Method for improving titanium / steel dissimilar metal connection through porous high-entropy alloy structure

By using laser selection melting between titanium and steel as the intermediate layer, the problems of heat uneven and internal stress during welding of titanium and steel are solved, and the high reliability of titanium/steel heterogeneous metals are achieved The joints improve welding quality and joint strength.

CN118989872AActive Publication Date: 2024-11-22SHANGHAI UNIV OF ENG SCI

Patent Information

Application Number
CN202411147956.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-22
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

During the welding process, titanium and steel are subjected to heat unevenness and internal stress due to performance differences such as melting point, thermal conductivity, expansion coefficient, etc., making it difficult to form a reliable connection, and the joints are prone to brittle intermetallic compounds, resulting in cracking.

Method used

The porous high-entropy alloy structure was prepared as the intermediate layer by laser selection melting technology, and a three-dimensional porous structure was formed between titanium and steel using FeCoCrNiMn high-entropy alloy powder, and a high-reliability connection of titanium/steel heterometal was achieved through laser wire-filled welding.

Benefits of technology

It realizes high-reliability connection of titanium/steel heterogeneous metal, solves the serious oxidation and cracks on the surface of the weld during welding, improves the continuity and strength of the joints, and forms a dense and firm porous high-entropy alloy structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989872A_ABST
    Figure CN118989872A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of laser welding, and particularly discloses a method for improving titanium / steel dissimilar metal connection by utilizing a porous high-entropy alloy structure, which comprises the following steps: by taking gas atomized FeCoCrNiMn high-entropy alloy powder as a raw material, forming a layer of three-dimensional porous high-entropy alloy structure on a steel plate by adopting a selective laser melting process; and then titanium wire filling welding is conducted on the porous high-entropy alloy structure. The prepared porous high-entropy alloy is compact and firm in structure, good in forming and high in strength and plasticity, and the back face and the side face of the base plate are free of deformation; under the condition that the porous high-entropy alloy middle layer exists, laser filler wire welding seam forming is continuous and uniform, no crack is generated, the problem that titanium / steel dissimilar metal cannot be effectively connected due to large physical and chemical property difference is solved, and the utilization rate and productivity of titanium / steel material connection are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of laser welding, and in particular to a method for improving titanium / steel heterogeneous metal connection by utilizing a porous high entropy alloy structure. Background Art

[0002] Titanium has the advantages of high specific strength, corrosion resistance and high temperature resistance, but its promotion and application is limited by high manufacturing costs. Steel is the most widely used traditional structural material with advantages such as low manufacturing cost and excellent mechanical properties. The high-reliability connection of titanium / steel heterogeneous materials can give full play to the complementary advantages of the two materials in performance and economy, and has broad application prospects in many fields such as aerospace, energy and chemical industry, marine equipment and medical equipment. However, there are large differences between titanium and steel in terms of properties such as melting point, thermal conductivity, and expansion coefficient. Uneven heating and internal stress are prone to occur during the welding process, which reduces the quality of the joint. Brittle intermetallic compounds are easily generated in the joint, causing the joint to crack easily and making it difficult to form a reliable connection.

[0003] High Entropy Alloys (HEAs) are usually composed of at least five main elements in equal molar ratios, and have attracted widespread attention due to their simple crystal structure and complex composition. Their high mixing entropy and multi-principal element characteristics will produce a high entropy effect, inhibiting the formation of intermetallic compounds, and the different sizes and bonding forces between elements will cause the alloy to have lattice distortion and slow diffusion effects. In addition, the "cocktail" effect in performance makes it usually have high strength, high temperature thermal stability and high corrosion resistance. It is precisely because of the various excellent properties of HEAs that their application fields are very wide, mainly including wear-resistant coatings, aviation materials, hydrogen storage materials, thermoelectric materials, biomedical materials, nuclear structural materials, superconducting materials and electromagnetic materials.

[0004] Selective Laser Melting (SLM) is an additive manufacturing (3D printing) technology that uses high-power lasers to melt and solidify metal powder layer by layer to eventually form complex metal parts. SLM technology can produce very complex and fine structures with extremely high material utilization. Since the specimen can be cooled quickly during the SLM process to achieve structural grain refinement, the manufactured metal parts usually have higher mechanical properties such as strength and hardness. The advantages of SLM make it one of the most widely used additive manufacturing technologies.

