Preparation method of titanium oxide ceramic nanofiltration membrane
The synthesis of titanium oxide nanoparticles by microwave hydrothermal method was solved, and the volume shrinkage caused by crystallization water in the sol-gel method and the long-term cycle of hydrothermal method was prepared, and a high-performance ceramic nanofiltration membrane was prepared, which improved mechanical strength and production efficiency. , reduces costs.
Patent Information
- Application Number
- CN202410964181.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-22
AI Technical Summary
In the existing ceramic nanofiltration membrane preparation methods, the sol-gel method causes nanoparticles to contain high crystallization water, resulting in volume shrinkage during calcination, affecting the structural integrity and performance of the membrane layer. The hydrothermal method has a long preparation cycle and production. Inefficient, increasing costs.
The titanium oxide nanoparticles were synthesized by microwave hydrothermal method. By mixing organic titanium salt, water and diethanolamine at room temperature, adding dispersant and polyethylene glycol, microwave hydrothermal reaction was carried out to form a uniform titanium oxide nano solution, and The coating liquid on the porous alumina ceramic membrane support was dried and calcined to prepare a high-quality titanium oxide ceramic nanofiltration membrane.
The uniformity and crystal shape of nanoparticles are achieved, the mechanical strength and separation performance of the film layer are improved, the production steps are simplified, the production costs are reduced, and the heating speed is fast and the uniformity is good, avoiding the traditional hydrothermal method. Lag effect.
Smart Images

Figure CN118988005A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nanofiltration membrane preparation, and specifically relates to a method for preparing a titanium oxide ceramic nanofiltration membrane. Background Art
[0002] Nanofiltration membrane is an important type of filtration material. According to the different materials, it is mainly divided into two categories: organic nanofiltration membrane and ceramic nanofiltration membrane. Organic nanofiltration membrane has been widely used in the market due to its advantages such as low preparation cost and simple method, and its commercialization degree is relatively high. However, due to the limitations of the material itself, the performance of organic nanofiltration membranes in acid and alkali resistance, high temperature resistance and solvent resistance is not satisfactory, which makes them more suitable for applications in mild systems.
[0003] In contrast, ceramic nanofiltration membranes have shown more excellent performance. They can not only withstand organic solvents, high temperatures and acid-base environments, but also have the characteristics of high mechanical strength, large flux and long service life. These characteristics make ceramic nanofiltration membranes more and more widely used in many industries such as chemical, energy, electronics, food and medicine.
[0004] In the existing technology, the preparation of nanoparticles for ceramic nanofiltration membranes mainly adopts the sol-gel method. This method can prepare nanoparticles with small and uniform particle size, which is crucial for forming a uniform film layer. However, the sol-gel method also has some disadvantages in the preparation process. In particular, the nanoparticles prepared by this method contain a high amount of crystal water, which easily leads to a large volume shrinkage during the calcination process. This shrinkage may not only affect the structural integrity of the membrane layer, but also cause cracks, thereby reducing the performance of the membrane.
[0005] The hydrothermal method is another commonly used method for preparing nanoparticles. Compared with the sol-gel method, the nanoparticles prepared by the hydrothermal method are more crystalline and contain less crystalline water, which helps to reduce the volume shrinkage during calcination. However, the hydrothermal method also has some limitations. First, the prepared particles are larger in size, which may affect the filtration performance of the membrane. Second, the preparation cycle of the hydrothermal method is longer, which limits the production efficiency and increases the production cost. Summary of the invention
[0006] The present invention aims to overcome the defects of the prior art and provide a method for preparing a titanium oxide ceramic nanofiltration membrane.
