method. (D) Pictures of bacterial colonies on agar plates after contact with hydrogels with three PA / Zn complex concentrations, with PBS as control. (E) Figure 2 Bacterial viability of hydrogels of D. (F) Cell viability of L929 mouse fibroblasts at 1, 3, and 5 days of incubation. (G) Live / dead staining of L929 mouse fibroblasts at 1, 3, and 5 days of incubation. Scale bar, 200 μm. Data are presented as mean ± SD, NS indicates not significant, ****P < 0.0001.
[0017] Figure 4 . In vitro migration and remyelination assessment. (A) Cell migration assay of Schwann cells in normal glucose environment. Scale bar = 100 μm. (B) Cell migration assay of Schwann cells in high glucose environment. Scale bar = 100 μm. (C) Based on Figure 4 Quantification of cell migration based on A. (D) Figure 4 Quantification of cell migration in B. (EG) Immunofluorescence staining of S100β, Tuj1, and phalloidin in Schwann cells. Scale bar = 100 μm. Data are presented as mean ± SD, NS indicates not significant; *P < 0.05, **P < 0.01, ***P < 0.001.
[0018] Figure 5In vivo evaluation of diabetic wound healing of ker-PA / Zn 0.2 and ker-PA / Zn / PP 0.2 hydrogels in two diabetic model mice, db / db and STZ-induced C57BL / 6. Wounds treated with PBS were used as controls, and rb-bFGF was applied as a positive drug for comparison. (A) Schematic diagram of the experimental timeline of the wound healing assay. (B) Representative photographs of wounds in all groups at days 0, 2, 4, 6, and 9 after injury. (C) Quantitative analysis of wound healing rates in db / db mice. (n=5). (D) Quantitative analysis of wound healing rates in STZ-induced C57BL / 6 mice (n=5). P<0.05, **P<0.01, ***P<0.001.
[0019] Figure 6 In vivo evaluation of collagen deposition and tissue remodeling of ker-PA / Zn 0.2 and ker-PA / Zn / PP 0.2 hydrogels in diabetic wounds. (A) H&E staining of wounds at 4 and 9 days after wounding. Scale bar = 300 μm. The red dashed line outlines the migration of the epithelial tongue; the black dashed line marks the edge of the wound. (B) Figure 6 A Quantitative assessment of epidermal migration length on day 4. (C) Quantitative measurement of the remaining width of the wound on day 9 according to panel A. (D) Masson staining of wounds on days 4 and 9 after wounding. Scale bar = 100 μm. Yellow arrows indicate the appearance of new dermal appendages on day 9. (E) Quantitative assessment of collagen density on day 4. (F) Quantification of the number of dermal appendages on day 9. Data are presented as mean ± SD, NS indicates not significant; *P < 0.05, **P < 0.01, ***P < 0.001, ****P < 0.0001.
[0020] Figure 7 Effects of ker-PA / Zn / PP 0.2 hydrogel on Schwann cell maturation in diabetic wounds. (A) Immunohistochemical staining of glial cells and neural proteins (Tuj1, MBP, and S100β) (n=3). Scale bar = 150 μm. (B-D) Quantitative analysis of Tuj1, MBP, and S100β on days 4 and 9. Data are presented as mean ± SD, NS indicates not significant; *P<0.05, **P<0.01, ***P<0.001, ****P<0.0001.
[0021] Figure 8Effects of ker-PA / Zn / PP 0.2 hydrogel on axonal regeneration in diabetic wounds. (A) Immunohistochemical staining of GAP43 and PGP9.5 on days 4 and 9 (n=3). Scale bar=150 μm. (B) Quantitative analysis of GAP43. (C) Quantitative analysis of PGP9.5. Data are presented as mean ± SD, NS indicates not significant; *P<0.05, **P<0.01, ***P<0.001, ****P<0.0001.
[0022] Fig. 9 Effects of ker-PA / Zn / PP 0.2 hydrogel on angiogenesis in diabetic wounds on days 4 and 9. (A) Immunohistochemical staining of CD31 and VEGF (n=3). Scale bar=150μm. (B) Quantitative analysis of CD31. (C) Quantitative analysis of VEGF. Data are expressed as mean ± SD. *P<0.05, **P<0.01, ***P<0.001, ****P<0.0001. DETAILED DESCRIPTION
[0023] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0024] Example 1
[0025] In this paper, we developed a protein-based therapeutic hydrogel for skin nerve regeneration and diabetic wound healing ( Figure 1). For this hydrogel, keratin was used as the sole matrix, and the naturally derived chemical protocatechuic aldehyde (PA) and zinc ions were used as building blocks to form dynamic chemical crosslinks with keratin in a mild and simple manner. Keratin is a natural protein rich in cysteine that is widely present in the skin and skin appendages (such as hair and wool)
[11] . Emerging evidence shows that keratin has good biocompatibility and wound repair capabilities
[12] . Notably, the inherent free thiol groups in keratin can be used as active groups to explore functional hydrogels
[12] . Zinc ions have been reported to stimulate nerve regeneration and angiogenesis during wound healing
[13] . PA is derived from the Chinese herbal medicine Salvia miltiorrhiza and has an aldehyde group and a catechol group in its chemical structure
[14] . The unique chemical structure enables PA to form catechol-metal ion coordination bonds with zinc ions and dynamically crosslink with keratin through aldehyde-thiol addition reactions. The preparation process of the hydrogel only requires physical mixing under mild conditions, without the involvement of additional catalysts or crosslinkers, and without the need for chemical modification of keratin. In addition, the natural compound chorthiolide (PP) extracted from the traditional Chinese medicine Angelica dahurica was encapsulated in F127 / F68 mixed micelles and loaded into hydrogels. The effects of PP and PP-loaded hydrogels on nerve regeneration were investigated in vitro and their wound healing effects were evaluated in full-thickness wounds of both db / db and streptozotocin-induced C57BL / 6 diabetic mice.
