Preparation method of high-strength chain wheel based on powder metallurgy

Through powder metallurgy technology and high-frequency quenching technology, the problems of heat transfer and stress distribution control in sprocket preparation are solved, and the preparation of high-strength sprockets are realized, ensuring the hardness and wear resistance of sprockets, and improving production efficiency and Accurate coordination.

CN118989328AInactive Publication Date: 2024-11-22HAIAN YINGQIU POWDER METALLURGY CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411102486.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing sprocket preparation method, it is difficult to effectively control the heat transfer and stress distribution during quenching, resulting in defects such as orifice cracking, poor combination of hardness and toughness, short service life, and inconsistent shape and dimensional tolerances, which affects other components. The precise coordination and low production efficiency.

Method used

Powder metallurgy technology, including raw material mixing and preparation, pressing, sintering and heat treatment, through high-frequency quenching and tempering steps, copper plunger fills the orifices, controls heat transfer and stress distribution, and combines molded mass production to ensure the sprocket High strength and precise fit.

Benefits of technology

It effectively avoids orifice cracking, improves the hardness and wear resistance of the sprocket, extends the service life, ensures the precise coordination of the sprocket with other components, reduces production costs and material consumption, and improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989328A_ABST
    Figure CN118989328A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-strength chain wheel based on powder metallurgy, which relates to the technical field of powder metallurgy and comprises the following steps of: 1, mixing and preparing raw materials; 2, pressing; 3, sintering; 4, heat treatment; the heat treatment comprises the following steps: 1, wheel hole treatment; 2, high-frequency quenching; 3, cooling after quenching; and 4, tempering. The four orifices are filled with copper plungers in the high-frequency quenching process, so that heat transfer and stress distribution during quenching can be effectively controlled, defects such as orifice cracking can be avoided, the chain wheel can obtain the optimal hardness and toughness combination after quenching, and the service life of the chain wheel is prolonged. The anti-fatigue performance and the stability of the chain wheel are improved through stress relief in the quenching process, erosion of quenching media to orifices can be reduced through the copper columns, the structural integrity of the chain wheel is further protected, the hardness and the abrasion resistance of the chain wheel are remarkably improved after high-frequency quenching and reasonable heat treatment, and the service life of the chain wheel is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of powder metallurgy, and in particular to a method for preparing a high-strength sprocket based on powder metallurgy. Background Art

[0002] The sprocket is an important component of the sprocket drive system. The sprocket drive mode has the advantages of no elastic sliding and slipping, accurate average transmission ratio, reliable operation, high efficiency, large power transmission, strong overload capacity, etc. It is widely used in fields including household, industrial and agricultural machinery. Especially under working conditions requiring high speed, heavy load, low noise and large center distance, the chain drive composed of toothed chain sprocket and toothed chain shows its superior transmission performance.

[0003] The defects in the sprocket preparation in the prior art are:

[0004] 1. Patent document JP2004204353A discloses a manufacturing method and a sprocket. During the preparation process of the sprocket, the heat transfer and stress distribution during quenching cannot be effectively controlled, which easily leads to defects such as hole cracking. The hardness and toughness combination of the sprocket after quenching is not good, and the service life of the prepared sprocket is short.

[0005] 2. Patent document CN105014077B discloses a method for preparing powder metallurgy gears and sprockets. During the preparation process of the sprocket, the heat transfer and stress distribution during quenching cannot be effectively controlled, which easily leads to defects such as hole cracking. The combination of hardness and toughness obtained by the sprocket after quenching is not good, and the service life of the prepared sprocket is short.

[0006] 3. Patent document CN113523285A discloses a method for preparing a powder metallurgy high-density multi-row tooth sprocket. The sprocket prepared by this method cannot maintain a high degree of consistency in shape and position tolerances and dimensional tolerances, and cannot ensure the precise fit of the sprocket with other components during use, resulting in low production efficiency.

[0007] 4. Patent document CN106238733B discloses a method for preparing a three-boss timing sprocket for an automobile engine. The sprocket prepared by this method cannot maintain a high degree of consistency in shape and position tolerances and dimensional tolerances, and cannot ensure the precise fit of the sprocket with other components during use, resulting in low production efficiency. Summary of the invention

[0008] The object of the present invention is to provide a method for preparing a high-strength sprocket based on powder metallurgy to solve the problems raised in the above background technology.

[0009] To achieve the above object, the present invention provides the following technical solution: A method for preparing a high-strength sprocket based on powder metallurgy, comprising the following steps: 1. mixing and preparing raw materials; 2. pressing; 3. sintering; 4. heat treatment;

[0010] The heat treatment comprises the following steps: 1. wheel hole treatment; 2. high frequency quenching; 3. cooling after quenching; 4. tempering.