[0005] There is currently no method to combine high entropy alloys with selective laser melting technology to solve the problem of joining titanium and steel. Summary of the invention

[0006] In view of the problem that titanium / steel heterogeneous metals are difficult to effectively connect, the present invention proposes a method for improving the connection of titanium / steel heterogeneous metals by utilizing a porous high entropy alloy structure. The porous high entropy alloy structure is prepared by laser selective melting technology as an intermediate layer to achieve high-reliability connection of titanium / steel heterogeneous metals.

[0007] In order to achieve the above object, the specific technical solution adopted by the present invention is as follows:

[0008] A method for improving titanium / steel heterogeneous metal connection by using a porous high entropy alloy structure is to use atomized FeCoCrNiMn high entropy alloy powder as raw material, and adopt a laser selective melting process to form a three-dimensional porous high entropy alloy structure between titanium and steel. The three-dimensional porous high entropy alloy structure is a three-dimensional structure with a hollow interior, and the three-dimensional structure has two parallel mesh surfaces with through holes evenly distributed on the upper and lower sides. Such a hollow three-dimensional structure of the porous high entropy alloy structure of the present invention can ensure that the welding wire can be fully wetted and spread after melting during titanium wire and filler wire welding, so as to achieve better bonding between interfaces.

[0009] More specifically, the method for improving titanium / steel heterogeneous metal connection using a porous high entropy alloy structure comprises the following steps:

[0010] S1. Use a steel plate as the substrate, polish it with sandpaper to remove the surface oxide film, clean and wipe it, and finally dry it for use;

[0011] S2. The raw materials were weighed according to the molar ratio of each element in the chemical composition of the high entropy alloy, and FeCoCrNiMn high entropy alloy powder was prepared by vacuum atomization method;

[0012] S3. Draw the porous high entropy alloy structure using 3D mapping software, slice the 3D model, set the thickness of each slice according to the structure height, convert it into a CLS format file and import it into the metal powder rapid prototyping system;

[0013] S4. Place the high entropy alloy powder prepared in S2 into the metal powder rapid prototyping system equipment in S3, clamp the substrate and fixture in S1 to the laser action area, set various process parameters, melt the high entropy alloy powder and solidify it to obtain a porous high entropy alloy structure;

[0014] S5. Use semiconductor laser to perform titanium wire welding on porous high-entropy alloy structure to form an effective connection of titanium / steel dissimilar metals.

[0015] Preferably, in step S2, the particle size of the high entropy alloy powder is in the range of 15 to 50 μm. Powders in this range can provide better printing accuracy and surface finish, facilitate better spreading, absorb laser energy faster, and thus melt faster, thereby improving the density and strength of the finished product; while too small a particle size may result in poor fluidity, making it difficult to spread evenly, affecting the forming effect; too large a particle size may easily produce larger pores in the printed layer, resulting in reduced density of the finished product and deterioration of mechanical properties. The components of the high entropy alloy powder according to mass percentage content are as follows: Fe: 19.98%; Co: 21.06%; Cr: 18.24%; Ni: 21.03%; Mn: 19.69%.

[0016] Preferably, in step S4, the main process parameters used in the laser selective melting structure forming process are: spot diameter 50 μm, laser power 90-120 W, scanning speed 800-1100 mm / s, and one-time powder spreading thickness 0.02 mm.

[0017] Preferably, in step S4, an inert gas with a purity greater than 99.9% is introduced into the printing chamber for high entropy alloy structure forming and heated to 125°C. Too high or too low a temperature may make the structure unsatisfactory, further affecting subsequent forming. If the temperature is too high, the grains will coarsen, and it is easy to form a brittle hard phase or an unfavorable phase transition, resulting in a decrease in mechanical properties; if the temperature is too low, the powder will not be heated sufficiently, which may easily cause problems such as unmelted powder and high particle size, which in turn leads to problems such as poor interface connectivity. Furthermore, the inert gas passed is pure argon.