[0007] The technical solution of the present invention is as follows:
[0008] A method for preparing a titanium oxide ceramic nanofiltration membrane comprises the following steps:
[0009] (1) mixing an organic titanium salt, diethanolamine and water in a molar ratio of 1:1:10-100, stirring at room temperature for 10-30 minutes, and then performing solid-liquid separation, adding water to the obtained solid and stirring it evenly, adding nitric acid, adjusting the pH to 1-2, continuing to stir for 30 minutes, and then heating and stirring at 75-85° C. for 2-4 hours to obtain a transparent titanium oxide sol;
[0010] (2) adding a dispersant to the titanium oxide sol obtained in step (1), stirring the mixture evenly, placing the mixture in a microwave hydrothermal reaction system, wherein the filling degree of the hydrothermal reactor is 50-80%, and reacting the mixture under a pressure of 0.5-2 MPa for 1-3 h, cooling the mixture, and obtaining a titanium oxide nano-solution with uniform particles;
[0011] (3) adding polyethylene glycol with a weight average molecular weight of 350-450 and a cellulose compound with a molecular weight of 6000-10000 to the titanium oxide nano-solution obtained in step (2), and then adding an organosilicon defoamer BYK028, mixing well, and obtaining a coating solution;
[0012] (4) Apply the coating liquid obtained in step (3) on the porous alumina ceramic membrane support, heat to 80-120°C at a humidity of 30-40%, keep warm and dry for 2-5 hours, then heat to 350-600°C and calcine for 2-5 hours, and cool to obtain the titanium oxide ceramic nanofiltration membrane.
[0013] In a preferred embodiment of the present invention, the organic titanium salt is n-butyl titanate or isopropyl titanate.
[0014] More preferably, the organic titanium salt is n-butyl titanate.
[0015] In a preferred embodiment of the present invention, the dispersant is PEG400 or glycerol.
[0016] Further preferably, the dispersant is glycerol.
[0017] In a preferred embodiment of the present invention, the cellulose compound is hydroxymethyl cellulose, hydroxyethyl cellulose or hydroxypropyl cellulose.
[0018] More preferably, the cellulose compound is hydroxymethyl cellulose.
[0019] In a preferred embodiment of the present invention, the organic titanium salt is n-butyl titanate, the dispersant is glycerol, and the cellulose compound is hydroxymethyl cellulose.
[0020] In a preferred embodiment of the present invention, in the step (2), the dispersant is added to a final concentration of 1-3wt%; in the step (2), the second dispersant is added to a final concentration of 1wt%; in the step (3), the polyethylene glycol and the cellulose compound are added to final concentrations of 3-10wt% and 0.1-1wt%, respectively, and the organosilicon defoamer is added to a final concentration of 0.01-0.1wt%.
[0021] Further preferably, the step (4) is: applying the coating liquid prepared in step (3) on the porous alumina ceramic membrane support, heating to 80-120°C at a rate of 1-3°C / min at a humidity of 30-40%, and drying for 2-5 hours, then heating to 350-600°C at a rate of 1-5°C / min, calcining for 2-5 hours, and cooling to obtain the titanium oxide ceramic nanofiltration membrane.
[0022] The beneficial effects of the present invention are:
[0023] 1. The microwave hydrothermal synthesis method adopted in the present invention has achieved a significant technological breakthrough by introducing microwave radiation technology on the basis of the traditional hydrothermal method. This method has significant advantages such as fast heating speed, uniform heating, and no hysteresis effect. The uniform heating characteristics of microwaves ensure the consistency of temperature during the reaction process, thereby improving the reaction efficiency and the quality of the product.
[0024] 2. The titanium dioxide powder prepared by the microwave hydrothermal method of the present invention not only has uniform particle size, but also has complete crystal development and avoids agglomeration. These characteristics are crucial for preparing high-performance nanofiltration membranes. By adding an appropriate amount of additives to the prepared nanoparticle sol, the viscosity and concentration of the coating liquid can be adjusted to make it more suitable for the coating process. This adjustment not only improves the uniformity and density of the film layer, but also enhances the mechanical strength and separation performance of the membrane.