[0026] 1 Method
[0027] 1.1 Materials
[0028] According to our previous work
[39] , keratin was extracted from duck feathers. Briefly, 10 g of duck feathers were immersed in a reaction solution containing 8 mol / L urea, 0.2 mol / L SDS, and 0.5 mol / L Na2S2O5 at 70 °C for 1 h. Subsequently, the solution was dialyzed and freeze-dried to obtain keratin powder. Protocatechuic aldehyde, choriocarpone, and zinc acetate were purchased from Shanghai Yuanye Biotechnology Co., Ltd. (China).
[0029] 1.2 Extraction and purification of keratin
[0030] Keratin was extracted by soaking 10 g of duck feathers in 100 mL of a solution containing 8 mol / L urea (Shanghai Lingfeng Chemical Reagent Co., Ltd.), 0.2 mol / L SDS (Sinopharm Chemical Reagent Co., Ltd.), and 0.5 M mol / L Na2S2O5 (Sinopharm Chemical Reagent Co., Ltd.). The mixture was heated to 70 °C for 1 hour. The solution was then filtered and dialyzed against distilled water using a cellulose tube (molecular mass cutoff of 8–14 kDa). After dialysis, the solution was freeze-dried to obtain keratin powder.
[0031] 1.3 Preparation of PA / Zn complex
[0032] To prepare the PA / Zn complex, protocatechuic aldehyde (PA, 1 mmol) was dissolved in deionized water at 80 °C, and then anhydrous zinc acetate (0.5 mmol) was added to the PA solution (the molar ratio of PA to zinc acetate was set to 2:1). The pH value of the mixture was then adjusted to 10 by adding ammonium hydroxide. Moreover, the coordination of zinc is much slower than that of iron. Therefore, after stirring at room temperature overnight, the PA / Zn complex was obtained.
[0033] 1.4 Preparation of ker-PA / Zn hydrogel
[0034] PA / Zn complexes were prepared according to the literature [15,16]. PA was dissolved in deionized water at 80 °C and then mixed with zinc acetate solution at a PA:Zn molar ratio of 2:1. The pH of the solution was adjusted to 10.0 with ammonium hydroxide. PA / Zn complexes were obtained after stirring at room temperature for 12 h and analyzed using a UV-Vis spectrophotometer. An 18% w / v keratin solution was prepared by dissolving 0.09 g keratin in 0.5 ml deionized water. The PA / Zn complex solution was mixed with the keratin solution to adjust the final PA concentration in the hydrogel to 0.1, 0.2, and 0.3% w / v, respectively. The mixed solution was stirred for a few seconds and left statically to form a hydrogel. The resulting hydrogels were ker-PA / Zn 0.1, ker-PA / Zn 0.2, and ker-PA / Zn 0.3, respectively.
[0035] 1.5SEM observation
[0036] The microstructure of the hydrogel was observed using a scanning electron microscope (SEM) (HITACHI / TM-1000). Before observation, the hydrogel was freeze-dried and sprayed with gold. Based on the SEM images, the pore size of the hydrogel was measured using Image J software.
[0037] 1.6 Swelling capacity
[0038] The swelling behavior of ker-PA / Zn hydrogel was determined at 37°C by immersing the hydrogel (5 mm in height and 10 mm in diameter) in 5 mL of PBS (0.01 M, pH 7.4). At a certain time point, the hydrogel was taken out of the PBS solution and weighed after wiping the surface water with filter paper. The swelling ratio was calculated using the following formula: (M1-M0) / M0×100%, where M0 and M1 represent the weight of the hydrogel before and after swelling, respectively.
[0039] 1.7 Rheological test
[0040] Rheological tests were performed on a rheometer (HAKKE MARS 60). Before the test, the hydrogel with a diameter of 10 mm and a height of 8 mm was placed on parallel plates. A strain amplitude sweep test was performed to determine the linear viscoelastic region with a strain range of 0.01-1000%. The frequency sweep test conditions were set as: constant strain 1%, constant frequency 1 Hz, temperature 25 °C, and frequency sweep range 0.1-100 rad / s. The shear thinning properties of the hydrogel were determined by -1 The viscosity is determined by measuring the viscosity under a continuous ramp shear rate.
[0041] 1.8 In vitro blood compatibility test
[0042] Mouse blood was centrifuged at 1,500rpm to obtain red blood cells. Subsequently, the red blood cells were washed three times with PBS and diluted to a concentration of 5v / v%. 500μL of hydrogel was added to 500μL of red blood cell solution and incubated in an incubator at 37°C and 100rpm for 1 hour. Deionized water and PBS solutions were used as positive and negative controls, respectively. Then, the mixture was centrifuged at 1,000rpm for 10 minutes. The absorbance of the supernatant was measured at 540nm by an enzyme reader. The hemolysis rate was calculated using the following formula: Hemolysis rate (%) = [(As-Al-Ap) / (Aw-Ap)] × 100%, where As, Al, Aw and Ab are the absorbance values of the supernatant treated with hydrogel, the leached solution of the hydrogel in PBS, the supernatant treated with deionized water, and the supernatant treated with PBS, respectively.
[0043] 1.9 Evaluation of cytocompatibility of hydrogels
[0044] The cytocompatibility of ker-PA / Zn hydrogels was tested on L929 mouse embryonic cells using CCK-8 and Live / Dead assays. 5 UL -1DMEM with penicillin and 100 mg / L streptomycin was used as complete growth medium. The freeze-dried ker-PA / Zn hydrogel was sterilized under UV light for 24 hours, and 20 mg of the hydrogel was soaked in 10 mL of DMEM complete growth medium for 24 hours to obtain the extracted solution. L929 cells were seeded into 96-well plates at a density of 5000 cells / well. After culturing at 37°C for 24 hours, the culture medium was removed and supplemented with the extraction solution of the hydrogel. For CCK-8 assay, when the cells were cultured for 1, 3, and 5 days, the culture medium in the well was aspirated and replaced with 100 μL DMEM culture medium containing 10% CCK-8 dye. After incubation at 37°C for 1 hour, the absorbance value of the solution was measured at a wavelength of 450 nm using a microplate reader. For Live / Dead assay, 100 μL Calcein-AM / PI dye was used instead of CCK-8 dye. After incubation at 37°C for 40 minutes, the cells were observed and photographed with an inverted fluorescence microscope.
