Preparation method and application of lanthanum-zirconium composite metal oxide loaded nickel catalyst

Through the preparation of lanthanum-zirconium composite metal oxide-supported nickel catalyst, the high cost and selectivity problems of precious metal catalysts are solved, and efficient hydrogenation conversion of lignite ethanol-soluble substances is achieved. The catalyst has high activity and selectivity and can effectively convert phenols. It is a cycloalkane alcohol, which increases the added value of the derivative organic matter.

CN118988332APending Publication Date: 2024-11-22YULIN UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410901473.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, precious metal catalysts are expensive, have poor carbon deposit resistance, long synthesis cycle of molecular sieve and harsh process conditions, making it difficult to efficiently depolymerize the phenols in lignites are cycloalkanes, and the catalyst selectivity is not high.

Method used

The preparation method of lanthanum zirconium composite metal oxide supported nickel catalyst was adopted to obtain lanthanum zirconium composite metal oxide by co-precipitation-hydrothermal synthesis method, and a supported nickel catalyst was prepared by using the modified deposition-precipitation method to achieve high dispersion and high nickel. active.

Benefits of technology

The catalyst has a simple process, short production cycle, high activity and selectivity, can efficiently cleave C-X bridge bonds, obtain high yields of methylcyclohexane and cyclohexanol in catalytic hydrogenation reaction, and convert phenols almost completely It is a cycloalkanool, which significantly increases the added value of the derivative organic matter.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a preparation method and application of a lanthanum-zirconium composite metal oxide loaded nickel catalyst, and belongs to the technical field of alkaline metal catalysts.The preparation method comprises the steps that a lanthanum source, a zirconium source and dilute ammonia water are dispersed in deionized water, and a lanthanum-zirconium composite metal oxide is obtained through a coprecipitation-hydrothermal synthesis method; and preparing the lanthanum-zirconium composite metal oxide loaded nickel catalyst by using a modified deposition-precipitation method. The preparation process is simple, the production period is short, the catalytic cracking activity is high, and the selectivity is good; when the catalyst prepared by the method is applied to the catalytic hydrogenation reaction of benzyl phenyl ether, gt can be effectively cracked; the Cal-O bridge bond is hydrogenated into an aromatic ring, so that methylcyclohexane and cyclohexanol with relatively high yield are obtained; when the catalyst is applied to catalytic conversion of p-methylphenol, high-efficiency hydrogenation of aromatic rings can be realized to obtain p-methylcyclohexanol with extremely high yield; the catalyst is applied to catalytic hydrogenation reaction of lignite alcoholysis soluble substances, aromatic ring hydrogenation and nitrogen-containing and sulfur-containing heteroatom removal can be efficiently achieved, and almost all phenols are converted into naphthenic alcohol.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of alkaline metal catalyst preparation, and in particular to a preparation method and application of a lanthanum-zirconium composite metal oxide-supported nickel catalyst. Background Art

[0002] Lignite, due to its high original moisture and ash content, has a low utilization rate when used as a heating and power generation fuel, as well as a raw material for coal chemical industry. Since lignite is less metamorphic and still retains some macromolecular groups from coal-forming plants, the oxygen content in the organic matter is relatively high, including oxygen-containing functional groups such as >COO-, >CO-, >C=O, and -OH. Therefore, the effective depolymerization of the macromolecular structure of lignite organic matter can produce a rich variety of derivative organic compounds (most of which contain aromatic rings). Many compounds containing aromatic rings (especially condensed aromatic rings) and heteroatoms are high-value-added fine organic chemicals that can be used in multiple directions or fields such as medicine, pesticides, dyes, and functional materials.

[0003] The organic compounds derived from lignite depolymerization are often hydrogenated through precious metal-loaded molecular sieves, such as Ru / HZSM-5 and Pd / Hβ. Precious metals can efficiently activate H2 to form H···H, which is more inclined to hydrogenate aromatic rings, while solid acid molecular sieves release H + , inducing the cleavage of the CO-bond and removing heteroatoms (especially O). However, precious metals are expensive, have poor resistance to carbon deposition, and are easily poisoned and deactivated. Molecular sieve synthesis processes are long and require demanding process conditions, significantly increasing catalyst manufacturing costs. Furthermore, the phenols present in a high concentration of lignite-derived organic compounds are indiscriminately converted to cycloalkanes. If a highly active and selective catalyst could be developed to convert phenols to cycloalkanols, the added value of these derived organic compounds would be significantly increased.