[0025] 3. The present invention applies a specially prepared coating liquid to a porous support, forms a uniform gel film through coating treatment, and then undergoes drying and sintering to finally prepare a high-quality nanofiltration membrane. This process not only simplifies the production steps, but also improves production efficiency and significantly reduces production costs.
[0026] 4. Compared with the traditional sol-gel method, the microwave hydrothermal method of the present invention has obvious advantages in heating speed and uniformity. The sol-gel method usually takes a long time to complete the gelation and drying process, while the microwave hydrothermal method of the present invention can complete these steps in a short time. In addition, the microwave hydrothermal method of the present invention avoids the hysteresis effect common in the traditional hydrothermal method, ensuring the continuity and consistency of the entire reaction process.
[0027] 5. Compared with the hydrothermal method, the microwave hydrothermal method of the present invention reduces the dependence on equipment during the preparation process, is easier to operate, and also reduces energy consumption. The hydrothermal method needs to be carried out under high pressure, which places high demands on both equipment and operators. The microwave hydrothermal method of the present invention can be carried out under lower pressure, is safer to operate, and has lower maintenance costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a scanning electron microscope photograph of the membrane layer of the titanium oxide ceramic nanofiltration membrane prepared in Example 1 of the present invention.
[0029] Figure 2 This is a scanning electron microscope photograph of the membrane layer of the comparative ceramic nanofiltration membrane prepared in Comparative Example 1 of the present invention.
[0030] Figure 3 This is a scanning electron microscope photograph of the membrane layer of the comparative ceramic nanofiltration membrane prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0031] The technical solution of the present invention is further illustrated and described below through specific implementation modes in combination with the accompanying drawings.
[0032] Example 1
[0033] (1) n-butyl titanate, diethanolamine and water were mixed in a molar ratio of 1:1:50, stirred at room temperature for 30 minutes, and then filtered to remove impurities. The filter cake was stirred evenly with water, nitric acid was added, the pH was adjusted to 1.5, and stirring was continued for 30 minutes. Then, heating and stirring were performed at 80° C. for 3 hours to obtain a transparent titanium oxide sol.
[0034] (2) adding 1% glycerol to the titanium oxide sol obtained in step (1), stirring evenly, placing the mixture in a microwave hydrothermal reaction system, with the filling degree of the hydrothermal reactor being 60%, and reacting at a pressure of 0.5 MPa for 2 h, cooling the mixture, and obtaining a titanium oxide nano-solution with uniform particles;
[0035] (3) adding PEG-400 and hydroxymethyl cellulose with a molecular weight of 6000-10000 to the titanium oxide nano-solution prepared in step (2) to a final concentration of 5 wt % and 0.5 wt %, respectively, and then adding silicone defoamer BYK028 to a final concentration of 0.05 wt %, and mixing to prepare a coating solution;
[0036] (4) The coating liquid prepared in step (3) is applied to a porous alumina ceramic membrane support having an average pore size of 5 nm, and the temperature is raised to 100° C. at a rate of 2° C. / min at a humidity of 40%, and the temperature is kept warm and dried for 3 h, and then the temperature is raised to 500° C. at a rate of 2° C. / min, and the temperature is kept warm and calcined for 3 h, and cooled to obtain the ceramic nanofiltration membrane. The membrane layer is intact and has no defects (such as Figure 1As shown). Under the test conditions of room temperature and 0.69 MPa, the rejection rate of 0.1% PEG1000 solution is 95% and the flux is 45 LHM.
[0037] Example 2
[0038] (1) n-butyl titanate, diethanolamine and water were mixed in a molar ratio of 1:1:50, stirred at room temperature for 30 minutes, and then filtered to remove impurities. The filter cake was stirred evenly with water, nitric acid was added, the pH was adjusted to 1.5, and stirring was continued for 30 minutes. Then, heating and stirring were performed at 80° C. for 3 hours to obtain a transparent titanium oxide sol.