[0018] Preferably, in step S5, main process parameters of laser wire-filling welding are: spot diameter 50 μm, laser power 900-1100 W, welding speed 3-4 mm / s, wire feeding speed 90-110 cm / min, and defocus 0 mm.

[0019] Preferably, in step S5, an inert gas is introduced during welding, and the gas flow rate is 20 to 30 L / min, so that the front and side surfaces of the welding wire are isolated from the air during welding. If the gas flow rate is less than 20 L / min, the weld cannot be effectively protected, and if it is greater than 30 L / min, the surface quality of the weld will be affected and the strength of the weld will be reduced. Furthermore, the inert gas introduced is pure argon.

[0020] Preferably, the substrate and the fixture are both made of 316L steel.

[0021] The present invention has the following beneficial effects:

[0022] The porous high entropy alloy prepared by the method of the present invention has a dense and firm structure, good forming, high strength and plasticity, and no macroscopic deformation on the back and sides of the substrate; in the case of a porous high entropy alloy intermediate layer, the laser wire welding weld is formed continuously and evenly without cracks, which effectively solves the problem of severe surface oxidation of the weld, multiple obvious cracks, and even separation of the weld from the substrate caused by direct titanium wire welding on the steel plate. Compared with the prior art, the addition of the porous high entropy alloy intermediate layer of the present invention enables the titanium / steel heterogeneous metal to form a high-reliability connection. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 : A schematic diagram of the structure of the fixture designed in Example 1. In the figure, 1-counterbore, 2-groove, 3-threaded hole.

[0024] Figure 2 : Three-dimensional image of the porous high-entropy alloy structure drawn in Example 1.

[0025] Figure 3 : The porous high-entropy alloy structure printed by the metal powder rapid prototyping system equipment in Example 1; wherein, Figure a is the front macroscopic morphology, and Figures b and c are the microscopic morphologies of the structure formed under confocal microscopy.

[0026] Figure 4 : Schematic diagram of the connection of the porous high-entropy alloy structure intermediate layer and the titanium wire laser filling welding joint in Example 1.

[0027] Figure 5 : In Example 1, 316L is the substrate, the porous high-entropy alloy structure is the middle layer, and the macroscopic morphology of titanium wire laser filling welding.

[0028] Figure 6 : The morphology of titanium wire laser welding with wire filling directly on the 316L substrate in Comparative Example 1. Among them, Figure a is a schematic diagram of the connection of the titanium wire laser welding joint with wire filling, Figure b is the macro crack morphology of the weld, and Figure c is the macro peeling morphology of the weld. DETAILED DESCRIPTION

[0029] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.

[0030] Example 1

[0031] In this embodiment, after adding a porous high entropy alloy structure as an intermediate layer, titanium wire laser welding is performed. The specific steps are as follows:

[0032] (1) Draw a CAD drawing, and according to the requirements of fit and tolerance, use milling, drilling and other processes to manufacture a substrate fixture made of 316L material with high positioning accuracy and strong clamping force. The fixture structure of this embodiment is as follows: Figure 1As shown, it includes four countersunk holes 1 for fixing the fixture to the printing chamber, a 4 mm deep groove 2 for placing the substrate, and a threaded hole 3 in the groove 2 for fixing the substrate;

[0033] (2) The substrate is a 316L plate with a size of 150 mm (length) × 150 mm (width) × 4 mm (height). The substrate surface is punched with holes to match the threaded holes 3 in the fixture and can be fixed by tightening with nuts. The substrate is polished with 200#, 400#, and 800# sandpapers in turn to remove the oxide film on the surface, and then repeatedly cleaned and wiped with alcohol cotton balls, and finally dried for use.

[0034] (3) The raw materials are weighed according to the molar ratio of each element in the chemical composition of the high entropy alloy, and a FeCoCrNiMn high entropy alloy powder with high purity, low oxygen content, uniform composition and good sphericity is prepared by a vacuum atomization method; the particle size of the high entropy alloy powder is in the range of 15 to 50 μm, and its component composition in terms of mass percentage is as follows: Fe: 19.98%; Co: 21.06%; Cr: 18.24%; Ni: 21.03%; Mn: 19.69%.