[0004] Non-noble metals such as Ni can also activate H2 to form H···H. Transition metal alkaline oxides are not only cheap and easy to obtain, with a short synthesis cycle, but can also effectively activate H2 to release H - , selectively cleaving the CO-bridge in oxygen-containing compounds and exhibiting good tolerance to heteroatoms. This overcomes the carbon deposition, sintering, and S / N sensitivity often seen with existing catalysts at relatively high temperatures. Summary of the Invention

[0005] To solve the above problems, the present invention provides a preparation method and application of a lanthanum-zirconium composite metal oxide-loaded nickel catalyst, wherein a lanthanum source, a zirconium source and dilute ammonia water are dispersed in deionized water, and a lanthanum-zirconium composite metal oxide is obtained by a coprecipitation-hydrothermal synthesis method, and then a lanthanum-zirconium composite metal oxide-loaded nickel catalyst is obtained by a modified deposition-precipitation method.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for preparing a lanthanum-zirconium composite metal oxide-supported nickel catalyst comprises the following steps:

[0008] a. Preparation of lanthanum-zirconium composite metal oxide

[0009] a1. Dissolve the lanthanum source and zirconium source in deionized water, add dilute ammonia dropwise and stir evenly, centrifuge, and wash alternately with deionized water and anhydrous ethanol several times to obtain a white solid;

[0010] a2. Disperse the white solid obtained in step a1 in a potassium hydroxide solution, stir evenly, and then transfer to a polytetrafluoroethylene-lined hydrothermal autoclave, heat to a certain temperature and keep warm. After naturally cooling to room temperature, centrifuge the product, and then wash it alternately with deionized water and acetic acid several times. After vacuum drying, a lanthanum-zirconium composite metal oxide can be obtained;

[0011] b. Preparation of lanthanum-zirconium composite metal oxide supported nickel catalyst

[0012] b1. Disperse the lanthanum-zirconium composite metal oxide and nickel salt obtained in step a2 into deionized water, heat in a water bath to a certain temperature under continuous stirring and keep warm, add dilute ammonia water dropwise while continuing to stir, centrifuge, wash with deionized water several times, and vacuum dry to obtain a solid powder;

[0013] b2. Place the solid powder obtained in step b1 in a tube furnace and perform high-temperature reduction under a H2 atmosphere to obtain a lanthanum-zirconium composite metal oxide-supported nickel catalyst.

[0014] Furthermore, in step a1, the lanthanum source is selected from at least one of lanthanum nitrate, lanthanum sulfate or lanthanum chloride, and the zirconium source is selected from at least one of zirconium nitrate, zirconium sulfate, zirconium chloride or zirconium hydroxide;

[0015] The mass ratio of the lanthanum source, the mass of the zirconium source, the volume of deionized water, and the volume of ammonia water is mmol:mmol:mL:mL=(10-40):(40-10):50:(10-50);

[0016] The centrifugal speed is 4000-6000 rpm and the centrifugal time is 10-30 min.

[0017] Furthermore, in step a2, the molar concentration of the potassium hydroxide solution is 2-8 mol / L, and the solid-liquid ratio of the white solid to the potassium hydroxide solution is g:mL=1:(10-50);

[0018] The hydrothermal reaction temperature is 150-250°C and the holding time is 12-24h;

[0019] The centrifugal speed is 4000-6000 rpm and the centrifugal time is 10-30 min.

[0020] Furthermore, in step b1, the nickel source is selected from at least one of nickel nitrate, nickel sulfate or nickel chloride;

[0021] The mass of the lanthanum-zirconium composite metal oxide, the mass of the nickel salt, the volume ratio of deionized water and ammonia water is g:mmol:mL:mL=1:(0.15-3.5):(30-60):(30-100);

[0022] The water bath heating temperature is 40-80℃ and the holding time is 0.5-3h;

[0023] The centrifugal speed is 4000-6000 rpm and the centrifugal time is 10-30 min;

[0024] The vacuum drying temperature is 60-90°C, and the vacuum drying time is 4-24h.