[0011] Preferably, the raw material mixing and preparation steps are as follows: Step 1: Raw material pretreatment: FC0208 powder, Cu and C powders are dried and sieved to remove impurities and moisture; Step 2: Raw material mixing: FC0208 powder, Cu and C powders are put into a metal powder mixer according to a proportion and mixed evenly, and mechanically mixed and stirred for 80 to 100 minutes at a speed of 200 r / min to form a metallurgical mixed powder.

[0012] Preferably, the Cu powder content is 1.5-3.9%, and the C powder content is 0.6-0.9%.

[0013] Preferably, the pressing steps are as follows: Step 1: Mold preparation: prepare the mold required for pressing the sprocket, ensure that the shape, size and surface roughness of the mold meet the design requirements, and lubricate the mold with graphite lubricant after cleaning; Step 2: Powder loading: load the mixed metallurgical powder into the pressing mold, and the powder is evenly and tightly filled in every corner of the mold to avoid voids or looseness; Step 3: Pressing: unidirectionally press the powder in the mold on a press, and the molding pressure during the pressing process is 600-800MPa. The powder is tightly combined under the pressure in the mold to form a sprocket green body with a certain density and shape; Step 4: Demolding: remove the sprocket green body from the mold after pressing is completed.

[0014] Preferably, the overall compaction density of the sprocket green body is 7.25-7.35 g / cm 3 , tooth density is 7.3~7.35g / cm 3 .

[0015] Preferably, the sintering steps are as follows: Step 1 Sintering preheating: put the pressed blank into the sintering furnace, close the furnace door and seal it, use a vacuum pump to draw out the gas inside the sintering furnace, and the vacuum time is 50s. Then, turn on the sintering furnace, gradually increase the temperature in the furnace and control it at 600℃~800℃, and the preheating time is 25~30min; Step 2 Sintering temperature control: the temperature in the sintering furnace gradually rises to 1100~1250℃, and is maintained at the sintering temperature for 2.5~3h, so that the powder particles can fully undergo metallurgical bonding to form a sprocket with certain strength and hardness; Step 3 Post-sintering cooling: after sintering, take the blank out of the sintering furnace, and use a cooling nozzle to blow cold air on the sprocket blank. In the initial stage of cooling, strong wind is used to quickly reduce the surface temperature of the blank to promote the reduction of the temperature difference between the inside and the outside. After the initial strong wind is quickly cooled, it is naturally cooled to room temperature; Step 4 Post-treatment: the sprocket after sintering and cooling is deburred and flat-ground to improve its surface finish and precision.

[0016] Preferably, the heat treatment steps are as follows: Step 1: wheel hole treatment: use copper columns to fill the four small holes of the sprocket; Step 2: high-frequency quenching: place the sprocket blank in the hollow copper tube of the inductor, and the high-frequency alternating current generates an alternating magnetic field in the inductor. The input frequency of the high-frequency alternating current is 100000Hz, and an induced current of the same frequency is generated in the sprocket. The induced current is unevenly distributed in the sprocket, so that its surface current density is high and the internal current density is small. The skin effect causes the sprocket surface to be rapidly heated to 800-1000°C, and high-frequency quenching is performed for 15-20s; Step 3: cooling after quenching: quickly place the sprocket in a water-soluble quenching coolant and cool it for 10-18s; Step 4: tempering: temper the quenched sprocket at 250-350°C for 60-80min to eliminate the internal stress generated during the quenching process.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] 1. The present invention can effectively control the heat transfer and stress distribution during quenching by filling the four orifices with copper columns during the high-frequency quenching process, which helps to avoid the occurrence of defects such as cracking of the orifices. At the same time, the sprocket can obtain the best combination of hardness and toughness after quenching. The stress elimination during the quenching process improves the fatigue resistance and stability of the sprocket. The use of copper columns can also reduce the erosion of the quenching medium on the orifices, further protecting the structural integrity of the sprocket. After high-frequency quenching and reasonable heat treatment, the hardness and wear resistance of the sprocket are significantly improved, thereby extending the service life of the sprocket.