[0035] (4) Figure 2 As shown, a porous high-entropy alloy structure is drawn using 3D mapping software. In this embodiment, the porous high-entropy alloy structure is a flat, long rectangular structure with a hollow interior, and the upper and lower surfaces are mesh surfaces, with through holes evenly distributed on each surface. The 3D model is sliced, and the thickness of each slice is printed according to the height of the structure, and the file is converted into a CLS format and imported into the metal powder rapid prototyping system.

[0036] (5) The high entropy alloy powder prepared in (3) is placed in the metal powder rapid prototyping system equipment in (4), and the substrate in (2) is clamped and installed in the laser action area with the fixture in (1); various process parameters are set: spot diameter 50 μm, laser power 100 W, scanning speed 1000 mm / s, and one-time powder thickness 0.02 mm; pure argon gas with a purity greater than 99.9% is introduced into the printing chamber and heated to 125° C., and then the high entropy alloy powder is melted and solidified to obtain a porous high entropy alloy structure, such as Figure 3 As shown, the prepared porous high entropy alloy has a dense and strong structure and is well formed.

[0037] (6) Using semiconductor laser to perform titanium wire welding on porous high entropy alloy structure (the schematic diagram of welding joint connection is shown in Figure 4As shown in the figure, the main process parameters of laser wire filling welding are: spot diameter 50μm, laser power 1100W, welding speed 3mm / s, wire feeding speed 100cm / min, defocusing amount 0mm; pure argon gas is introduced during welding with a gas flow rate of 25L / min to isolate the front and sides of the welding wire from the air during welding.

[0038] like Figure 5 As shown, in this embodiment, when there is a porous high-entropy alloy intermediate layer, the laser wire welding weld is formed continuously and uniformly, with slight oxidation and no cracks.

[0039] Comparative Example 1

[0040] This comparative example has no porous high entropy alloy structure, and the titanium wire is directly welded on the steel plate. The specific steps are as follows:

[0041] (1) The 316L substrate was polished with 200#, 400#, and 800# sandpaper in turn to remove the surface oxide film, and then repeatedly cleaned and wiped with alcohol cotton balls, and finally dried for later use.

[0042] (2) Assemble and fix the processed 316L substrate.

[0043] (3) A semiconductor laser was used to perform titanium wire welding on the steel plate. The main process parameters of laser wire welding were: spot diameter 50 μm, laser power 1100 W, welding speed 3 mm / s, wire feeding speed 100 cm / min, and defocus 0 mm. During the welding process, pure argon gas was introduced at a flow rate of 25 L / min to isolate the front of the welding area of ​​the plate to be welded from the air.

[0044] like Figure 6 As shown in the figure, the weld surface is severely oxidized, with many obvious cracks, and even the weld is peeled off from the substrate. The weld cross section is observed under a light microscope, and there are many obvious cracks.

[0045] Comparative Example 2

[0046] In this comparative example, the porous high entropy alloy intermediate layer of Example 1 was prepared by a sintering method for connecting titanium / steel dissimilar metals.

[0047] Experiments have found that sintering methods usually require higher temperatures (about 1200°C) and complex equipment, which increases the complexity of the process and production costs. For high-entropy alloy materials, controlling the temperature and time during the sintering process is particularly critical. Any carelessness will lead to the degradation of material properties. In addition, during the high-temperature sintering process, high-entropy alloy powders may react with oxygen in the air, causing oxidation, which in turn affects the performance of the coating.

[0048] In contrast, the porous high-entropy alloy intermediate layer structure prepared by laser selective melting has no redox reaction, good forming effect, strong connection performance, and simple process and preparation.

[0049] In summary, the method of preparing porous high-entropy alloy intermediate layer structure by laser selective melting for titanium / steel dissimilar metal joining is superior.

[0050] This specific implementation is only an explanation of the present invention, not a limitation of the present invention. Any changes made by those skilled in the art after reading the specification of the present invention will be protected by the patent law as long as they are within the scope of the claims of the present invention.

Claims

1. A method for improving titanium / steel heterogeneous metal connection using a porous high entropy alloy structure, characterized in that: It uses atomized FeCoCrNiMn high entropy alloy powder as raw material and adopts laser selective melting process to form a three-dimensional porous high entropy alloy structure between titanium and steel.