[0039] (2) adding 1% glycerol to the titanium oxide sol obtained in step (1), stirring evenly, placing the sol in a microwave hydrothermal reaction system, filling the hydrothermal reactor with a degree of 60%, keeping the reaction temperature at 1 MPa for 2 h, cooling, and obtaining a titanium oxide nano-solution with uniform particles;
[0040] (3) adding PEG-400 and hydroxymethyl cellulose with a molecular weight of 6000-10000 to the titanium oxide nano-solution prepared in step (2) to a final concentration of 5 wt % and 0.5 wt %, respectively, and then adding silicone defoamer BYK028 to a final concentration of 0.05 wt %, and mixing to prepare a coating solution;
[0041] (4) The coating liquid prepared in step (3) is applied to a porous alumina ceramic membrane support having an average pore size of 5 nm, and the temperature is raised to 100° C. at a rate of 2° C. / min at a humidity of 40%, and the membrane is kept warm and dried for 3 hours, and then the temperature is raised to 500° C. at a rate of 2° C. / min, and the membrane is kept warm and calcined for 3 hours, and then cooled to obtain the ceramic nanofiltration membrane. Under the test conditions of room temperature and 0.69 MPa, the retention rate of 0.1% PEG1000 solution is 93%, and the flux is 50 LHM.
[0042] Example 3
[0043] (1) n-butyl titanate, diethanolamine and water were mixed in a molar ratio of 1:1:50, stirred at room temperature for 30 minutes, and then filtered to remove impurities. The filter cake was stirred evenly with water, nitric acid was added, the pH was adjusted to 1.5, and stirring was continued for 30 minutes. Then, heating and stirring were performed at 80° C. for 3 hours to obtain a transparent titanium oxide sol.
[0044] (2) adding 1% glycerol to the titanium oxide sol obtained in step (1), stirring evenly, placing the sol in a microwave hydrothermal reaction system, filling the hydrothermal reactor with a degree of 60%, keeping the reaction temperature at 1 MPa for 2 h, cooling, and obtaining a titanium oxide nano-solution with uniform particles;
[0045] (3) adding PEG-400 and hydroxymethyl cellulose with a molecular weight of 6000-10000 to the titanium oxide nano-solution prepared in step (2) to a final concentration of 5 wt % and 0.5 wt %, respectively, and then adding silicone defoamer BYK028 to a final concentration of 0.05 wt %, and mixing to prepare a coating solution;
[0046] (4) The coating liquid prepared in step (3) is applied to a porous alumina ceramic membrane support having an average pore size of 5 nm, and the temperature is raised to 100° C. at a rate of 2° C. / min at a humidity of 40%, and the membrane is kept warm and dried for 3 hours, and then the temperature is raised to 500° C. at a rate of 2° C. / min, and the membrane is kept warm and calcined for 3 hours, and then cooled to obtain the ceramic nanofiltration membrane. Under the test conditions of room temperature and 0.69 MPa, the retention rate of 0.1% PEG1000 solution is 90%, and the flux is 53 LHM.
[0047] Comparative Example 1
[0048] (1) n-butyl titanate, diethanolamine and water were mixed in a molar ratio of 1:1:50, stirred at room temperature for 30 minutes, and then filtered to remove impurities. The filter cake was stirred evenly with water, nitric acid was added, the pH was adjusted to 1.5, and stirring was continued for 30 minutes. Then, heating and stirring were performed at 80° C. for 3 hours to obtain a transparent titanium oxide sol.
[0049] (2) adding PEG-400 and hydroxymethyl cellulose with a molecular weight of 6000-10000 to the titanium oxide sol prepared in step (1) to a final concentration of 5 wt% and 0.5 wt%, respectively, and then adding silicone defoamer BYK028 to a final concentration of 0.05 wt%, and mixing to prepare a coating solution;
[0050] (3) The coating liquid prepared in step (2) is applied to a porous alumina ceramic membrane support with an average pore size of 5 nm, and the temperature is raised to 100°C at a rate of 2°C / min at a humidity of more than 65%, and the mixture is kept warm and dried for 3 hours. The temperature is then raised to 500°C at a rate of 3°C / min, and the mixture is kept warm and calcined for 3 hours. The mixture is cooled to obtain a comparative ceramic nanofiltration membrane.