[0019] 2. The present invention adopts powder metallurgy process to manufacture sprockets, which is inexpensive and can reduce the weight of the parts themselves. Powder metallurgy process can greatly reduce production costs through mold-based mass production, making the price of the sprocket more economical and significantly reducing the consumption of materials and energy. The high-precision characteristics of powder metallurgy process enable the produced sprockets to maintain a high degree of consistency in form and position tolerances and dimensional tolerances, and can ensure the precise fit of the sprocket with other components during use. The powder metallurgy process produces high-precision, high-quality sprockets, which reduces unnecessary processing steps in the subsequent processing process, reduces production costs and improves production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The sprocket preparation process flow chart of the present invention;

[0021] Figure 2 It is a schematic diagram of the sprocket structure of the present invention.

[0022] In the figure: 1. sprocket body; 2. sprocket tooth portion; 3. hole opening. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] In the description of the present invention, it should be noted that the terms "upper", "lower", "inner", "outer", "front end", "rear end", "two ends", "one end", "the other end" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0025] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "provided with", "connected", etc. should be understood in a broad sense. For example, "connected" can be a fixed connection or a movable connection, or a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0026] Embodiment 1, an embodiment provided by the present invention: a method for preparing a high-strength sprocket based on powder metallurgy, comprising the following steps: 1. mixing and preparing raw materials; 2. pressing; 3. sintering; 4. heat treatment;

[0027] The steps of raw material mixing and preparation are as follows: 1. Raw material pretreatment: FC0208 powder, Cu and C powders are dried and sieved to remove impurities and moisture; 2. Mixed raw materials: FC0208 powder, Cu and C powders are put into a metal powder mixer according to a proportion and uniformly mixed, the Cu powder content is 1.5-3.9%, the C powder content is 0.6%, and the mechanical mixing and stirring is carried out for 80 minutes at a speed of 200r / min to form a metallurgical mixed powder;

[0028] The pressing steps are as follows: 1. Mold preparation: prepare the mold required for pressing the sprocket, ensure that the shape, size and surface roughness of the mold meet the design requirements, clean the mold and lubricate it with graphite lubricant; 2. Powder loading: load the mixed metallurgical powder into the pressing mold, and fill the powder evenly and tightly in every corner of the mold to avoid voids or looseness; 3. Pressing: press the powder in the mold in one direction on the press. The pressing pressure during the pressing process is 600-800MPa, and the overall pressing density of the sprocket green body is 7.25-7.35g / cm 3 , tooth density is 7.3~7.35g / cm 3 , the powder is tightly combined under the pressure in the mold to form a sprocket green body with a certain density and shape; 4. Demolding: After the pressing is completed, the sprocket green body is taken out of the mold;

[0029] The sintering steps are as follows: 1. Sintering preheating: put the pressed blank into the sintering furnace, close the furnace door and seal it, use the vacuum pump to draw out the gas inside the sintering furnace, and vacuumize for 50 seconds. Then start the sintering furnace, gradually increase the temperature in the furnace and control it at 800°C, and the preheating time is 25 minutes; 2. Sintering temperature control: the temperature in the sintering furnace gradually rises to 1250°C, and is maintained at the sintering temperature for 2.5 hours to allow the powder particles to fully undergo metallurgical bonding to form a sprocket with certain strength and hardness; 3. Cooling after sintering: after sintering, take the blank out of the sintering furnace, and use the cooling nozzle to blow cold air on the sprocket blank. In the initial stage of cooling, strong wind is used to quickly reduce the surface temperature of the blank to promote the reduction of the temperature difference between the inside and the outside. After the initial strong wind quickly cools, it is naturally cooled to room temperature; 4. Post-treatment: the sprocket after sintering and cooling is deburred and flat-ground to improve its surface finish and precision;

[0030] The heat treatment steps are as follows: 1. High-frequency quenching: Place the sprocket blank in the hollow copper tube of the inductor. High-frequency alternating current generates an alternating magnetic field in the inductor. The input frequency of high-frequency alternating current is 100,000 Hz, and an induced current of the same frequency is generated in the sprocket. The induced current is unevenly distributed in the sprocket, so that its surface current density is high and the internal current density is small. The skin effect causes the sprocket surface to be rapidly heated to 800-1000°C, and high-frequency quenching is performed for 20 seconds; 2. Cooling after quenching: The sprocket is quickly placed in a water-soluble quenching coolant at room temperature and cooled for 10 seconds; 3. Tempering: The quenched sprocket is tempered at 250-350°C for 60 minutes to eliminate the internal stress generated during the quenching process.