[0045] 1.10 Preparation of Coralline Lactone-Loaded Hydrogel
[0046] PP-loaded F127 / F68 mixed micelles were prepared by thin film hydration method to enhance water solubility [40-42]. Briefly, 50 μg PP, 26.7 mg Pluronic F127, and 13.3 mg Pluronic F68 were dissolved in 1 mL of anhydrous ethanol to form a clear and transparent solution. The mixture was then evaporated under reduced pressure by a rotary evaporator to obtain a thin film of PP / F127 / F68 complex. Then, the film was hydrated with 2 mL of deionized water and dispersed by ultrasound to form a micellar suspension. The suspension was filtered through a 0.45 μm filter membrane to produce PP-loaded micelles. The PP concentration was measured by UV spectrophotometer to be 10 μg / mL. To prepare PP-loaded hydrogels, 100 μL of PP micelles were mixed with 400 μL of hydrogel precursor solution, and the mixture was left static to form a hydrogel. The resulting hydrogel was recorded as ker-PA / Zn / PP 0.2 with a final PP concentration of 2 μg / mL.
[0047] 1.11 Release curve of choriolide
[0048] The release profile of sphaerolide from the hydrogel was evaluated by incubating the drug-loaded hydrogel in saline at 37°C. The samples were prepared in a cylindrical shape with a diameter of about 1 cm and a height of about 1 cm and placed in the wells of a 12-well plate. Subsequently, 2 mL of saline was added to cover the surface of the hydrogel, and the system was incubated at 37°C. At predetermined time intervals, the release medium was collected, the concentration of PP was determined by high performance liquid chromatography (HPLC), and replaced with the same volume of fresh saline.
[0049] 1.12 Evaluation of antimicrobial activity
[0050] The antibacterial activity of the hydrogels was evaluated by inhibition zone and spread plate colony count tests using Gram-positive Staphylococcus aureus (S. aureus) as a model bacterium. In the zone inhibition test, 100 μL of bacterial suspension (1×10 8 CFU / mL) was dropped onto an agar plate and spread evenly. Subsequently, the sterilized hydrogel sample was placed on an agar plate and incubated at 37°C for 24 hours. The resulting inhibition zone around the hydrogel was observed. In the spread plate colony count test, 500 μL of hydrogel was added to a 48-well microplate. Then, 100 μL of bacterial suspension (10 5 CFU / mL) and 100 μL sterilized PBS were added to the surface of the hydrogel disk. The system was incubated at 37°C for 24 hours. After incubation, the live bacteria were resuspended using sterilized PBS and cultured on agar plates at appropriate dilutions to count the number of live bacterial colonies.
[0051] 1.13 In vitro Schwann cell migration assessment
[0052] The cells were supplemented with 10% fetal bovine serum (FBS), 1.0 × 10 5 UL -1 DMEM with penicillin and 100 mg / L streptomycin was used as complete growth medium. 25 mM / L glucose was added to simulate a high-sugar environment. An appropriate number of RSC96 cells were seeded in a 6-well plate to reach 100% confluence within 24 hours. The cells were then scratched using a 200 μl pipette tip pressed vertically and firmly on the bottom of the plate. The medium and cell debris were then carefully aspirated. The cells were washed twice with PBS. The medium was then added to the wells in a slow and steady manner, ensuring that it covered the bottom of the wells. Preliminary photos were taken after the scratch was generated and 24 hours later. The unhealed area was then analyzed using ImageJ. The non-healing rate (%) can be calculated by dividing the non-healing area at 24 hours by the non-healing area at 0 hours.
[0053] 1.14 In vitro Schwann cell immunofluorescence assay
[0054] Cells were treated with PBS, ker-PA / Zn 0.2 hydrogel, PP-loaded hydrogel (ker-PA / Zn / PP 0.2), and PP solution (same concentration of 2 μg / ml, not encapsulated in F127 / F68 micelles) in culture medium for 48 h. Cell debris was then washed away with PBS. Cells were fixed with 4% paraformaldehyde (Servicebio, China) at 25°C for 15 min, immersed in 0.1% Triton X-10 (Servicebio, China) for 10 min, and blocked with 5% bovine serum albumin (Servicebio, China). IF555-phalloidin (Servicebio, 1:300, China) was used for staining. Alternatively, they were incubated with anti-S100β (1:100) and anti-Tuj1 (1:100) primary antibodies (Servicebio, China) at 4°C overnight. The samples were then incubated with FITC-labeled secondary antibodies (1:200, Servicebio, China) at 25°C in the dark for 1 hour. Subsequently, nuclear staining was performed using DAPI (1:500, Servicebio, China). Fluorescence images were acquired using a confocal microscope (LSM800, Zeiss).
[0055] 1.15 In vivo evaluation of diabetic wound healing
[0056] Animal experiments were approved by the Animal Care and Use Committee of Yueyang Hospital of Integrated Traditional Chinese and Western Medicine, Shanghai University of Traditional Chinese Medicine. Male db / db mice (8–10 weeks old) and C57BL / 6J mice (6–8 weeks old) were purchased from Shanghai SLAC Laboratory Animal Co., Ltd. C57BL / 6J mice were fed a high-fat diet for 3 weeks and then intraperitoneally injected with a low-dose streptozotocin (STZ) solution (50 mg / kg STZ dissolved in 0.5 mol / L, pH 4.5 sodium citrate buffer) for 7 days to induce type 1 diabetes. Mice with blood glucose levels exceeding 16.7 mmol / L one week after the last STZ injection were considered diabetic mice. After disinfection with 75% alcohol, full-thickness circular wounds with a diameter of approximately 6 mm were formed in the dorsal region using surgical scissors. The wounds were grouped and treated topically with sterilized PBS solution, ker-PA / Zn 0.2 hydrogel, ker-PA / Zn / PP 0.2 hydrogel, and rb-bFGF (Zhuhai Essence Biopharmaceuticals, Zhuhai, China). The hydrogel or rb-bFGF was replaced every 2 days. The wounds were recorded on days 0, 2, 4, 6, and 9. The wound area was measured using Image J software, and the wound healing rate was calculated based on the wound area
[12] .