[0025] Furthermore, in step a1 and step b1, the concentration of the dilute ammonia solution is 2-10 wt%;

[0026] Furthermore, in step b2, the high-temperature reduction temperature is 400-600° C., and the high-temperature reduction time is 2-6 hours.

[0027] Furthermore, in step b2, the theoretical loading amount of metallic nickel in the prepared lanthanum-zirconium composite metal oxide-supported nickel catalyst is 1-20 wt%.

[0028] The invention also discloses a lanthanum-zirconium composite metal oxide loaded nickel catalyst prepared by the preparation method.

[0029] In addition, the invention also discloses the application of the lanthanum-zirconium composite metal oxide-supported nickel catalyst in the catalytic hydrogenation reaction of soluble matter from lignite ethanolysis.

[0030] The present invention has the following advantages: first, a lanthanum-zirconium composite metal oxide is obtained by a coprecipitation-hydrothermal synthesis method, and then a lanthanum-zirconium composite metal oxide-supported nickel catalyst is prepared by a modified deposition-precipitation method. Compared with the existing technology, the lanthanum-zirconium composite metal oxide-supported nickel catalyst prepared by this method has the following advantages:

[0031] (1) The preparation process of lanthanum-zirconium composite metal oxide supported nickel catalyst is simple, the production cycle is short and the safety is high;

[0032] (2) The nickel species in the lanthanum-zirconium composite metal oxide-supported nickel catalyst are highly dispersed and have no obvious agglomeration.

[0033] (3) The lanthanum-zirconium composite metal oxide-loaded nickel catalyst has a large specific surface area, strong alkalinity, high activity and selectivity, and is more conducive to the cracking of >CX bridge bonds (X mainly refers to N, S and O).

[0034] (4) The catalyst was used in the catalytic hydrogenation reaction of benzyl phenyl ether to obtain methylcyclohexane and cyclohexanol in higher yields.

[0035] (5) The catalyst was applied to the catalytic conversion of p-methylphenol, which could efficiently hydrogenate the aromatic ring and obtain p-methylcyclohexanol in a very high yield.

[0036] (6) The catalyst was applied to the catalytic hydrogenation reaction of lignite ethanolysis solubles, which could efficiently achieve aromatic ring hydrogenation saturation and removal of N- and S-containing heteroatoms, while phenols were almost completely converted into cycloalkanols. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 Ni prepared in Example 1 10% / X-ray diffraction pattern of LaZr;

[0038] Figure 2 Ni prepared in Example 1 10% Scanning electron microscopy (SEM), transmission electron microscopy (TEM) and element distribution maps of the / LaZr catalyst;

[0039] Figure 3 Ni prepared in Example 1 10% X-ray photoelectron spectroscopy of / LaZr catalyst;

[0040] Figure 4 Ni prepared in Example 1 10% / CO2-TPD diagram of LaZr catalyst;

[0041] Figure 5 Ni prepared in Example 1 10% Group composition distribution of the LaZr / LaZr catalyst before and after catalytic hydrogenation of soluble matter from ethanolysis of lignite in Dongming Town, Inner Mongolia. DETAILED DESCRIPTION

[0042] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention without making any creative efforts shall fall within the scope of protection of the present invention.

[0043] Example 1

[0044] A method for preparing a lanthanum-zirconium composite metal oxide-supported nickel catalyst, the specific process is as follows:

[0045] 1. Add 10 mmol of lanthanum nitrate and 10 mmol of zirconium hydroxide to 50 mL of deionized water, stir until clear, add 30 mL of 5 wt% dilute ammonia water dropwise and stir for 1 hour, then centrifuge at a speed of 5000 rpm for 5 minutes, and finally wash alternately with deionized water and anhydrous ethanol to obtain a white solid.

[0046] 2. The white solid obtained in step 1 was dispersed in 150 mL of 3 mol / L potassium hydroxide solution, stirred evenly, and then transferred to a polytetrafluoroethylene-lined hydrothermal autoclave, heated to 180° C. and kept warm for 24 h. After naturally cooling to room temperature, the product was centrifuged at a speed of 5000 rpm for 5 min. Finally, it was washed alternately with deionized water and 10% acetic acid several times and vacuum dried at 80° C. for 12 h to obtain a lanthanum-zirconium composite metal oxide.