[0031] Embodiment 2, an embodiment provided by the present invention: a method for preparing a high-strength sprocket based on powder metallurgy, comprising the following steps: 1. mixing and preparing raw materials; 2. pressing; 3. sintering; 4. heat treatment;

[0032] The steps of raw material mixing and preparation are as follows: 1. Raw material pretreatment: FC0208 powder, Cu and C powders are dried and sieved to remove impurities and moisture; 2. Mixing raw materials: FC0208 powder, Cu and C powders are put into a metal powder mixer according to a proportion and uniformly mixed, the Cu powder content is 1.5-3.9%, the C powder content is 0.9%, and the mechanical mixing and stirring is carried out for 80 minutes at a speed of 200r / min to form a metallurgical mixed powder;

[0033] The pressing steps are as follows: 1. Mold preparation: prepare the mold required for pressing the sprocket, ensure that the shape, size and surface roughness of the mold meet the design requirements, clean the mold and lubricate it with graphite lubricant; 2. Powder loading: load the mixed metallurgical powder into the pressing mold, and fill the powder evenly and tightly in every corner of the mold to avoid voids or looseness; 3. Pressing: press the powder in the mold in one direction on the press. The pressing pressure during the pressing process is 600-800MPa, and the overall pressing density of the sprocket green body is 7.25-7.35g / cm 3 , tooth density is 7.3~7.35g / cm 3 , the powder is tightly combined under the pressure in the mold to form a sprocket green body with a certain density and shape; 4. Demolding: After the pressing is completed, the sprocket green body is taken out of the mold;

[0034] The sintering steps are as follows: 1. Sintering preheating: put the pressed blank into the sintering furnace, close the furnace door and seal it, use the vacuum pump to draw out the gas inside the sintering furnace, and vacuumize for 50 seconds. Then start the sintering furnace, gradually increase the temperature in the furnace and control it at 800°C, and the preheating time is 25 minutes; 2. Sintering temperature control: the temperature in the sintering furnace gradually rises to 1250°C, and is maintained at the sintering temperature for 2.5 hours to allow the powder particles to fully undergo metallurgical bonding to form a sprocket with certain strength and hardness; 3. Cooling after sintering: after sintering, take the blank out of the sintering furnace, and use the cooling nozzle to blow cold air on the sprocket blank. In the initial stage of cooling, strong wind is used to quickly reduce the surface temperature of the blank to promote the reduction of the temperature difference between the inside and the outside. After the initial strong wind quickly cools, it is naturally cooled to room temperature; 4. Post-treatment: the sprocket after sintering and cooling is deburred and flat-ground to improve its surface finish and precision;

[0035] The heat treatment steps are as follows: 1. High-frequency quenching: Place the sprocket blank in the hollow copper tube of the inductor. High-frequency alternating current generates an alternating magnetic field in the inductor. The input frequency of high-frequency alternating current is 100,000 Hz, and an induced current of the same frequency is generated in the sprocket. The induced current is unevenly distributed in the sprocket, so that its surface current density is high and the internal current density is small. The skin effect causes the sprocket surface to be rapidly heated to 800-1000°C, and high-frequency quenching is performed for 20 seconds; 2. Cooling after quenching: The sprocket is quickly placed in a water-soluble quenching coolant at room temperature and cooled for 10 seconds; 3. Tempering: The quenched sprocket is tempered at 250-350°C for 60 minutes to eliminate the internal stress generated during the quenching process.

[0036] Embodiment 3, an embodiment provided by the present invention: a method for preparing a high-strength sprocket based on powder metallurgy, comprising the following steps: 1. mixing and preparing raw materials; 2. pressing; 3. sintering; 4. heat treatment;

[0037] The steps of raw material mixing and preparation are as follows: 1. Raw material pretreatment: drying and sieving FC0208 powder, Cu and C powder to remove impurities and moisture; 2. Mixing raw materials: putting FC0208 powder, Cu and C powder into a metal powder mixer according to a proportion and mixing them evenly, with the Cu powder content being 1.5-3.9% and the C powder content being 0.6-0.9%, mechanically mixing and stirring for 80 minutes at a speed of 200r / min to form a metallurgical mixed powder;

[0038] The pressing steps are as follows: 1. Mold preparation: prepare the mold required for pressing the sprocket, ensure that the shape, size and surface roughness of the mold meet the design requirements, clean the mold and lubricate it with graphite lubricant; 2. Powder loading: load the mixed metallurgical powder into the pressing mold, and fill the powder evenly and tightly in every corner of the mold to avoid voids or looseness; 3. Pressing: press the powder in the mold in one direction on the press. The pressing pressure during the pressing process is 600-800MPa, and the overall pressing density of the sprocket green body is 7.25-7.35g / cm 3 , tooth density is 7.3~7.35g / cm 3 , the powder is tightly combined under the pressure in the mold to form a sprocket green body with a certain density and shape; 4. Demolding: After the pressing is completed, the sprocket green body is taken out of the mold;