[0057] 1.16 Assessment of re-epithelialization
[0058] Hematoxylin and eosin (H&E) staining was used to assess skin tissue re-epithelialization. Mice were euthanized on day 5 and wound tissue samples, including adjacent normal skin, were collected on day 10. The samples were then fixed in paraformaldehyde for 24 hours, embedded in paraffin, and sectioned along the longest diameter of the wound. The sections were stained with hematoxylin (0.2%) and eosin (1%) (G1076, Servicebio). Imaging was performed using Pannoramic MIDI (3DHISTECH, Hungary). Quantitative analysis was performed to measure wound width and epithelial tongue extension to assess the extent of skin re-epithelialization.
[0059] 1.17 Collagen Assessment
[0060] For mice, wound tissues were processed with the same procedure as for hematoxylin-eosin staining. Masson trichrome staining was performed according to the instructions provided in the Masson staining kit (G1006, Servicebio). The resulting images were captured by PannoramicMIDI (3DHISTECH, Hungary). Quantitative analysis was performed using Image J analysis software. Skin collagen staining density was quantified to assess collagen maturation.
[0061] 1.18 Assessment of wound nerve and vascular regeneration
[0062] The wound tissue of mice received the same treatment as hematoxylin-eosin staining.Immunostaining was performed to evaluate the healing state at the molecular level, angiogenesis-related markers CD31 (1: 300, GB113151, Servicebio), VEGF (1: 100, GB13034, Servicebio) and neuronal markers GAP43 (1: 200, GB11195, Servicebio) and PGP9.5 (1: 1000, GB12159, Servicebio). Glial cells and neuronal protein markers MBP (1: 200, GB11226, Servicebio), Tuj1 (1: 600, GB15139, Servicebio) and S100Β (1: 1000, GB12359, Servicebio) were also assessed to determine the wound healing state at the molecular level.Immunostaining was performed to evaluate the wound healing state at the molecular level. Images were recorded by Pannoramic MIDI (3DHISTECH, Hungary) and subsequently quantified using Image J analysis software. The density of skin staining-positive areas was quantified and the results were expressed as the percentage of matrix covered by the positive area.
[0063] 1.19 Statistical analysis
[0064] All results are expressed as mean ± SD (n ≥ 3). ANOVA with multiple comparisons (Prism 8 GraphPad) was used for significance testing. Significance levels are indicated by asterisks (*P < 0.05, **P < 0.01, ***P < 0.001, and ****P < 0.0001)
[0065] 2 Results and discussion
[0066] 2.1 Preparation and evaluation of ker-PA / Zn hydrogel
[0067] The keratin solution and the PA / Zn complex solution were simply mixed at room temperature to prepare the keratin-PA / Zn hydrogel. The PA / Zn complex was formed by dynamic cross-linking between Zn ions and catechol groups in PA, which was confirmed by UV-vis absorption spectroscopy ( Figure 2 A). PA exhibits two absorption peaks at 278 and 313 nm, which is due to the presence of an aromatic ring connected to two phenolic hydroxyl groups and a carbonyl group. For the PA / Zn complex, due to Zn 2+ The coordination caused the absorption peak of PA molecules to red-shift, and a clear peak appeared at 344 nm
[18] . PA / Zn complex and keratin formed hydrogels through a reversible thiol-aldehyde addition reaction between the thiol groups in keratin and the aldehyde groups in PA
[19] . Figure 2 B shows digital photographs and SEM images of keratin-PA / Zn hydrogels with keratin concentration of 18 w / v% and PA / Zn composite concentrations of 0.1, 0.2, and 0.3 w / v%. All hydrogels showed porous microstructures with average pore sizes ranging from ∼60 to 110 μm ( Figure 2 C). The swelling rate of the hydrogels follows a similar trend to the pore size. Larger pore sizes lead to increased swelling rates of the hydrogels ( Figure 2 D).
[0068] Figure 2 E and Figure 2 F shows that ker-PA / Zn hydrogel has good adhesion ability. It can adhere to the bent finger joints without falling off, and can also adhere to other materials such as glass, plastic and metal, which is mainly due to the presence of catechol and aldehyde groups in PA. The dynamic cross-linking structure gives the hydrogel good elasticity, injectability and self-healing properties. Figure 2 G shows the hydrogel being compressed and stretched between fingers. After being compressed with fingers, the hydrogel can be stretched to more than 5 times its original height without obvious breakage, which means good elasticity. Rheological tests were performed to investigate the rheological properties of the hydrogel. The linear viscoelastic region of the hydrogel was determined, and a strain of 1% was selected for further rheological testing ( Figure 2 H). Figure 2I shows that at each frequency, the storage modulus (G') of the hydrogel is greater than the loss modulus (G"), verifying that the ker-PA / Zn hydrogel is elastic. The shear thinning properties of the hydrogel were also studied by rheological tests ( Figure 2 J). As the shear rate increases, the viscosity of the hydrogel decreases sharply, indicating that the hydrogel has obvious shear thinning behavior. This makes the hydrogel have excellent injectability. Figure 2 The inserted picture in J shows that the hydrogel can be easily injected into water through a 26-gauge syringe needle. Continuous cyclic strain tests show that under a high strain of 800%, the G' value of the hydrogel drops from ∼2000 Pa to ∼60 Pa, which is lower than G", indicating that the hydrogel network collapses. When the strain is reduced to 1%, the G' value almost returns to the initial level, which means that the hydrogel network has recovered. This collapse and recovery of the hydrogel network can be repeated for at least three cycles ( Figure 2 K). This result indicates that the hydrogel has good self-healing ability, which is further confirmed by macroscopic healing experiments ( Figure 2 L). The two parts of the hydrogel disc can be reconnected after 30 minutes of contact and maintain integrity when stretched after healing. The results show that ker-PA / Zn hydrogel has excellent injectability, tissue adhesion and self-healing properties, which is expected to meet the practical application of hydrogel as wound dressing.
