Composite phase type electrode wire and manufacturing process thereof

Through the composite phase electrode wire manufacturing process, a composite phase plating structure of β-phase and γ-phase is formed, which solves the problems of thickness uniformity and discharge stability of the electrode wire galvanized layer, improves the cutting efficiency and accuracy, and meets the modern manufacturing industry's requirements. High precision and speed requirements.

CN118989482AInactive Publication Date: 2024-11-22JIANGXI KAIQIANG NEW MATERIALS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411361117.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The thickness uniformity of the galvanized layer of existing electrode wires is difficult to control, resulting in poor discharge stability, low cutting efficiency, and the single-layer structure cannot meet the high requirements of modern manufacturing industry for processing accuracy and speed.

Method used

The composite phase electrode wire manufacturing process is adopted, and the composite phase type of β-phase and γ-phase is formed through the steps of smelting, giant pulling, bell furnace annealing, big pulling, medium pulling, electroplating, bell furnace secondary annealing and small pulling. The plating structure combines the continuous electroplating of electrodeposition and stretching large deformation process to control the thickness and microstructure of the galvanized layer.

Benefits of technology

The discharge effect and cutting performance of the electrode wire are significantly improved, the discharge stability and cutting speed are improved, the cutting efficiency is increased by more than 20%, and the tensile strength is greater than 900MPa, and the conductivity is 21-24% IACS.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989482A_ABST
    Figure CN118989482A_ABST
Patent Text Reader

Abstract

The invention relates to a composite phase type electrode wire and a manufacturing process thereof, the manufacturing process comprises the following steps: smelting, huge drawing, annealing in a bell furnace, large drawing, medium drawing, electroplating, secondary annealing in the bell furnace and small drawing, and the electroplating comprises alkali electrolysis, water washing, acid electrolysis, water washing, galvanizing, drying and take-up treatment. Compared with the prior art, the method has the advantages that the characteristic of common discharging of the beta-type electrode wire and the gamma-type electrode wire is integrated, the discharging effect of the electrode wires is greatly improved, and compared with a common brass wire, the cutting efficiency is improved by 20% or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrode wire manufacturing, and in particular to a composite phase type electrode wire and a manufacturing process thereof. Background Art

[0002] In recent years, mechanical processing technology has been changing with each passing day, and wire-cut EDM as a special precision mechanical processing technology has also developed rapidly. An important part of the development of wire cutting technology depends on the development of electrode wire technology. With the continuous advancement of material processing technology and mechanical processing technology, the electrode wire has undergone a transition from ordinary brass electrode wire to coated electrode wire. The galvanized electrode wire for wire cutting is generally made of ordinary brass with a layer of zinc on the outside, but the uniformity of the thickness of the zinc coating cannot be well controlled. The discharge stability of this electrode wire is relatively poor, and it often contains 35% or more zinc brass wire. Although the cost is reduced, the cutting efficiency is relatively low. In addition, with the popularization and application of wire EDM in intelligent manufacturing, medical equipment, automobile manufacturing, precision molds, electronic communications, high-end watches and other industries, higher requirements are placed on the processing accuracy and speed of electrode wires.

[0003] However, the electrode wires currently manufactured are all single-layer structures, which can no longer meet the needs of the manufacturing market in terms of processing accuracy and speed, and research and improvement are urgently needed. Summary of the invention

[0004] The purpose of the present invention is to provide a composite phase type electrode wire and a manufacturing process thereof in order to overcome the defects of the above-mentioned prior art.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] A manufacturing process of a composite phase type electrode wire, the manufacturing process comprising the following steps:

[0007] 1) Melting: 62.7% to 63.3% of Cu, 0 to 0.01% of Fe and the balance of Zn are put into a melting furnace according to a weight ratio for melting at a melting temperature of 1025° C. to 1035° C., and a Φ12.0 mm brass billet rod is cast at a pulling speed of 1.0 to 1.1 m / min;

[0008] 2) Giant drawing: Use a giant drawing machine to draw a Φ12.0mm brass billet rod into a Φ7.8mm brass wire billet. The drawing speed of the giant drawing machine is 110-130m / min.