[0047] 3. Disperse 2 g of the lanthanum-zirconium composite metal oxide obtained in step 2 and 1.01 g of nickel nitrate hexahydrate into 100 mL of deionized water, heat the mixture to 60 ° C. in a water bath and keep warm for 1 h, add 100 mL of 3 wt% dilute ammonia water dropwise (within 30 min) under continuous stirring, and continue heating and stirring in a water bath for 1 h; then centrifuge at a speed of 5000 rpm for 5 min, and finally wash the mixture with deionized water several times and vacuum dry it at 80 ° C. for 4 h to obtain a solid powder.

[0048] 4. The solid powder obtained in step 3 was placed in a tube furnace, H2 was introduced and purged at a flow rate of H2 of 40 mL / min for 30 min, and then heated to 420°C at a heating rate of 3°C / min and kept warm for 4 h. After cooling naturally to room temperature, a lanthanum-zirconium composite metal oxide catalyst with a theoretical nickel loading of 10 wt% (denoted as Ni 10% / LaZr).

[0049] Ni prepared in Example 1 10% The X-ray diffraction pattern of the / LaZr catalyst is shown in the attached Figure 1 As shown in the figure, it can be seen that Ni 10% Strong characteristic diffraction peaks of ZrO2 (JCPDS No: 37-1484) and La(OH)3 (JCPDS No: 36-1481) appeared in the Zr / LaZr catalyst. Weaker diffraction peaks of La2O2CO3 (JCPDS No: 37-0804) were also observed. Furthermore, diffraction peaks at 44.5° (111), 52° (200), and 76° (220) were attributed to elemental Ni (JCPDS No: 04-0850).

[0050] Ni prepared in Example 110% The scanning electron microscope images, transmission electron microscope images and element distribution diagrams of the / LaZr catalyst are shown in the attached Figure 2 As shown, Ni 10% / LaZr is in the shape of a strip. From the element surface distribution diagram, it can be observed that Ni, O, La and Zr are evenly distributed. The transmission electron microscope image confirms that Ni 10% / LaZr catalysts did not show obvious agglomeration, and the nickel species on the surface were evenly distributed.

[0051] Ni prepared in Example 1 10% The X-ray photoelectron spectrum of the / LaZr catalyst is shown in the attached figure. Figure 3 As shown in the figure, five elements, namely Ni, La, Zr, O and C, were detected. The binding energy peak of Ni 2p can be observed in the range of 844-889eV, and the binding energy near 852.0eV is attributed to Ni 0 , the binding energies near 855.6 and 872.5 eV are attributed to Ni 0 Surface oxidation reaction generates NiO, and Ni 0 The binding energy peak area of ​​La 3d is significantly larger than that of NiO. In the La 3d spectrum, the binding energy near 834.8 and 838.5 eV is attributed to La 3d 5 / 2 The characteristic peaks at 852.1eV and 855.7eV are attributed to La 3d 3 / 2 , indicating that La element exists mainly in the form of hydroxide. In the spectrum of Zr 3d, the vicinity of 181.9 and 184.3 eV is attributed to Zr 3d 5 / 2 The two main peaks indicate that the Zr element exists in the form of oxide.

[0052] Ni prepared in Example 1 10% The CO2-TPD diagram of the / LaZr catalyst is shown in the attached figure. Figure 4 As shown in the figure, desorption peaks appear at 381℃, 516℃ and 632℃, respectively, while 200-750℃ is located in the medium-strong base center, which indicates that Ni 10% / LaZr has more basic sites and larger peak area in this range, showing medium-strong basicity, and the basic sites on the catalyst surface can >cleave the CO bridge bond.

[0053] Example 2

[0054] A method for preparing a lanthanum-zirconium composite metal oxide-supported nickel catalyst, the specific process is as follows:

[0055] 1. Add 20 mmol of lanthanum nitrate and zirconium hydroxide to 50 mL of deionized water, stir until clear, add 30 mL of 5 wt% dilute ammonia water dropwise and stir for 1 hour. After centrifugation, wash with deionized water and anhydrous ethanol alternately several times to obtain a white solid.