[0069] 2.2 Drug release, antimicrobial ability and biocompatibility
[0070] PP was encapsulated with F127 / F68 mixed micelles to improve water solubility, and the drug loading was 2 μg / mL in the hydrogel. The release curve showed that after incubation in saline at 37°C for 48 hours, the cumulative release of PP reached about 36% ( Figure 3 A). Hemolysis test showed that the PA / Zn complex hydrogel with a concentration of 0.1-0.3% did not cause significant hemolysis, and the hemolysis rate was less than 5% ( Figure 3 B). Due to the presence of zinc ions, ker-PA / Zn hydrogel exhibited significant antibacterial ability against Staphylococcus aureus, as reflected by both inhibition zone and colony count tests. Figure 3 In C, the hydrogels with three PA / Zn complex concentrations showed obvious inhibition zones after 24 h of incubation, and the hydrogels with higher PA / Zn complex concentrations showed larger inhibition zones. The antibacterial ability of the hydrogels was quantitatively tested by colony counting assay ( Figure 3 D). The hydrogels with three PA / Zn composite concentrations achieved a high antibacterial rate close to 100% ( Figure 3E). The cytotoxicity of ker-PA / Zn hydrogels was evaluated by cell viability assay and live / dead assay using L929 mouse fibroblasts. CCK-8 assay showed that there was no significant difference in cell proliferation between the hydrogels with three PA / Zn complex concentrations and the PP-loaded hydrogels at 1, 3, and 5 days of incubation compared with the PBS group ( Figure 3 F). Live / dead staining assay confirmed that the number of live cells increased with increasing incubation time, while few dead cells were observed during the incubation period ( Figure 3 G).
[0071] 2.3 Evaluation of RSC96 cell migration and myelin regeneration in vitro
[0072] The innervation process is essential for high-quality wound repair [20-22]. Studies have shown that mature Schwann cells are able to form lamellipodia and promote axon extension [23-27]. They are also involved in domain differentiation and provide local structural and metabolic support for nerve regeneration and repair
[28] . In this work, a cell scratch test was performed to evaluate the effects of ker-PA / Zn 0.2 hydrogels, PP-loaded hydrogels (ker-PA / Zn / PP 0.2), and PP solutions (same concentration of 2 μg / ml, not encapsulated in F127 / F68 micelles) on Schwann cell migration in normal glucose and high glucose environments ( Figure 4 A and 4B). Cells without any treatment were set as controls. Under normal blood glucose conditions, ker-PA / Zn 0.2 and PP solutions significantly promoted cell migration and formed lamellipodia compared with the control group ( Figure 4 C). In particular, ker-PA / Zn / PP0.2 promoted complete cell binding in the center after 24 h of incubation. Cell migration assays were further performed on Schwann cells exposed to high glucose to evaluate the protective effect of the hydrogel. Compared with the glucose-free control group, the migration ability of cells in a high glucose environment was inhibited. In contrast, both ker-PA / Zn 0.2 and PP solutions resisted the inhibitory effect of glucose, and ker-PA / Zn / PP 0.2 was superior to either of them ( Figure 4 D).
[0073] The effect of ker-PA / Zn / PP 0.2 on Schwann cell glial expression was studied by immunofluorescence staining of neural-specific proteins such as Schwann cell surface markers (S100β) and myelin regeneration markers (Tuj1). The ker-PA / Zn 0.2 hydrogel and PP solution were set up for comparison. Compared with the control group, the expression levels of the three groups of protein markers were increased, among which the expression levels of the ker-PA / Zn / PP 0.2 group were significantly higher than those of the ker-PA / Zn 0.2 and PP solutions ( Figure 4E and 4F). In addition, cells in the ker-PA / Zn / PP 0.2 group showed a more stretched and elongated state, forming obvious lamellipodia ( Figure 4 F, marked by white arrows). The morphology of Schwann cells was further observed by staining the actin cytoskeleton with phalloidin ( Figure 4 G). The cells in the ker-PA / Zn / PP 0.2 group showed more elongated protrusions (lamellar protrusions) compared with the ker-PA / Zn 0.2 group and the PP group. The results showed that both ker-PA / Zn 0.2 and PP could promote Schwann cell migration under normal and even hyperglycemic conditions, while ker-PA / Zn / PP 0.2 could achieve better effects due to the synergistic effect of ker-PA / Zn0.2 and PP.
[0074] 2.4 Diabetes wound healing assay
[0075] The therapeutic efficacy of ker-PA / Zn 0.2 and ker-PA / Zn / PP 0.2 hydrogels was evaluated using a full-thickness diabetic wound model (~6 mm in diameter) in db / db mice and STZ-induced C57BL / 6 mice. Figure 5 A) Wounds treated with PBS were used as controls and rb-bFGF was used as a positive drug for comparison. Figure 5 B shows representative images of wounds in each group at 0, 2, 4, 6, and 9 days after wounding, and the corresponding quantitative wound healing rates were calculated based on these images ( Figure 5 C and 5D). For db / db mice and STZ-induced C57BL / 6 mice, ker-PA / Zn 0.2 hydrogels showed faster wound closure than controls after 2 days, with healing rates of 87.7% in db / db mice and 72.5% in C57BL / 6 mice. In contrast, wound healing rates of the control group were only 71.4% and 60.8%, respectively, at day 9. Notably, PP-loaded hydrogels further accelerated wound closure, with healing rates of db / db mice similar to those of the rb-bFGF group (94.0% vs. 96.2%) and even higher rates in C57BL / 6 mice than those of the rb-bFGF group (90.5% vs. 73.8%) at day 9.
[0076] 2.5 Epidermal and dermal remodeling in diabetic wounds
[0077] During wound healing, re-epithelialization is crucial for rebuilding the epidermal barrier. In this work, re-epithelialization of each wound group was evaluated by H&E staining on day 4 ( Figure 6 A). The results showed that the epidermal migration length of the ker-PA / Zn / PP 0.2 group on the 4th day was longer than that of the control group, ker-PA / Zn 0.2 and rb-bFGF groups ( Figure 6 B). The re-epithelialization process further accelerated wound healing, and the ker-PA / Zn / PP 0.2 group had the smallest wound width among all groups on day 9 ( Figure 6 C).