[0009] 3) Bell furnace annealing: Put the Φ7.8mm brass wire billet into a bell furnace for annealing at a temperature of 540-560°C, keep warm for 3 hours and then cool;

[0010] 4) Drawing: Use a drawing machine to draw the Φ7.8mm brass wire billet and anneal it online to produce a Φ3.0mm brass wire billet. The drawing speed of the drawing machine is 395-405m / min, and the annealing amount is 37±1%;

[0011] 5) Intermediate drawing: Use an intermediate drawing machine to perform intermediate drawing on a Φ3.0 mm brass wire billet and perform online annealing to produce a Φ1.0 mm brass wire billet. The drawing speed of the intermediate drawing machine is controlled at 600 m / min, and the annealing coefficient is 1.4±0.03;

[0012] 6) Electroplating: alkaline electrolysis, water washing, acid electrolysis, water washing, galvanizing, drying and wire taking-up are sequentially performed on the brass wire billet of Φ1.0mm; the alkaline electrolysis uses a degreasing solution with a concentration of 60-70g / L and a temperature of 60-70°C; the acid electrolysis uses sulfuric acid with a volume ratio of sulfuric acid to the pickling solution of 10%, and the temperature of the pickling solution is room temperature; zinc sulfate and buffer salt are used in the galvanizing process, with a zinc sulfate concentration of 470-480g / L, a buffer salt concentration of 35-45g / L, a galvanizing solution temperature of 30-40°C, a galvanizing tank voltage of 2.0-5.0V, and a current of 300-400A; the galvanizing process is repeated twice, with a drying temperature of 150-200°C and a wire taking-up speed of 80-110m / min.

[0013] 7) Secondary annealing in bell furnace: The Φ1.0mm composite phase electrode wire after galvanizing is put into the bell furnace for secondary annealing treatment. The annealing temperature is 210-240℃ and the holding time is 3.5-4.0h.

[0014] 8) Small drawing: Use a small drawing machine to stretch the Φ1.0mm composite phase electrode wire into a Φ0.2-Φ0.3mm finished composite phase electrode wire. The stretching speed of the small drawing machine is 1000±5m / min, and the annealing voltage is 35-40V.

[0015] Furthermore, in the step 1), the smelting temperature is controlled at 1030°C; and in the step 3), the annealing temperature is controlled at 550°C.

[0016] Furthermore, in the step 6), the concentration of the degreasing solution is controlled to 65 g / L, the temperature is controlled to 65° C., the concentration of zinc sulfate is controlled to 475 g / L, the concentration of the buffer salt is controlled to 40 g / L, the temperature of the galvanizing solution is controlled to 35° C., the voltage of the galvanizing tank is controlled to 3.5 V, and the current is controlled to 350 A.

[0017] Furthermore, the water washing is performed using pure water for five consecutive rinses.

[0018] A composite phase electrode wire manufactured by the manufacturing process, the electrode wire comprising a core material and a galvanized layer covering the surface of the core material; the galvanized layer is a composite phase coating structure of β phase and γ phase, and the surface is a microstructure of small holes and multiple pores; the single side thickness of the galvanized layer is 6-8um; the size of the electrode wire is Φ0.2-0.3mm.

[0019] Compared with the prior art, the present invention has the following advantages:

[0020] The present invention can better control the thickness of the zinc coating layer by controlling the uniformity of the zinc coating thickness on the surface of the electrode wire, using the electrodeposition continuous electroplating and stretching large deformation process, forming a composite phase structure combining β phase and γ phase on the surface of the electrode wire, combining the characteristics of the common discharge of β type electrode wire and γ type electrode wire, and the microscopic porous structure on the surface greatly improves the discharge effect of the electrode wire, which is conducive to improving the flushing performance, making it more stable and less likely to break the wire during the cutting discharge process compared with the brass wire; at the same time, due to the strong explosive gas pressure generated by the gasification of the zinc coating layer, the explosive gas will push the electro-corrosion product out of the discharge channel, thereby improving the washing and chip removal performance in the discharge channel, and improving the cutting speed and cutting accuracy of the electrode wire during discharge corrosion. The composite phase electrode wire of the present invention has a tensile strength greater than 900MPa, a conductivity of 21-24%IACS, and a straightness less than 30mm; compared with ordinary brass electrode wire, the cutting efficiency is improved by more than 20%. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 A manufacturing process flow chart provided by the present invention;