[0039] The sintering steps are as follows: 1. Sintering preheating: put the pressed blank into the sintering furnace, close the furnace door and seal it, use the vacuum pump to draw out the gas inside the sintering furnace, and vacuumize for 50 seconds. Then start the sintering furnace, gradually increase the temperature in the furnace and control it at 800°C, and the preheating time is 25 minutes; 2. Sintering temperature control: the temperature in the sintering furnace gradually rises to 1250°C, and is maintained at the sintering temperature for 2.5 hours to allow the powder particles to fully undergo metallurgical bonding to form a sprocket with certain strength and hardness; 3. Cooling after sintering: after sintering, take the blank out of the sintering furnace, and use the cooling nozzle to blow cold air on the sprocket blank. In the initial stage of cooling, strong wind is used to quickly reduce the surface temperature of the blank to promote the reduction of the temperature difference between the inside and the outside. After the initial strong wind quickly cools, it is naturally cooled to room temperature; 4. Post-treatment: the sprocket after sintering and cooling is deburred and flat-ground to improve its surface finish and precision;

[0040] The heat treatment steps are as follows: 1. High-frequency quenching: Place the sprocket blank in the hollow copper tube of the inductor. High-frequency alternating current generates an alternating magnetic field in the inductor. The input frequency of high-frequency alternating current is 100,000 Hz, and an induced current of the same frequency is generated in the sprocket. The induced current is unevenly distributed in the sprocket, so that its surface current density is high and the internal current density is small. The skin effect causes the sprocket surface to be quickly heated to 800-1000°C, and high-frequency quenching is performed for 20 seconds; 2. Cooling after quenching: The sprocket is quickly placed in a water-soluble quenching coolant at room temperature and cooled for 18 seconds; 3. Tempering: The quenched sprocket is tempered at 250-350°C for 60 minutes to eliminate the internal stress generated during the quenching process;

[0041] Embodiment 4, an embodiment provided by the present invention: a method for preparing a high-strength sprocket based on powder metallurgy, comprising the following steps: 1. mixing and preparing raw materials; 2. pressing; 3. sintering; 4. heat treatment;

[0042] The steps of raw material mixing and preparation are as follows: 1. Raw material pretreatment: drying and sieving FC0208 powder, Cu and C powder to remove impurities and moisture; 2. Mixing raw materials: putting FC0208 powder, Cu and C powder into a metal powder mixer according to a proportion and mixing them evenly, with the Cu powder content being 1.5-3.9% and the C powder content being 0.6-0.9%, mechanically mixing and stirring for 80 minutes at a speed of 200r / min to form a metallurgical mixed powder;

[0043] The pressing steps are as follows: 1. Mold preparation: prepare the mold required for pressing the sprocket, ensure that the shape, size and surface roughness of the mold meet the design requirements, clean the mold and lubricate it with graphite lubricant; 2. Powder loading: load the mixed metallurgical powder into the pressing mold, and fill the powder evenly and tightly in every corner of the mold to avoid voids or looseness; 3. Pressing: press the powder in the mold in one direction on the press. The pressing pressure during the pressing process is 600-800MPa, and the overall pressing density of the sprocket green body is 7.25-7.35g / cm 3 , tooth density is 7.3~7.35g / cm 3 , the powder is tightly combined under the pressure in the mold to form a sprocket green body with a certain density and shape; 4. Demolding: After the pressing is completed, the sprocket green body is taken out of the mold;

[0044] The sintering steps are as follows: 1. Sintering preheating: put the pressed blank into the sintering furnace, close the furnace door and seal it, use the vacuum pump to draw out the gas inside the sintering furnace, and vacuumize for 50 seconds. Then start the sintering furnace, gradually increase the temperature in the furnace and control it at 800°C, and the preheating time is 25 minutes; 2. Sintering temperature control: the temperature in the sintering furnace gradually rises to 1250°C, and is maintained at the sintering temperature for 2.5 hours to allow the powder particles to fully undergo metallurgical bonding to form a sprocket with certain strength and hardness; 3. Cooling after sintering: after sintering, take the blank out of the sintering furnace, and use the cooling nozzle to blow cold air on the sprocket blank. In the initial stage of cooling, strong wind is used to quickly reduce the surface temperature of the blank to promote the reduction of the temperature difference between the inside and the outside. After the initial strong wind quickly cools, it is naturally cooled to room temperature; 4. Post-treatment: the sprocket after sintering and cooling is deburred and flat-ground to improve its surface finish and precision;