[0078] Collagen deposition and tissue remodeling also play an important role in restoring the tensile strength of tissue at the wound site
[29] . Masson staining was performed on days 4 and 9 to evaluate collagen deposition and tissue remodeling in each group ( Figure 6 D). Compared with the control group, ker-PA / Zn / PP 0.2 and ker-PA / Zn 0.2 both promoted collagen deposition, and the effect of ker-PA / Zn / PP0.2 was better than that of rb-bFGF ( Figure 6 E). In addition, compared with rb-bFGF, both ker-PA / Zn / PP 0.2 and ker-PA / Zn 0.2 stimulated the regeneration of dermal appendages at day 9 ( Figure 6 F) These results are consistent with other studies showing that both zinc ions and keratin can promote hair follicle regeneration[30,31].
[0079] 2.6 Repair of skin nerves in diabetic wounds
[0080] The effects of ker-PA / Zn / PP 0.2 on the expression of Schwann cell-glial markers were investigated by immunohistochemical staining for a myelin regeneration marker (Tuj1), a Schwann cell surface marker (S100β), and a nerve fiber myelination marker (MBP). Figure 7 A)
[32] . Compared with the control group, ker-PA / Zn 0.2 and ker-PA / Zn / PP 0.2 showed higher expression of Tuj1, S100β and MBP on days 4 and 9, respectively, especially in ker-PA / Zn / PP 0.2 hydrogel ( Figure 7 B-7D).
[0081] Studies have shown that diabetic wounds are characterized by a decrease in axonal distribution marked by growth-associated protein 43 (GAP43)[33,34] and axonal loss marked by protein gene product 9.5 (PGP9.5)
[35] . The effects of ker-PA / Zn / PP 0.2 hydrogel on axonal regeneration were evaluated by immunohistochemical staining for axonal markers GAP43 and PGP9.5. Figure 8 A). The results showed that on the 4th and 9th days, the expression levels of GAP43 and PGP9.5 in ker-PA / Zn 0.2 hydrogel were higher than those in the control group ( Figure 8B and 8C). At the same time, the expression of GAP43 and PGP9.5 in ker-PA / Zn / PP 0.2 hydrogel was further increased compared with ker-PA / Zn 0.2, and the expression of GAP43 and PGP9.5 was higher or similar compared with the rb-bFGF group. These results indicate that ker-PA / Zn / PP 0.2 hydrogel promotes the regeneration of damaged nerves, which is mainly due to its effects on the activation, migration and myelination of Schwann cells [13,36].
[0082] 2.7 Neoangiogenesis in diabetic wounds
[0083] Neovascularization plays a key role in delivering nutrients and oxygen to the wound during the proliferative phase, thereby promoting fibroblast proliferation, collagen synthesis, re-epithelialization, and neurogenesis [37,38]. The effect of the hydrogel on neovascularization was evaluated by immunohistochemical staining of platelet endothelial cell adhesion molecule-1 (CD31) and vascular endothelial growth factor (VEGF) in granulation tissue ( Fig. 9 A). Quantitative analysis showed that ker-PA / Zn 0.2 increased the expression of CD31 and VEGF on days 4 and 9 compared with the control, indicating that zinc ions have a certain effect on angiogenesis. In addition, ker-PA / Zn / PP0.2 obtained the highest expression of CD31 and VEGF on day 4 among all groups ( Fig. 9 B and 9C), indicating that mixed micelles of PP can promote angiogenesis. According to the literature, angiogenesis can stimulate axon regeneration in chronic diabetic ulcers with axonal defects by supporting the increased metabolic demands of neurons, thereby accelerating wound healing
[38] .
[0084] In the present invention, we invented a protein-based functional hydrogel with injectability, skin adhesion, self-healing and antibacterial ability for diabetic wound repair. Mixed micelles of choriocarpa lactone (a natural compound extracted from the traditional Chinese medicine Angelica dahurica) were first shown to accelerate skin nerve regeneration and angiogenesis in diabetic full-thickness wounds. In addition, due to the synergistic effect of choriocarpa lactone and zinc ions, the therapeutic effect of choriocarpa lactone-loaded hydrogel on diabetic wound healing was superior to rb-bFGF. These results indicate that choriocarpa lactone-loaded hydrogel can be used as an ideal hydrogel dressing for diabetic wound treatment.
[0085] References
[0086] [1]McDermott,K.;Fang,M.;Boulton,A.J.M.;Selvin,E.;Hicks,C.W.Etiology,Epidemiology,and Disparities in theBurden of Diabetic Foot Ulcers.DiabetesCare 2023,46,209-221.
[0087] [2]Reiber,G.E.;Pecoraro,R.E.;Koepsell,T.D.Risk factors for amputationin patients with diabetes mellitus Acase-control study.Annals of internalmedicine 1992,117,97-105.
[0088] [3]McNeely,M.J.;Boyko,E.J.;Ahroni,J.H.;Stensel,V.L.;Reiber,G.E.;Smith,D.G.;Pecoraro,R.F.The independentcontributions of diabetic neuropathyand vasculopathy in foot ulceration.How great are the risks?Diabetes Care1995,18,216-219.
[0090] [4]Reiber,G.E.;Vileikyte,L.;Boyko,E.J.;del Aguila,M.;Smith,D.G.;Lavery,L.A.;Boulton,A.J.Causal pathways forincident lower-extremity ulcers inpatients with diabetes from two settings.Diabetes Care 1999,22,157-162.
[0091] [5]Ahmed,E.M.Hydrogel:Preparation,characterization,and applications:Areview.J Adv Res 2015,6,105-121.
[0092] [6]Liang,Y.P.;He,J.H.;Guo,B.L.Functional Hydrogels as Wound Dressingto Enhance Wound Healing.ACS NANO2021,15,12687-12722.
[0094] [7]Ma,X.;Liu,B.;Fan,L.;Liu,Y.;Zhao,Y.;Ren,T.;Li,Y.;Li,Y.Native andengineered exosomes for inflammatory disease.
[0095] Nano Res 2023,16,6991-7006.