[0056] 2. The white solid obtained in step 1 was dispersed in 150 mL of 3 mol / L potassium hydroxide solution, stirred evenly, and then transferred to a polytetrafluoroethylene-lined hydrothermal autoclave, heated to 180° C. and kept warm for 24 h. After naturally cooling to room temperature, the product was centrifuged, washed alternately with deionized water and 10% acetic acid several times, and vacuum-dried at 80° C. for 12 h to obtain a lanthanum-zirconium composite metal oxide.

[0057] 3. Disperse 2 g of lanthanum-zirconium composite metal oxide and 1.01 g of nickel nitrate hexahydrate obtained in step 2 into 100 mL of deionized water, heat to 60 ° C in a water bath and keep warm for 1 hour, add 100 mL of 3 wt% dilute ammonia water dropwise (within 30 minutes) under continuous stirring and continue heating and stirring in a water bath for 1 hour; after centrifugation, multiple washing with deionized water and vacuum drying at 80 ° C for 4 hours, a solid powder can be obtained.

[0058] 4. The solid powder obtained in step 3 was placed in a tube furnace, H2 was introduced and purged at a flow rate of H2 of 40 mL / min for 30 min, and then heated to 420°C at a heating rate of 3°C / min and kept warm for 4 h. After cooling naturally to room temperature, a lanthanum-zirconium composite metal oxide-supported nickel catalyst (denoted as Ni 10% / La x Zr y , where x and y are the amount ratios of lanthanum and zirconium).

[0059] Example 3

[0060] A method for preparing a lanthanum-zirconium composite metal oxide-supported nickel catalyst, the specific process is as follows:

[0061] 1. Add 10 mmol of lanthanum nitrate and 10 mmol of zirconium hydroxide to 50 mL of deionized water and stir until clear. Add 30 mL of 5 wt% dilute ammonia dropwise and stir for 1 hour. Centrifuge and wash alternately with deionized water and anhydrous ethanol to obtain a white solid.

[0062] 2. The white solid obtained in step 1 was dispersed in 150 mL of 3 mol / L potassium hydroxide solution, stirred evenly, and then transferred to a polytetrafluoroethylene-lined hydrothermal autoclave, heated to 180° C. and kept warm for 24 h. After naturally cooling to room temperature, the product was centrifuged, washed alternately with deionized water and 10% acetic acid several times, and vacuum-dried at 80° C. for 12 h to obtain a lanthanum-zirconium composite metal oxide.

[0063] 3. Disperse 2 g of the lanthanum-zirconium composite metal oxide obtained in step 2 and a certain amount of nickel nitrate hexahydrate into 100 mL of deionized water, heat the mixture to 60° C. in a water bath and keep warm for 1 h. Add 100 mL of 3 wt% dilute ammonia water dropwise (within 30 min) under continuous stirring and continue heating and stirring in a water bath for 1 h. After centrifugation, multiple washings with deionized water, and vacuum drying at 80° C. for 4 h, a solid powder was obtained.

[0064] 4. The solid powder obtained in step 3 was placed in a tube furnace, H2 was introduced and purged at a flow rate of H2 of 40 mL / min for 30 min, and then heated to 420°C at a heating rate of 3°C / min and kept warm for 4 h. After cooling naturally to room temperature, a lanthanum-zirconium composite metal oxide-supported nickel catalyst (denoted as Ni z / LaZr, where z is the theoretical loading of metallic nickel, ranging from 1 to 20 wt%).

[0065] Example 4

[0066] A method for preparing a lanthanum-zirconium composite metal oxide-supported nickel catalyst, the specific process is as follows:

[0067] 1. Add 10 mmol of lanthanum nitrate and 10 mmol of zirconium hydroxide to 50 mL of deionized water, stir until clear, add 30 mL of 5 wt% dilute ammonia water dropwise and stir for 1 hour, centrifuge, and wash alternately with deionized water and anhydrous ethanol several times to obtain a white solid;

[0068] 2. The white solid obtained in step 1 was dispersed in 150 mL of 3 mol / L potassium hydroxide solution, stirred evenly, and then transferred to a polytetrafluoroethylene-lined hydrothermal autoclave, heated to 200° C. and kept warm for 12 h. After naturally cooling to room temperature, the product was centrifuged, washed alternately with deionized water and 10% acetic acid several times, and vacuum-dried at 80° C. for 12 h to obtain a lanthanum-zirconium composite metal oxide.