[0045] The heat treatment steps are as follows: 1. High-frequency quenching: Place the sprocket blank in the hollow copper tube of the inductor. High-frequency alternating current generates an alternating magnetic field in the inductor. The input frequency of high-frequency alternating current is 100,000 Hz, and an induced current of the same frequency is generated in the sprocket. The induced current is unevenly distributed in the sprocket, so that its surface current density is high and the internal current density is small. The skin effect causes the sprocket surface to be rapidly heated to 800-1000°C, and high-frequency quenching is performed for 20 seconds; 2. Cooling after quenching: After the coolant is heated to 25-30°C, the sprocket is quickly placed in the heated water-soluble quenching coolant and cooled for 18 seconds; 3. Tempering: The quenched sprocket is tempered at 250-350°C for 60 minutes to eliminate the internal stress generated during the quenching process.

[0046] Embodiment 5, an embodiment provided by the present invention: a method for preparing a high-strength sprocket based on powder metallurgy, comprising the following steps: 1. mixing and preparing raw materials; 2. pressing; 3. sintering; 4. heat treatment;

[0047] The steps of raw material mixing and preparation are as follows: 1. Raw material pretreatment: drying and sieving FC0208 powder, Cu and C powder to remove impurities and moisture; 2. Mixing raw materials: putting FC0208 powder, Cu and C powder into a metal powder mixer according to a proportion and mixing them evenly, with the Cu powder content being 1.5-3.9% and the C powder content being 0.6-0.9%, mechanically mixing and stirring for 80 minutes at a speed of 200r / min to form a metallurgical mixed powder;

[0048] The pressing steps are as follows: 1. Mold preparation: prepare the mold required for pressing the sprocket, ensure that the shape, size and surface roughness of the mold meet the design requirements, clean the mold and lubricate it with graphite lubricant; 2. Powder loading: load the mixed metallurgical powder into the pressing mold, and fill the powder evenly and tightly in every corner of the mold to avoid voids or looseness; 3. Pressing: press the powder in the mold in one direction on the press. The pressing pressure during the pressing process is 600-800MPa, and the overall pressing density of the sprocket green body is 7.25-7.35g / cm 3 , tooth density is 7.3~7.35g / cm 3 , the powder is tightly combined under the pressure in the mold to form a sprocket green body with a certain density and shape; 4. Demolding: After the pressing is completed, the sprocket green body is taken out of the mold;

[0049] The sintering steps are as follows: 1. Sintering preheating: put the pressed blank into the sintering furnace, close the furnace door and seal it, use the vacuum pump to draw out the gas inside the sintering furnace, and vacuumize for 50 seconds. Then start the sintering furnace, gradually increase the temperature in the furnace and control it at 800°C, and the preheating time is 25 minutes; 2. Sintering temperature control: the temperature in the sintering furnace gradually rises to 1250°C, and is maintained at the sintering temperature for 2.5 hours to allow the powder particles to fully undergo metallurgical bonding to form a sprocket with certain strength and hardness; 3. Cooling after sintering: after sintering, take the blank out of the sintering furnace, and use the cooling nozzle to blow cold air on the sprocket blank. In the initial stage of cooling, strong wind is used to quickly reduce the surface temperature of the blank to promote the reduction of the temperature difference between the inside and the outside. After the initial strong wind quickly cools, it is naturally cooled to room temperature; 4. Post-treatment: the sprocket after sintering and cooling is deburred and flat-ground to improve its surface finish and precision;

[0050] The heat treatment steps are as follows: 1. Wheel hole treatment: Use copper columns to fill the four small holes of the sprocket; 2. High-frequency quenching: Place the sprocket blank in the hollow copper tube of the inductor. High-frequency alternating current generates an alternating magnetic field in the inductor. The input frequency of high-frequency alternating current is 100,000 Hz, and an induced current of the same frequency is generated in the sprocket. The induced current is unevenly distributed in the sprocket, so that its surface current density is high and the internal current density is small. The skin effect causes the sprocket surface to be rapidly heated to 800-1000°C, and high-frequency quenching is performed for 20 seconds; 3. Cooling after quenching: The sprocket is quickly placed in a water-soluble quenching coolant and cooled for 10-18 seconds; 4. Tempering: The quenched sprocket is tempered at 250-350°C for 60 minutes to eliminate the internal stress generated during the quenching process.