[0096] [8]Xu,Z.;Liu,G.;Li,Q.;Wu,J.A novel hydrogel with glucose-responsivehyperglycemia regulation and antioxidantactivity for enhanced diabetic woundrepair.Nano Research 2022,15,5305-5315.
[0097] [9]Ji,Z.;Wei,T.;Zhu,J.;Hu,J.;Xiao,Z.;Bai,B.;Lv,X.;Miao,Y.;Chen,M.;Wang,C.;Pan,F.;Yang,Y.;Li,M.;Chen,Q.
[0098] Actively contractible and antibacterial hydrogel for acceleratedwound healing.Nano Research 2024,
[0099] 10.1007 / s12274-024-6674-6.
[0100]
[10] Yoo,M.C.;Chon,J.;Jung,J.;Kim,S.S.;Bae,S.;Kim,S.H.;Yeo,S.G.Potential Therapeutic Strategies and Substancesfor Facial NerveRegeneration Based on Preclinical Studies.Int J Mol Sci 2021,22.
[0101]
[11] Ye,W.;Qin,M.;Qiu,R.;Li,J.Keratin-based wound dressings:From wasteto wealth.Int J Biol Macromol 2022,211,183-197.
[0103]
[12] Chen,Y.,YingYang,XuexiaCao,ZhangjunNie,HualiBian,YonggangYang,Guang Glucose-triggered in situ formingkeratin hydrogel for the treatment ofdiabetic wounds.Acta biomaterialia 2021,125.
[0104]
[13] Zhang,H.;Ma,W.;Ma,H.;Qin,C.;Chen,J.;Wu,C.Spindle-Like ZincSilicate Nanoparticles Accelerating Innervated andVascularized Skin BurnWound Healing.Adv Healthc Mater 2022,11,e2102359.
[0105]
[14] Gan,D.;Xing,W.;Jiang,L.;Fang,J.;Zhao,C.;Ren,F.;Fang,L.;Wang,K.;Lu,X.Plant-inspired adhesive and toughhydrogel based on Ag-Ligninnanoparticles-triggered dynamic redox catechol chemistry.Nat Commun 2019,10,1487.
[15] Geng,H.;Zhong,Q.-Z.;Li,J.;Lin,Z.;Cui,J.;Caruso,F.;Hao,J.Metal Ion-Directed Functional Metal–Phenolic Materials.
[0106] Chemical Reviews 2022,122,11432-11473.
[0107]
[16] Zhang,Q.;Huang,K.;Tan,J.;Lei,X.;Huang,L.;Song,Y.;Li,Q.;Zou,C.;Xie,H.Metal-phenolic networks modifiedpolyurethane as periosteum for boneregeneration.Chinese Chemical Letters 2022,33,1623-1626.
[0108]
[17] Sun,C.;Li,W.;Ma,P.;Li,Y.;Zhu,Y.;Zhang,H.;Adu-Frimpong,M.;Deng,W.;Yu,J.;Xu,X.Development ofTPGS / F127 / F68 mixed polymeric micelles:Enhanced oralbioavailability and hepatoprotection of syringic acid againstcarbontetrachloride-induced hepatotoxicity.Food Chem Toxicol 2020,137,111126.
[0109]
[18] Huang,Y.;Gao,Q.;Li,C.;Chen,X.;Li,X.;He,Y.;Jin,Q.;Ji,J.FacileSynthesis of Zn2+-Based Hybrid Nanoparticles as aNew Paradigm for theTreatment of Internal Bacterial Infections.Advanced Functional Materials2021,32.
[0110]
[19] Hua,Y.;Gan,Y.;Zhang,Y.;Ouyang,B.;Tu,B.;Zhang,C.;Zhong,X.;Bao,C.;Yang,Y.;Lin,Q.;Zhou,Q.;Zhu,L.Adaptableto Mechanically Stable Hydrogels Basedon the Dynamic Covalent Cross-Linking of Thiol-Aldehyde Addition.ACSMacroLetters 2019,8,310-314.
[0111]
[20] Cheng,C.;Singh,V.;Krishnan,A.;Kan,M.;Martinez,J.A.;Zochodne,D.W.Loss of innervation and axon plasticityaccompanies impaired diabeticwound healing.PLoS One 2013,8,e75877.
[0112]
[21] Li,Q.;Jiao,L.;Shao,Y.;Li,M.;Zhang,Y.Topical GDF11 acceleratesskin wound healing in both type 1 and 2 diabeticmouse models.Biochemical andBiophysical Research Communications 2020,529,7-14.
[0113]
[22] Theocharidis,G.;Veves,A.Autonomic nerve dysfunction and impaireddiabetic wound healing:The role ofneuropeptides.Auton Neurosci 2020,223,102610.
[0114]
[23] Nodari,A.;Zambroni,D.;Quattrini,A.;Court,F.A.;D"Urso,A.;Recchia,A.;Tybulewicz,V.L.J.;Feltri,L.W.L.β1
[0115] Integrin Activates Rac1 in Schwann Cells to Generate Radial Lamellaeduring Axonal Sorting and Myelination.Journalof Cell Biology 2007,177,1063-1075.
[0116]
[24] Colombelli,C.;Zambroni,D.;Occhi,S.;Wrabetz,L.;Feltri,M.L.ROLE OFSCHWANN CELL DYSTROGLYCAN INTHE ARCHITECTURE OF NODES OF RANVIER.Journal ofthe Peripheral Nervous System 2009,36-36.
[0117]
[25] Jin,F.;Dong,B.;Georgiou,J.;Jiang,Q.;Zhang,J.;Bharioke,A.;Qiu,F.;Lommel,S.;Feltri,M.L.;Wrabetz,L.N-WASp isrequired for Schwann cellcytoskeletal dynamics,normal myelin gene expression and peripheral nervemyelination.
[0118] Development 2011.
[0119]
[26] Tello Velasquez,J.;Nazareth,L.;Quinn,R.J.;Ekberg,J.A.;St John,J.A.Stimulating the proliferation,migration andlamellipodia of Schwann cellsusing low-dose curcumin.Neuroscience 2016,324,140-150.