[0051] The ceramic nanofiltration membrane is prone to cracks (such as Figure 2 As shown), under the test conditions of room temperature and 0.69 MPa, the retention rate of 0.1% PEG1000 solution is 0 and the flux is 102 LHM.
[0052] Comparative Example 2
[0053] (1) n-butyl titanate, diethanolamine and water were mixed in a molar ratio of 1:1:50, stirred at room temperature for 30 minutes, and then filtered to remove impurities. The filter cake was stirred evenly with water, nitric acid was added, the pH was adjusted to 1.5, and stirring was continued for 30 minutes. Then, heating and stirring were performed at 80° C. for 3 hours to obtain a transparent titanium oxide sol.
[0054] (2) placing the titanium oxide sol obtained in step (1) into a hydrothermal reactor with a filling degree of 60%, reacting at 200° C. for 10 h, and cooling to obtain a titanium oxide nano-solution with uniform particles;
[0055] (3) adding PEG-400 and hydroxymethyl cellulose with a molecular weight of 6000-10000 to the titanium oxide nano-solution prepared in step (2) to a final concentration of 5 wt % and 0.5 wt %, respectively, and then adding silicone defoamer BYK028 to a final concentration of 0.05 wt %, and mixing to prepare a coating solution;
[0056] (4) The coating liquid prepared in step (3) is applied to a porous alumina ceramic membrane support having an average pore size of 5 nm, and the temperature is raised to 100°C at a rate of 2°C / min at a humidity of 40%, and the membrane is kept warm and dried for 3 hours. The temperature is then raised to 500°C at a rate of 2°C / min, and the membrane is kept warm and calcined for 3 hours. The membrane is cooled to obtain a comparative ceramic nanofiltration membrane.
[0057] The membrane layer of the comparative ceramic nanofiltration membrane is intact (eg Figure 3 As shown), under the test conditions of room temperature and 0.69 MPa, the retention rate of 0.1% PEG1000 solution is 35% and the flux is 70 LHM.
[0058] Comparative Example 3
[0059] (1) n-butyl titanate, diethanolamine and water were mixed in a molar ratio of 1:1:50, and stirred at room temperature for 30 minutes to mix evenly. The titanium oxide solution was placed in a microwave hydrothermal reaction system, the filling degree of the hydrothermal reactor was 60%, and the reaction was carried out at a pressure of 0.5 MPa for 2 hours, and then cooled to obtain a titanium oxide nano solution;
[0060] (2) adding PEG-400 and hydroxymethyl cellulose with a molecular weight of 6000-10000 to the titanium oxide nano-solution prepared in step (1) to a final concentration of 5 wt % and 0.5 wt %, respectively, and then adding silicone defoamer BYK028 to a final concentration of 0.05 wt %, and mixing to prepare a coating solution;
[0061] (3) The coating liquid prepared in step (2) is applied to a porous alumina ceramic membrane support with an average pore size of 5 nm, and the temperature is raised to 100°C at a rate of 2°C / min at a humidity of 40%, and the mixture is kept warm and dried for 3 hours. The temperature is then raised to 500°C at a rate of 2°C / min, and the mixture is kept warm and calcined for 3 hours. The mixture is cooled to obtain a comparative ceramic nanofiltration membrane.
[0062] Under the test conditions of room temperature and 0.69 MPa, the comparative ceramic nanofiltration membrane has a rejection rate of 15% and a flux of 82 LHM for a 0.1% PEG1000 solution.