[0069] 3. Disperse 2 g of the lanthanum-zirconium composite metal oxide and 1.01 g of nickel nitrate hexahydrate obtained in step 2 into 100 mL of deionized water, heat the mixture to 60° C. in a water bath and keep warm for 1 h. Add 100 mL of 3 wt% dilute ammonia water dropwise (within 30 min) under continuous stirring and continue heating and stirring in a water bath for 1 h. After centrifugation, washing with deionized water several times, and vacuum drying at 80° C. for 4 h, a solid powder was obtained.

[0070] 4. The solid powder obtained in step 3 was placed in a tube furnace, H2 was introduced and purged at a H2 flow rate of 40 mL / min for 30 min, then heated to 500°C at a heating rate of 3°C / min and kept warm for 2 h. After naturally cooling to room temperature, a lanthanum-zirconium composite metal oxide-loaded nickel catalyst with a theoretical loading of 10 wt% was obtained.

[0071] The lanthanum-zirconium composite metal oxide-supported nickel catalyst prepared in Example 1 was used in a catalytic hydrogenation reaction of lignite ethanolysis solubles. This can be explained by comparing the soluble composition before and after catalytic hydrogenation. The lignite used was lignite from Dongming Town, Inner Mongolia. Furthermore, the lanthanum-zirconium composite metal oxide-supported nickel catalyst prepared in Example 1 was also used for model compounds related to lignite ethanolysis solubles.

[0072] The following are two examples of the application of lanthanum-zirconium composite metal oxide supported nickel catalyst.

[0073] Application Example 1

[0074] The Ni prepared in Example 3 z / LaZr catalysts are used for the catalytic hydrogenation of model compounds (benzyl phenyl ether or p-methylphenol) related to lignite ethanolysis solubles. The specific application process is as follows:

[0075] (1) 1g Ni z / LaZr catalyst, 2 g benzyl phenyl ether or p-methylphenol and 20 mL n-hexane were placed in a 100 mL stainless steel autoclave;

[0076] (2) After purging the autoclave with N2 three times, pressurize it with H2 at room temperature;

[0077] (3) Subsequently, the autoclave is heated to a certain temperature and maintained for a period of time;

[0078] (4) After cooling to room temperature, the reaction mixture is taken out and the filtrate is tested and analyzed.

[0079] At a reaction temperature of 200 °C, an initial hydrogen pressure (IHP) of 5 MPa, and a reaction time of 2 h, Ni z / The analysis results of the catalytic hydrogenation performance of LaZr catalyst for benzyl phenyl ether are shown in Table 1.

[0080] Table 1

[0081]

[0082] Among them, the prepared Ni 10% The results of catalytic hydrogenation of benzyl phenyl ether by / LaZr under different reaction conditions are shown in Table 2.

[0083] Table 2

[0084]

[0085] In addition, the Ni 10% The results of catalytic hydrogenation of p-methylphenol by / LaZr under different reaction conditions are shown in Table 3.

[0086] Table 3

[0087]

[0088]

[0089] As shown in Table 1, as the Ni loading gradually increased to 10 wt%, the conversion of benzyl phenyl ether also increased to 100%, and the main products were methylcyclohexane and cyclohexanol. Further increasing the Ni loading, although the conversion of benzyl phenyl ether remained 100%, the yield of toluene began to increase. This suggests that excess Ni may cover the active sites of the catalyst, thereby inhibiting the hydrogenation of the aromatic ring.