[0120]
[27] Ness,J.K.;Snyder,K.M.;Tapinos,N.Lck tyrosine kinase mediatesbeta1-integrin signalling to regulate Schwann cellmigration andmyelination.Nat Commun 2013,4,1912.
[0121]
[28] Taveggia,C.;Feltri,M.L.Beyond Wrapping:Canonical and NoncanonicalFunctions of Schwann Cells.Annu RevNeurosci 2022,45,561-580.
[0122]
[29] Wang,C.;Wang,Q.;Gao,W.;Zhang,Z.;Lou,Y.;Jin,H.;Chen,X.;Lei,B.;Xu,H.;Mao,C.Highly efficient local deliveryof endothelial progenitor cellssignificantly potentiates angiogenesis and full-thickness woundhealing.ActaBiomaterialia 2018.
[0123]
[30] Zhang,Z.;Li,W.;Chang,D.;Wei,Z.;Wang,E.;Yu,J.;Xu,Y.;Que,Y. ;Chen,Y.;Fan,C.;Ma,B.;Zhou,Y.;Huan,Z.;Yang,C.;Guo,F.;Chang,JA combination therapy for androgenic alopecia based on quercetin and zinc / copper dual-doped mesoporous silica nanocomposite microneedle patch. Bioact Mater 2023,24,81-95.
[0124]
[31] Hu,S.;Li,Z.;Lutz,H.;Huang,K.;Su,T.;Cores,J.;Dinh,PC;Cheng,K.Dermal exosomes containing miR-218-5promote hair regeneration by regulating beta-catenin signaling.Sci Adv 2020,6,eaba1685.
[0125]
[32] Feliu, A. Bonilla Del Rio, I. Carrillo-Salinas, F. J. Hernandez-Torres, G. Mestre, L. Puente, N. Ortega-Gutierrez, S. Lopez-Rodriguez, ML Grandes, P. Mecha, M. Guaza, C. 2-Arachidonoylglycerol Reduces Proteoglycans and Enhances Remyelination in a Progressive Model of Demyelination. J Neurosci 2017, 37, 8385-8398.
[0126]
[33] Fantini,F.;Johansson,O.Expression of growth-associated protein 43and nerve growth factor receptor in human skin:acomparativeimmunohistochemical investigation.J Invest Dermatol 1992,99,734-742.
[0127]
[34] Pradhan,L.;Nabzdyk,C.;Andersen,N.D.;LoGerfo,F.W.;Veves,A.Inflammation and neuropeptides:the connection indiabetic woundhealing.Expert Rev Mol Med 2009,11,e2.
[0128]
[35] Boyette-Davis,J.;Xin,W.;Zhang,H.;Dougherty,P.M.Intraepidermalnerve fiber loss corresponds to the developmentof taxol-induced hyperalgesiaand can be prevented by treatment with minocycline.Pain 2011,152,308-313.
[0129]
[36] Xuan,Y.;Li,L.;Yin,X.;He,D.;Li,S.;Zhang,C.;Yin,Y.;Xu,W.;Zhang,Z.Bredigite-Based Bioactive Nerve GuidanceConduit for Pro-Healing MacrophagePolarization and Peripheral Nerve Regeneration.Adv Healthc Mater 2024,13,
[0130] e2302994.
[0131]
[37] Okonkwo,U.A.;DiPietro,L.A.Diabetes and Wound Angiogenesis.Int JMol Sci 2017,18.
[0132]
[38] Nowak,N.C.;Menichella,D.M.;Miller,R.;Paller,A.S.Cutaneousinnervation in impaired diabetic wound healing.
[0133] Transl Res 2021,236,87-108.
[0134]
[39] SHI T,LU H,ZHU J,et al.Naturally derived dual dynamic crosslinkedmultifunctional hydrogel for diabetic woundhealing[J].Composites Part B:Engineering,2023,257.
[0135]
[40] ZHAO L,DU J,DUAN Y,et al.Curcumin loaded mixed micelles composedof Pluronic P123 and F68:Preparation,
[0136] optimization and in vitro characterization[J].Colloids and SurfacesB:Biointerfaces,2012,97:101-8.
[0137]
[41] SUN C,LI W,MA P,et al.Development of TPGS / F127 / F68 mixedpolymeric micelles:Enhanced oral bioavailabilityand hepatoprotection ofsyringic acid against carbon tetrachloride-induced hepatotoxicity[J].Food andChemicalToxicology,2020,137.
[0138]
[42] THAPA RK,CAZZADOR F, KG,et al.Effect of curcumin andcosolvents on the micellization of PluronicF127 in aqueous solution[J].Colloids and Surfaces B:Biointerfaces,2020,195.
[0139] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the method of the present invention. These improvements and supplements should also be regarded as the scope of protection of the present invention.
Claims
1. A natural protein-based functional hydrogel, characterized in that: The hydrogel comprises keratin, protocatechuic aldehyde and zinc ions. The hydrogel is prepared by dual dynamic cross-linking reaction of thiol-aldehyde addition and catechol-zinc ion coordination using keratin as a matrix and protocatechuic aldehyde and zinc ions as building blocks.
2. The hydrogel according to claim 1, characterized in that The keratin is a natural protein rich in cysteine.
3. A ker-PA / Zn hydrogel loaded with choriocarp lactone, characterized in that: The ker-PA / Zn hydrogel loaded with choriocarpa lactone comprises choriocarpa lactone, F127 / F68 and the hydrogel according to any one of claims 1 or 2.
4. The ker-PA / Zn hydrogel loaded with chorioalveolar lactone according to claim 3, characterized in that: The ker-PA / Zn hydrogel loaded with keratin lactone is a keratin lactone encapsulated in F127 / F68 mixed micelles and loaded into the hydrogel according to any one of claims 1 or 2.
5. Use of the hydrogel according to claim 1 or 2 in the preparation of drugs for promoting nerve repair or diabetic wound healing.
6. Use of the ker-PA / Zn hydrogel loaded with choriophyllide according to claim 4 or 5 in the preparation of a drug for promoting nerve repair or diabetic wound healing.