[0022] Figure 2 The finished product structure diagram of the composite phase type electrode wire provided by the present invention;

[0023] Figure 3 A schematic diagram of the structure of the zinc-plated layer of the composite phase type electrode wire provided by the present invention under a microscope;

[0024] Figure 4 This is a schematic diagram of the surface microstructure of the composite phase type electrode wire under a microscope provided by the present invention. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0026] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example

[0028] like Figure 1 As shown, a manufacturing process of a composite phase type electrode wire comprises the following steps:

[0029] 1) Melting: 62.7% to 63.3% of Cu, 0 to 0.01% of Fe and the balance of Zn are put into a melting furnace according to a weight ratio for melting, the melting temperature is 1025° C. to 1035° C., and a Φ12.0 mm brass billet rod is cast at a pulling speed of 1.0 to 1.1 m / min. The melting temperature is optimally controlled at 1030° C. At this time, the surface of the brass billet rod has no cold shut, scarring, and the fracture has no pores, shrinkage holes, inclusions, peeling and other casting defects, the tensile strength is 330 to 410 MPa, and the elongation is ≥35%.

[0030] 2) Giant drawing: Use a giant drawing machine to stretch a Φ12.0mm brass billet rod into a Φ7.8mm brass wire billet. The stretching speed of the giant drawing machine is 110-130m / min. At this time, the surface of the brass wire billet is smooth without obvious scratches, crystal spots, cracks and other defects.

[0031] 3) Bell furnace annealing: Put the Φ7.8mm brass wire billet into a bell furnace for annealing at 540-560°C. Keep warm for 3 hours and then cool. The optimal annealing temperature is controlled at 550°C. At this time, the tensile strength of the brass wire billet is 300-400Mpa, and the elongation is ≥40%.

[0032] 4) Drawing: Use a drawing machine to draw the Φ7.8mm brass wire billet and anneal it online to stretch it into a Φ3.0mm brass wire billet. The drawing speed of the drawing machine is 395-405m / min, and the annealing amount is 37±1%. At this time, the surface of the brass wire billet is smooth, without obvious scratches, cracks, electric shocks and other defects, the tensile strength is 410-470Mpa, and the elongation is ≥26%.

[0033] 5) Intermediate drawing: Use an intermediate drawing machine to perform intermediate drawing on the Φ3.0mm brass wire billet and anneal it online to produce a Φ1.0mm brass wire billet. The drawing speed of the intermediate drawing machine is controlled at 600m / min, and the annealing coefficient is 1.4±0.03; at this time, the surface of the brass wire billet is smooth, without obvious scratches, cracks, electric shocks and other defects, the tensile strength is 470-520Mpa, and the elongation is ≥20%.

[0034] 6) Electroplating: alkaline electrolysis, water washing, acid electrolysis, water washing, galvanizing, drying and wire winding are sequentially performed on the brass wire blank of Φ1.0mm; the alkaline electrolysis uses a degreasing solution with a concentration of 60-70g / L, preferably 65g / L, and a temperature of 60-70°C, preferably 65°C; the acid electrolysis uses sulfuric acid with a concentration volume ratio of 10% of the pickling solution, and the temperature of the pickling solution is room temperature; the galvanizing process uses zinc sulfate and buffer salt, with a zinc sulfate concentration of 470-480g / L, preferably 475g / L, a buffer salt concentration of 35-45g / L, preferably 40g / L, a galvanizing solution temperature of 30-40°C, preferably 35°C, and a galvanizing tank voltage of 2.0-5.0V, preferably The best value is 3.5V, the current is 300-400A, and the best value is 350A; the galvanizing process is repeated twice, the drying temperature is 150-200℃, and the winding speed is 80-110m / min; the water washing is to use pure water for five consecutive rinses; the surface of the electrode wire after galvanizing needs to meet the following requirements: a. No dense zinc lumps are allowed, which are visible to the naked eye and feel rough; b. No wrinkles or cracks in the coating are allowed; c. No wire flow-like scratches are allowed, and the coating is scraped off or cracked; d. The core material is not allowed to be exposed (copper leakage) due to scratches, electric shocks, indentations, etc.; e. There is no oxidation or black spots on the surface, and the color is uniform; at this time, the tensile strength of the composite phase electrode wire is 470-520Mpa, and the single-sided film thickness is 6-8um.