[0051] Comparative Example 1, a method for preparing a high-strength sprocket based on powder metallurgy, comprising the following steps: 1. mixing and preparing raw materials; 2. pressing; 3. sintering; 4. heat treatment;

[0052] The steps of raw material mixing and preparation are as follows: 1. Raw material pretreatment: drying and sieving FC0208 powder, Cu and C powder to remove impurities and moisture; 2. Mixing raw materials: putting FC0208 powder, Cu and C powder into a metal powder mixer according to a proportion and mixing them evenly, with the Cu powder content being 1.5-3.9% and the C powder content being 0.6-0.9%, mechanically mixing and stirring for 80 minutes at a speed of 200r / min to form a metallurgical mixed powder;

[0053] The pressing steps are as follows: 1. Mold preparation: prepare the mold required for pressing the sprocket, ensure that the shape, size and surface roughness of the mold meet the design requirements, clean the mold and lubricate it with graphite lubricant; 2. Powder loading: load the mixed metallurgical powder into the pressing mold, and fill the powder evenly and tightly in every corner of the mold to avoid voids or looseness; 3. Pressing: press the powder in the mold in one direction on the press. The pressing pressure during the pressing process is 600-800MPa, and the overall pressing density of the sprocket green body is 7.0-7.1g / cm 3 , tooth density is 7.05~7.15g / cm 3 , the powder is tightly combined under the pressure in the mold to form a sprocket green body with a certain density and shape; 4. Demolding: After the pressing is completed, the sprocket green body is taken out of the mold;

[0054] The sintering steps are as follows: 1. Sintering preheating: put the pressed blank into the sintering furnace, close the furnace door and seal it, use the vacuum pump to draw out the gas inside the sintering furnace, and vacuumize for 50 seconds. Then start the sintering furnace, gradually increase the temperature in the furnace and control it at 800°C, and the preheating time is 25 minutes; 2. Sintering temperature control: the temperature in the sintering furnace gradually rises to 1250°C, and is maintained at the sintering temperature for 2.5 hours to allow the powder particles to fully undergo metallurgical bonding to form a sprocket with certain strength and hardness; 3. Cooling after sintering: after sintering, take the blank out of the sintering furnace, and use the cooling nozzle to blow cold air on the sprocket blank. In the initial stage of cooling, strong wind is used to quickly reduce the surface temperature of the blank to promote the reduction of the temperature difference between the inside and the outside. After the initial strong wind quickly cools, it is naturally cooled to room temperature; 4. Post-treatment: the sprocket after sintering and cooling is deburred and flat-ground to improve its surface finish and precision;

[0055] The heat treatment steps are as follows: 1. High-frequency quenching: Place the sprocket blank in the hollow copper tube of the inductor. High-frequency alternating current generates an alternating magnetic field in the inductor. The input frequency of high-frequency alternating current is 100,000 Hz, and an induced current of the same frequency is generated in the sprocket. The induced current is unevenly distributed in the sprocket, so that its surface current density is high and the internal current density is small. The skin effect causes the sprocket surface to be rapidly heated to 800-1000°C, and high-frequency quenching is performed for 20 seconds; 2. Cooling after quenching: The sprocket is quickly placed in a water-soluble quenching coolant and cooled for 10 seconds; 3. Tempering: The quenched sprocket is tempered at 250-350°C for 60 minutes to eliminate the internal stress generated during the quenching process.

[0056] Performance Test:

[0057] 1. Tooth hardness: Use Leeb hardness tester or E-type Shore hardness tester to measure the hardness of sprocket teeth. Based on the principle of dynamic hardness detection, the hardness value is calculated by measuring the rebound speed of the impact body after it hits the sample surface;

[0058] 2. Hole status detection: Observe with the naked eye whether there are obvious cracks, damage or deformation around the sprocket hole, place the ultrasonic probe near the sprocket hole and send ultrasonic signals into the material, then receive and analyze the reflected ultrasonic signals to determine whether there are cracks inside the hole and their location and size.

[0059] The test data of each embodiment under the same test conditions are shown in Table 1

[0060]

[0061] Table 1

[0062] From the experimental data in Table 1, it can be seen that the overall density of the powder is controlled at 7.25-7.35 g / cm during pressing. 3 The tooth density is 7.3~7.35gg / cm 3 The four small holes are filled with copper pillars and then high-frequency quenched. The sprocket size and hardness performance prepared by room temperature coolant cooling can meet the requirements. The copper pillars filling the holes can effectively control the heat transfer and stress distribution during quenching, which helps to avoid the occurrence of defects such as hole cracking. After high-frequency quenching and reasonable heat treatment, the hardness and wear resistance of the sprocket are significantly improved.