[0090] It can be seen from Table 2 and Table 3 that the Ni 10% The main products of benzyl phenyl ether catalytic hydrogenation cracking by Ni / LaZr are methylcyclohexane and cyclohexanol, and the main hydrogenation product of p-methylphenol is p-methylcyclohexanol. 10% The active hydrogen species formed by H2 activation on the LaZr catalyst plays a crucial role in the hydrogenation of aromatic rings and the selectivity of cycloalkanols. First, the metal active sites can convert H2 into H…H and promote H…H transfer to hydrogenate the aromatic ring, while the basic active sites can catalyze the heterolytic cleavage of bound H + The release of H - , H…H and H - The coordinated transfer promotes the conversion of benzyl phenyl ether and its intermediates to methylcyclohexane and cyclohexanol, and p-methylphenol is converted into p-methylcyclohexanol. 10% / LaZr catalyst has the characteristics of high aromatic ring hydrogenation activity and high cyclohexanol selectivity.

[0091] Application Example 2

[0092] The Ni prepared in Example 1 10% / LaZr catalyst is used in the catalytic hydrogenation reaction of soluble matter from lignite ethanolysis in Dongming Town, Inner Mongolia. The specific application process is as follows:

[0093] (1) 2 g of lignite from Dongming Town, Inner Mongolia and 20 mL of ethanol were added to a 100 mL magnetically coupled mechanically stirred reactor.

[0094] (2) After replacing the air in the reactor with N2 three times and filling it with an initial nitrogen pressure of 1 MPa, set the stirring speed of the reactor to 300 rpm, increase the temperature to 300 °C at 5 °C / min and keep it warm for 2 h.

[0095] (3) After cooling naturally to room temperature, the reaction mixture is quickly transferred to a Soxhlet extraction apparatus, and the reaction mixture is thoroughly extracted with ethanol to obtain an ethanol soluble product.

[0096] (4) 0.5g Ni 10% / LaZr catalyst and 0.5 g of ethanolysis solubles were placed in a 100 mL high-pressure reactor, and 20 mL of n-hexane was added.

[0097] (5) After replacing the air in the reactor with N2, H2 was filled in with an IHP of 5 MPa. The reactor was heated to 200°C and maintained for 16 h.

[0098] (6) After cooling to room temperature, the mixture was filtered using a 0.22 μm organic filter to obtain catalytic hydrogenation ethanolysis soluble material (CHESP).

[0099] The obtained ethanolysis soluble matter (ESP) and ethanolysis soluble matter after catalytic hydrogenation (CHESP) were detected, analyzed and compared. Figure 5 shown.

[0100] From the attached Figure 5 As can be seen, the main species in ESP include paraffins (8.8%), oxygenates (56.3%, including phenols 25.2% and esters and ketones 31.1%), nitrogen-containing compounds (4.6%), and aromatics (24.9%). The main species in CHESP are paraffins (12.2%), cycloalkanes (50.4%), and oxygenates (29.3%, including cycloalkanols 23.9% and esters and ketones 5.4%). This indicates that the aromatics have been completely converted to cycloalkanes, significantly increasing their relative content. Phenols are selectively hydrogenated into cycloalkanols, while esters and ketones remain unconverted at 5.4%. No nitrogen-containing compounds were detected.

[0101] The present invention first adopts the coprecipitation-hydrothermal synthesis method to obtain lanthanum zirconium composite metal oxide, and then uses the modified deposition-precipitation method to prepare lanthanum zirconium composite metal oxide supported nickel catalyst. This supported catalyst solves the problems of expensive precious metals, poor carbon deposition resistance and easy poisoning and deactivation, long molecular sieve synthesis cycle, harsh process conditions and low cycloalkanol selectivity. Experiments have shown that the highly active Ni 10% The / LaZr catalyst achieved the effect of catalytic hydrogenation of related model compounds of lignite ethanolysis solubles and lignite ethanolysis solubles from Dongming Town, Inner Mongolia to obtain high-content cycloalkanes and cycloalkanols.

[0102] The present invention has a simple preparation process, a short production cycle, good stability, and is safe and feasible. The catalyst obtained by the present invention has high activity and selectivity and can effectively activate H2 to H···H and H - , which can efficiently obtain cycloalkanes and cycloalkanols from the ethanol soluble matter of lignite by catalytic hydrogenation, and has broad market application prospects.

[0103] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the scope of protection of the present invention.