[0035] 7) Secondary annealing in bell furnace: The Φ1.0mm composite phase electrode wire after galvanizing is put into the bell furnace for secondary annealing treatment. The annealing temperature is 210-240℃ and the insulation time is 3.5-4.0h. At this time, there is no peeling, cracking, dezincification, powdering, copper exposure, dark oxidation, color difference and other problems.

[0036] 8) Small drawing: Use a small drawing machine to stretch the Φ1.0mm composite phase electrode wire into a finished composite phase electrode wire of Φ0.2-Φ0.3mm. The stretching speed of the small drawing machine is 1000±5m / min, and the annealing voltage is 35-40V. At this time, the surface of the composite phase electrode wire has no peeling, burrs and rough pulling marks, no serious spots, darkening and oxidation color, no obvious exposed copper points, and the tensile strength is 900-1050MPa, the conductivity is 21-24%IACS, and the straightness is ≤30mm.

[0037] like Figures 2 to 4 As shown, a composite phase electrode wire is manufactured using the manufacturing process, the electrode wire includes a core material and a galvanized layer covering the surface of the core material; the galvanized layer is a composite phase coating structure of β phase and γ phase, and the surface is a microstructure of small holes and porous; the single-side thickness of the galvanized layer is 6-8um; the size of the electrode wire is Φ0.2-0.3mm.

[0038] Four sections of the manufactured composite phase electrode wire were taken for cutting test and compared with ordinary brass wire. The experiment was carried out three times in succession. The experimental results are shown in Tables 1 to 3 below.

[0039] Table 1 Comparison of composite phase type electrode wire cutting test data - Composite phase type electrode wire cutting test data

[0040]

[0041]

[0042] Table 2 Comparison of cutting test data of composite phase electrode wire and two composite phase electrode wire cutting test data

[0043]

[0044] Table 3 Comparison of cutting test data of composite phase electrode wire and three composite phase electrode wire

[0045]

[0046] By comparing the various performance indicators in Tables 1 to 3, it can be concluded that the composite phase electrode wire of the present invention has a more stable discharge process, is less likely to break, has a faster processing speed, and has a cutting efficiency improved by more than 20% compared to ordinary brass wire, especially in Table 3, where the cutting efficiency is improved by 22.35%.

[0047] The composite phase type electrode wire of the present invention is advanced mainly in controlling the uniformity of the thickness of the zinc coating on the surface of the electrode wire. By using the electrodeposition continuous electroplating and large stretching deformation process, the thickness of the zinc coating can be better controlled, and a composite phase structure combining β phase and γ phase is formed on the surface of the electrode wire, which combines the characteristics of the common discharge of β type electrode wire and γ type electrode wire, and forms a micro porous structure that is beneficial to improving the flushing performance. Compared with the brass wire, during the cutting discharge process, although the temperature in the discharge channel is as high as 8000℃-12000℃, the temperature first acts on the zinc coating with a low melting point (the melting point of zinc is about 420℃). On the one hand, the zinc coating first absorbs most of the heat through its own gasification, thereby protecting the electrode wire matrix, making the discharge stable and not easy to break during the processing process; at the same time, due to the strong explosive gas pressure generated by the gasification of the zinc coating layer, the explosive gas will push the electro-corrosion products out of the discharge channel, thereby improving the washing and chip removal performance in the discharge channel, and improving the cutting speed and cutting accuracy of the electrode wire during discharge corrosion.