[0063] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing a high-strength sprocket based on powder metallurgy, characterized in that: The process includes the following steps:

1. mixing and preparing raw materials; 2. pressing; 3. sintering; 4. heat treatment; The heat treatment comprises the following steps:

1. wheel hole treatment; 2. high frequency quenching; 3. cooling after quenching; 4. tempering.

2. The method for preparing a high-strength sprocket based on powder metallurgy according to claim 1, characterized in that: The raw material mixing and preparation steps are as follows: step (1) raw material pretreatment: FC0208 powder, Cu and C powders are dried and sieved to remove impurities and moisture; step (2) raw material mixing: FC0208 powder, Cu and C powders are put into a metal powder mixer according to a proportion and uniformly mixed, and mechanically mixed and stirred for 80 to 100 minutes at a speed of 200 r / min to form a metallurgical mixed powder.

3. The method for preparing a high-strength sprocket based on powder metallurgy according to claim 2, characterized in that: The content of the Cu powder is 1.5-3.9%, and the content of the C powder is 0.6-0.9%.

4. The method for preparing a high-strength sprocket based on powder metallurgy according to claim 1, characterized in that: The pressing steps are as follows: step (1) mold preparation: prepare the mold required for pressing the sprocket, ensure that the shape, size and surface roughness of the mold meet the design requirements, and use graphite lubricant to lubricate the mold after cleaning; step (2) powder loading: load the mixed metallurgical powder into the pressing mold, and the powder is evenly and tightly filled in each corner of the mold to avoid voids or looseness; step (3) pressing: unidirectionally press the powder in the mold on a press, and the molding pressure during the pressing process is 600-800MPa. The powder is tightly combined under the action of pressure in the mold to form a sprocket green body with a certain density and shape; step (4) demolding: after the pressing is completed, the sprocket green body is taken out of the mold.

5. The method for preparing a high-strength sprocket based on powder metallurgy according to claim 4, characterized in that: The overall compaction density of the sprocket green body is 7.25-7.35 g / cm 3 , tooth density is 7.3~7.35g / cm 3 .

6. The method for preparing a high-strength sprocket based on powder metallurgy according to claim 1, characterized in that: The sintering steps are as follows: Step (1) Sintering preheating: put the pressed blank into the sintering furnace, close the furnace door and seal it, use a vacuum pump to draw out the gas inside the sintering furnace, and evacuate for 50 seconds. Then start the sintering furnace, gradually raise the temperature in the furnace to 600°C to 800°C, and preheat for 25 to 30 minutes. Step (2) Sintering temperature control: gradually raise the temperature in the sintering furnace to 1100 to 1250°C, and keep it at the sintering temperature for 2.5 to 3 hours to make the powder The particles are fully metallurgically bonded to form a sprocket with certain strength and hardness; Step (3) cooling after sintering: after sintering, the blank is taken out of the sintering furnace, and the cooling nozzle is used to blow cold air to the sprocket blank. In the initial cooling stage, strong wind is used to quickly reduce the surface temperature of the blank to promote the reduction of the temperature difference between the inside and the outside. After the initial strong wind rapid cooling, it is naturally cooled to room temperature; Step (4) post-treatment: the sprocket after sintering and cooling is deburred and flat-ground to improve its surface finish and precision.

7. The method for preparing a high-strength sprocket based on powder metallurgy according to claim 1, characterized in that: The heat treatment steps are as follows: step (1) wheel hole treatment: use copper columns to fill the four small holes of the sprocket; step (2) high-frequency quenching: place the sprocket blank in the hollow copper tube of the inductor, and high-frequency alternating current generates an alternating magnetic field in the inductor. The input frequency of the high-frequency alternating current is 100000 Hz, and an induced current of the same frequency is generated in the sprocket. The induced current is unevenly distributed in the sprocket, so that its surface current density is high and the internal current density is small. The skin effect causes the sprocket surface to be rapidly heated to 800-1000° C., and high-frequency quenching is performed for 15-20 seconds; step (3) cooling after quenching: the sprocket is quickly placed in a water-soluble quenching coolant and cooled for 10-18 seconds; step (4) tempering: the quenched sprocket is tempered at 250-350° C. for 60-80 minutes to eliminate the internal stress generated during the quenching process.

Citation Information

Patent Citations

  • Manufacturing method of powder metallurgy chain wheel

    CN102049519A

  • Chain wheel for VVT system and preparation method of chain wheel

    CN107795664A

  • Quenching-preventing device

    CN202297710U

  • High frequency hardening method

    JP1984190317A

  • Method of high-frequency induction hardening for sintered part

    JP2006291232A