Claims

1. A method for preparing a lanthanum-zirconium composite metal oxide-supported nickel catalyst, It is characterized in that The specific steps include: a. Preparation of lanthanum-zirconium composite metal oxide a1. Dissolve the lanthanum source and zirconium source in deionized water, add dilute ammonia water dropwise and stir evenly, centrifuge, and wash with deionized water and anhydrous ethanol alternately for multiple times to obtain a white solid; a2. Disperse the white solid obtained in step a1 in a potassium hydroxide solution, transfer it to a polytetrafluoroethylene-lined hydrothermal kettle after stirring evenly, heat it to a certain temperature and keep it warm, and after naturally cooling to room temperature, centrifuge the product, and then wash it alternately with deionized water and acetic acid for several times, and vacuum dry it to obtain a lanthanum-zirconium composite metal oxide; b. Preparation of lanthanum-zirconium composite metal oxide supported nickel catalyst b1. Disperse the lanthanum zirconium composite metal oxide and nickel salt obtained in step a2 into deionized water, heat in a water bath to a certain temperature and keep warm under continuous stirring, add dilute ammonia water dropwise and continue stirring, centrifuge, wash with deionized water for multiple times, and vacuum dry to obtain a solid powder; b2. Place the solid powder obtained in step b1 in a tube furnace at H 2 High temperature reduction is carried out under atmosphere to obtain a lanthanum-zirconium composite metal oxide-supported nickel catalyst.

2. The method for preparing the lanthanum-zirconium composite metal oxide supported nickel catalyst according to claim 1, It is characterized in that In step a1, the lanthanum source is selected from at least one of lanthanum nitrate, lanthanum sulfate or lanthanum chloride, and the zirconium source is selected from at least one of zirconium nitrate, zirconium sulfate, zirconium chloride or zirconium hydroxide; The mass ratio of the lanthanum source, the mass ratio of the zirconium source, the volume of deionized water and the volume of ammonia water is mmol:mmol:mL:mL=(10-40):(40-10):50:(10-50); The centrifugal speed is 4000-6000rpm and the centrifugal time is 10-30min.

3. The method for preparing the lanthanum-zirconium composite metal oxide supported nickel catalyst according to claim 2, It is characterized in that In step a2, the molar concentration of the potassium hydroxide solution is 2-8 mol / L, and the solid-liquid ratio of the white solid to the potassium hydroxide solution is g:mL=1:(10-50); The hydrothermal reaction temperature is 150-250°C and the insulation time is 12-24h; The centrifugal speed is 4000-6000rpm and the centrifugal time is 10-30min.

4. The method for preparing the lanthanum-zirconium composite metal oxide supported nickel catalyst according to claim 3, It is characterized in that In step b1, the nickel source is at least one of nickel nitrate, nickel sulfate or nickel chloride; The mass of lanthanum zirconium composite metal oxide, the mass of nickel salt, the volume ratio of deionized water and ammonia water is g:mmol:mL:mL=1:(0.15-3.5):(30-60):(30-100); The water bath heating temperature is 40-80℃, and the insulation time is 0.5-3h; The centrifugal speed is 4000-6000rpm, and the centrifugal time is 10-30min; The vacuum drying temperature is 60-90°C, and the vacuum drying time is 4-24h.

5. The method for preparing the lanthanum-zirconium composite metal oxide supported nickel catalyst according to claim 4, It is characterized in that In step a1 and step b1, the concentration of the dilute ammonia water is 2-10 wt %.

6. The method for preparing the lanthanum-zirconium composite metal oxide supported nickel catalyst according to claim 5, It is characterized in that In step b2, the high temperature reduction temperature is 400-600°C, and the high temperature reduction time is 2-6h.

7. The method for preparing the lanthanum-zirconium composite metal oxide supported nickel catalyst according to claim 6, It is characterized in that In step b2, the theoretical loading amount of metal nickel in the prepared lanthanum-zirconium composite metal oxide-supported nickel catalyst is 1-20 wt%.

8. A lanthanum-zirconium composite metal oxide supported nickel catalyst prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the lanthanum-zirconium composite metal oxide supported nickel catalyst as claimed in claim 8 in the catalytic hydrogenation reaction of soluble matter from lignite ethanolysis.