[0048] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A manufacturing process for a composite phase type electrode wire, characterized in that: The manufacturing process comprises the following steps: 1) Melting: 62.7% to 63.3% of Cu, 0 to 0.01% of Fe and the balance of Zn are put into a melting furnace according to a weight ratio for melting at a melting temperature of 1025° C. to 1035° C., and a Φ12.0 mm brass billet rod is cast at a pulling speed of 1.0 to 1.1 m / min; 2) Giant drawing: Use a giant drawing machine to draw a Φ12.0mm brass billet rod into a Φ7.8mm brass wire billet. The drawing speed of the giant drawing machine is 110-130m / min. 3) Bell furnace annealing: Put the Φ7.8mm brass wire billet into a bell furnace for annealing at a temperature of 540-560°C, keep warm for 3 hours and then cool; 4) Drawing: Use a drawing machine to draw the Φ7.8mm brass wire billet and anneal it online to produce a Φ3.0mm brass wire billet. The drawing speed of the drawing machine is 395-405m / min, and the annealing amount is 37±1%; 5) Intermediate drawing: Use an intermediate drawing machine to perform intermediate drawing on a Φ3.0 mm brass wire billet and perform online annealing to produce a Φ1.0 mm brass wire billet. The drawing speed of the intermediate drawing machine is controlled at 600 m / min, and the annealing coefficient is 1.4±0.03; 6) Electroplating: alkaline electrolysis, water washing, acid electrolysis, water washing, galvanizing, drying and wire taking-up are sequentially performed on the brass wire billet of Φ1.0mm; the alkaline electrolysis uses a degreasing solution with a concentration of 60-70g / L and a temperature of 60-70°C; the acid electrolysis uses sulfuric acid with a volume ratio of sulfuric acid to the pickling solution of 10%, and the temperature of the pickling solution is room temperature; zinc sulfate and buffer salt are used in the galvanizing process, with a zinc sulfate concentration of 470-480g / L, a buffer salt concentration of 35-45g / L, a galvanizing solution temperature of 30-40°C, a galvanizing tank voltage of 2.0-5.0V, and a current of 300-400A; the galvanizing process is repeated twice, with a drying temperature of 150-200°C and a wire taking-up speed of 80-110m / min. 7) Secondary annealing in bell furnace: The Φ1.0mm composite phase electrode wire after galvanizing is put into the bell furnace for secondary annealing treatment. The annealing temperature is 210-240℃ and the holding time is 3.5-4.0h. 8) Small drawing: Use a small drawing machine to stretch the Φ1.0mm composite phase electrode wire into a Φ0.2-Φ0.3mm finished composite phase electrode wire. The stretching speed of the small drawing machine is 1000±5m / min, and the annealing voltage is 35-40V.

2. The manufacturing process of a composite phase type electrode wire according to claim 1, characterized in that: In the step 1), the smelting temperature is controlled at 1030°C; and in the step 3), the annealing temperature is controlled at 550°C.

3. The manufacturing process of a composite phase type electrode wire according to claim 1, characterized in that: In the step 6), the concentration of the degreasing solution is controlled to 65 g / L, the temperature is controlled to 65° C., the zinc sulfate concentration is controlled to 475 g / L, the buffer salt concentration is controlled to 40 g / L, the temperature of the galvanizing solution is controlled to 35° C., the voltage of the galvanizing tank is controlled to 3.5 V, and the current is controlled to 350 A.

4. The manufacturing process of a composite phase type electrode wire according to claim 1, characterized in that: The water washing is to use pure water to perform five consecutive rinses.

5. A composite phase type electrode wire manufactured by the manufacturing process according to claim 1, characterized in that: The electrode wire comprises a core material and a galvanized layer covering the surface of the core material; the galvanized layer is a composite phase coating structure of β phase and γ phase, and the surface is a microstructure of small holes and porous; the single-side thickness of the galvanized layer is 6-8um; the size of the electrode wire is Φ0.2-0.3mm.

Citation Information

Patent Citations

  • Wire electrode for WEDM-LS electrical discharge machining and preparation method of wire electrode

    CN103537768A

  • Novel electrode wire production manner

    CN110180914A

  • High-speed plating electrode wire manufacturing process

    CN113714749A

  • Galvanized electrode wire manufacturing method

    CN113909599A

  • High-Precision Zinc-Based Alloy Electrode Wire and Manufacture Method Thereof

    US20160368070A1