2. The method for improving titanium / steel heterogeneous metal connection using a porous high entropy alloy structure according to claim 1, characterized in that: The three-dimensional porous high entropy alloy structure is a three-dimensional structure with a hollow interior, and the three-dimensional structure has two upper and lower parallel mesh surfaces with evenly distributed through holes.

3. The method for improving titanium / steel heterogeneous metal connection by using a porous high entropy alloy structure according to claim 1 or 2, characterized in that: The following steps are involved: S1. Use a steel plate as the substrate, polish it with sandpaper to remove the surface oxide film, clean and wipe it, and finally dry it for use; S2. The raw materials were weighed according to the molar ratio of each element in the chemical composition of the high entropy alloy, and FeCoCrNiMn high entropy alloy powder was prepared by vacuum atomization method; S3. Draw the porous high entropy alloy structure using 3D mapping software, slice the 3D model, set the thickness of each slice according to the structure height, convert it into a CLS format file and import it into the metal powder rapid prototyping system; S4. Place the high entropy alloy powder prepared in S2 into the metal powder rapid prototyping system equipment in S3, clamp the substrate and fixture in S1 to the laser action area, set various process parameters, melt the high entropy alloy powder and solidify it to obtain a porous high entropy alloy structure; S5. Use semiconductor laser to perform titanium wire welding on porous high-entropy alloy structure to form an effective connection of titanium / steel dissimilar metals.

4. The method for improving titanium / steel heterogeneous metal bonding using a porous high entropy alloy structure according to claim 3, characterized in that: In step S2, the particle size of the high entropy alloy powder is in the range of 15 to 50 μm, and its components are as follows according to mass percentage content: Fe: 19.98%; Co: 21.06%; Cr: 18.24%; Ni: 21.03%; Mn: 19.69%.

5. The method for improving titanium / steel heterogeneous metal connection by using a porous high entropy alloy structure according to claim 3, characterized in that: In step S4, the main process parameters used in the laser selective melting structure forming process are: spot diameter 50 μm, laser power 90-120 W, scanning speed 800-1100 mm / s, and one-time powder coating thickness 0.02 mm.

6. The method for improving titanium / steel heterogeneous metal connection using a porous high entropy alloy structure according to claim 3, characterized in that: In step S4, the high entropy alloy structure is formed by introducing an inert gas with a purity greater than 99.9% into the printing chamber and heating it to 125°C.

7. The method for improving titanium / steel heterogeneous metal connection using a porous high entropy alloy structure according to claim 6, characterized in that: In step S4, the inert gas is pure argon.

8. The method for improving titanium / steel heterogeneous metal connection using a porous high entropy alloy structure according to claim 3, characterized in that: In step S5, the main process parameters of laser wire welding are: spot diameter 50 μm, laser power 900-1100 W, welding speed 3-4 mm / s, wire feeding speed 90-110 cm / min, and defocusing amount 0 mm.

9. The method for improving titanium / steel heterogeneous metal connection by using a porous high entropy alloy structure according to claim 3, characterized in that: In step S5, an inert gas is introduced during the welding process, and the gas flow rate is 20 to 30 L / min, so that the front and side surfaces of the welding wire are isolated from the air during the welding process.

10. The method for improving titanium / steel heterogeneous metal connection by using a porous high entropy alloy structure according to claim 9, characterized in that: In step S5, the inert gas is pure argon.

Citation Information

Patent Citations

  • High speed welding apparatus with interchangeable weld fixture capability

    CA2358279A1

  • High-entropy flux-cored wire used for titanium-steel MIG welding and preparing method thereof

    CN107999991A

  • High entropy alloy material for welding and application

    CN109955004A

  • Presetting powder high-entropy alloy laser welding method

    CN111318805A

  • Method for inhibiting generation of brittle intermetallic compounds of welded joint through laser high-entropy powder filling welding

    CN111590204A

Cited By

  • Laser arc hybrid welding method and T-shaped structure

    CN120985103A

  • Laser beam machining method for aluminum steel laser melt-brazing dot matrix high-entropy alloy transition layer

    CN122378262A