Resin-based nickel-plated diamond grinding wheel and microwave heating preparation method thereof
By combining resin-based nickel-plated diamond grinding wheels with microwave heating, the problem of weak bonding between abrasive grains and binders is solved, achieving a highly efficient and uniform curing process. This improves the grinding performance and service life of the grinding wheel, making it suitable for precision machining in high-end intelligent equipment, integrated circuits, aerospace technology, and other fields.
Patent Information
- Application Number
- CN202411128154.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
AI Technical Summary
Existing diamond grinding wheels suffer from problems such as weak bonding between abrasive grains and binder, poor self-sharpening properties, and insufficient impact resistance when machining difficult-to-machine materials. This is especially true in manufacturing industries with high efficiency, energy saving, and environmental protection requirements, where traditional preparation methods struggle to achieve an efficient and uniform curing process.
A resin-based nickel-plated diamond grinding wheel is used. By combining nickel-plated diamond abrasive with resin powder and incorporating recycled carbon fiber as a reinforcing phase, and then using microwave heating for post-curing, the bonding force between the abrasive grains and the resin is enhanced, thereby improving the overall performance of the grinding wheel.
It improves grinding performance and service life, reduces grinding temperature, enhances the mechanical properties of grinding wheels, and achieves the goals of short sintering time, simple operation, energy saving and environmental protection, while reducing the risk of internal stress and structural deformation.
Smart Images

Figure CN118990358A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of superhard material application and processing, and in particular relates to a resin-based nickel-plated diamond grinding wheel and a microwave heating preparation method thereof. Background Art
[0002] With the rapid development of high-end intelligent equipment, integrated circuits, industrial automation, aerospace technology, military industry and other industries, higher requirements are placed on the surface quality of various parts, devices and materials processing accuracy. Among them, various difficult-to-process materials, such as composite materials, electronic ceramics, engineering ceramics, optical crystals, etc., have increasing demands for high surface processing at the submicron and nanometer levels. High surface quality processing requires the use of various high-performance diamond grinding wheels. In addition, the requirements for efficient energy saving, emission reduction, and environmental protection in the manufacturing industry are constantly increasing. Precision and ultra-precision grinding processing puts higher requirements on grinding wheels. Grinding wheels must maintain high processing efficiency and processing accuracy, as well as sharpness and self-sharpening. Diamond, as the hardest substance in nature known to humans, is widely used in the preparation of various superhard material tools. In addition to its ultra-high hardness, it also benefits from its high elastic modulus and high wear resistance. Diamond grinding wheel is a superhard material grinding tool made by evenly mixing artificial diamond, auxiliary abrasives, binders and other components in a reasonable proportion and then sintering at high temperature. It is often used in grinding various hard and brittle materials (such as single crystal silicon, ceramic tools, glass, etc.) and components in the field of mechanical precision machining.
[0003] The binders used for diamond grinding wheels are metal, ceramic, and resin. Among them, metal-bonded diamond grinding wheels have high strength, wear resistance, and long service life, but poor self-sharpening. Ceramic binders have good self-sharpening, sharp grinding, and easy dressing. They are not prone to blockage and burning of workpieces during processing; however, ceramic binders themselves are brittle, with poor toughness and impact resistance, and low bonding strength with diamonds, resulting in serious diamond shedding during actual processing. Resin-bonded diamond grinding wheels are impact-resistant, self-sharpening, and simple to manufacture; however, the processing temperature is low, and at the same time, the high surface energy between diamond abrasives and the binder results in weak bonding between diamonds and the binder. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a resin-based nickel-plated diamond grinding wheel and a microwave heating preparation method thereof.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] One of the technical solutions of the present invention:
[0007] A resin-based nickel-plated diamond grinding wheel comprises the following components by mass percentage: 15-40% nickel-plated diamond abrasive, 25-35% resin powder, 30-50% copper powder and 5-10% carbon fiber.
[0008] Furthermore, the particle size of the nickel-plated diamond abrasive is 60-200 meshes, the particle size of the carbon fiber is 100-200 meshes, the particle size of the copper powder is 100-300 meshes, and the particle size of the resin powder is 100-180 meshes.
[0009] Furthermore, the resin powder is polyimide resin powder, epoxy resin powder or phenolic resin powder.
[0010] Furthermore, the carbon fiber is recycled carbon fiber, which is recycled for the second time by microwave pyrolysis.