[0063] The effects of the nanofiltration membranes obtained in the above comparative example and the embodiment are compared as shown in the following table:
[0064] Case Preparation method Film Average pore size of membrane Drying humidity Comparative Example 1 Sol-Gel Method Easy to crack 5-7nm More than 65% Comparative Example 2 Sol-hydrothermal method Complete film 20-40nm 20%-100% Comparative Example 3 Microwave hydrothermal method Complete film 40-50nm 20%-100% Example 1 Sol-microwave hydrothermal method Complete film 5-6nm 20%-100% Example 2 Sol-microwave hydrothermal method Complete film 6-7nm 20%-100% Example 3 Sol-microwave hydrothermal method Complete film 8-9nm 20%-100%
[0065] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.
Claims
1. A method for preparing a titanium oxide ceramic nanofiltration membrane, characterized in that: The steps include: (1) mixing an organic titanium salt, diethanolamine and water in a molar ratio of 1:1:10-100, stirring at room temperature for 10-30 minutes, and then performing solid-liquid separation, adding water to the obtained solid and stirring it evenly, adding nitric acid, adjusting the pH to 1-2, continuing to stir for 30 minutes, and then heating and stirring at 75-85° C. for 2-4 hours to obtain a transparent titanium oxide sol; (2) adding a dispersant to the titanium oxide sol obtained in step (1), stirring the mixture evenly, placing the mixture in a microwave hydrothermal reaction system, wherein the filling degree of the hydrothermal reactor is 50-80%, and reacting the mixture under a pressure of 0.5-2 MPa for 1-3 h, cooling the mixture, and obtaining a titanium oxide nano-solution with uniform particles; (3) adding polyethylene glycol with a weight average molecular weight of 350-450 and a cellulose compound with a molecular weight of 6000-10000 to the titanium oxide nano-solution obtained in step (2), and then adding an organosilicon defoamer BYK028, mixing well, and obtaining a coating solution; (4) Apply the coating liquid obtained in step (3) on the porous alumina ceramic membrane support, heat to 80-120°C at a humidity of 30-40%, keep warm and dry for 2-5 hours, then heat to 350-600°C and calcine for 2-5 hours, and cool to obtain the titanium oxide ceramic nanofiltration membrane.
2. The preparation method according to claim 1, characterized in that: The organic titanium salt is n-butyl titanate or isopropyl titanate.
3. The preparation method according to claim 2, characterized in that: The organic titanium salt is n-butyl titanate.
4. The preparation method according to claim 1, characterized in that: The dispersant is PEG400 or glycerol.
5. The preparation method according to claim 4, characterized in that: The dispersant is glycerol.
6. The preparation method according to claim 1, characterized in that: The cellulose compound is hydroxymethyl cellulose, hydroxyethyl cellulose or hydroxypropyl cellulose.
7. The preparation method according to claim 6, characterized in that: The cellulose compound is hydroxymethyl cellulose.
8. The preparation method according to claim 1, characterized in that: The organic titanium salt is n-butyl titanate, the dispersant is glycerol, and the cellulose compound is hydroxymethyl cellulose.
9. The preparation method according to any one of claims 1 to 8, characterized in that: In the step (2), the dispersant is added to a final concentration of 1-3 wt %; in the step (2), the second dispersant is added to a final concentration of 1 wt %; in the step (3), the polyethylene glycol and the cellulose compound are added to final concentrations of 3-10 wt % and 0.1-1 wt %, respectively, and the organosilicon defoamer is added to a final concentration of 0.01-0.1 wt %.
10. The preparation method according to claim 1, characterized in that: The step (4) is as follows: applying the coating liquid obtained in the step (3) onto the porous alumina ceramic membrane support, heating the mixture to 80-120°C at a rate of 1-3°C / min at a humidity of 30-40%, and drying the mixture for 2-5 hours; then heating the mixture to 350-600°C at a rate of 1-5°C / min, calcining the mixture for 2-5 hours, and cooling the mixture to obtain the titanium oxide ceramic nanofiltration membrane.