[0011] Based on the low bonding force between diamond abrasive and resin, the present invention adopts nickel-plated diamond abrasive. Compared with the flat and smooth surface of ordinary diamond abrasive, the surface of nickel-plated diamond abrasive is wrapped with a layer of small uneven protrusions, which increases the holding force between diamond abrasive and resin binder. In addition, the present invention adopts recycled carbon fiber as the reinforcing phase of resin-based nickel-plated diamond grinding wheel. Carbon fiber has the characteristics of light weight, high strength and wear resistance. On the one hand, it enhances the strength of diamond grinding wheel, and on the other hand, it can reduce the weight of grinding wheel and improve the installation and disassembly efficiency; at the same time, carbon fiber has good wave absorption performance, which is conducive to microwave heating in the post-curing stage. Compared with the original carbon fiber, the tensile strength of recycled carbon fiber is slightly reduced, the elastic modulus remains unchanged, and the performance of the original carbon fiber is maintained at more than 90%, and the price is also cheaper.
[0012] The second technical solution of the present invention:
[0013] A method for preparing the resin-based nickel-plated diamond grinding wheel comprises weighing each component according to mass percentage, mixing and tableting, and performing pre-curing and post-curing to obtain the resin-based nickel-plated diamond grinding wheel;
[0014] The post-curing is carried out by microwave heating.
[0015] Furthermore, the post-curing temperature is 100-200° C., and the heat preservation time is 2-10 hours.
[0016] Furthermore, the pre-curing temperature is 100-180° C., and the heat preservation time is 20-50 minutes.
[0017] Furthermore, the method specifically includes the following steps:
[0018] The nickel-plated diamond abrasive and copper powder are soaked with a wetting agent and mixed evenly, and then resin powder and carbon fiber are added and mixed evenly to obtain a mixture, and then the mixture is poured into a mold for tableting to obtain a green sample, and the green sample is pre-cured and post-cured in sequence, and the post-cured sample is deburred and trimmed to obtain the resin-based nickel-plated diamond grinding wheel.
[0019] Furthermore, the wetting agent is phenolic resin liquid.
[0020] Furthermore, the tabletting pressure is 20-50 MPa, and the pressure holding time is 10-30 min.
[0021] Compared with the prior art, the present invention has the following advantages and technical effects:
[0022] (1) The resin-based nickel-plated diamond grinding wheel of the present invention adopts nickel-plated diamond abrasive grains, which increases the holding force of the resin on the diamond abrasive grains, thereby enhancing the grinding performance and service life of the grinding wheel; and adopts recycled carbon fiber as the reinforcing phase of the grinding wheel, which provides a new way for the recycling of carbon fiber.
[0023] (2) The present invention uses microwaves to post-cure the grinding wheel, which achieves the goals of short sintering time, simple operation, energy saving and environmental protection. At the same time, the diamond grinding wheel cured by microwave sintering has better comprehensive performance. Microwave curing heats the inside and outside of the raw material at the same time, which can reduce or eliminate temperature gradients, achieve more uniform curing, and reduce the internal stress generated during the curing process of the raw material, thereby reducing the risk of structural deformation. The uniform and rapid curing process helps to improve the comprehensive performance of the raw material.
[0024] (3) The resin-based diamond grinding wheel prepared by the present invention has good thermal conductivity, which can reduce the temperature of the surface of the grinding workpiece during grinding, avoiding damage to the workpiece surface due to excessive temperature during grinding, and can withstand large loads during high-speed grinding, and has excellent mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0026] Figure 1 This is a microscopic morphology of the grinding surface of the resin-based nickel-plated diamond grinding wheel prepared in Example 1;
[0027] Figure 2 This is a microscopic morphology of the grinding surface of the resin-based nickel-plated diamond grinding wheel prepared in Example 2;
[0028] Figure 3This is a microscopic morphology of the grinding surface of the resin-based nickel-plated diamond grinding wheel prepared in Example 3;
[0029] Figure 4 This is a microscopic morphology of the grinding surface of the resin-based nickel-plated diamond grinding wheel prepared in Comparative Example 1;
[0030] Figure 5 This is a microscopic morphology of the grinding surface of the resin-based nickel-plated diamond grinding wheel prepared in Comparative Example 2;
[0031] Figure 6 This is a microscopic morphology of the grinding surface of the resin-based nickel-plated diamond grinding wheel prepared in Comparative Example 3;
[0032] Figure 7 This is a microscopic morphology of the grinding surface of the resin-based nickel-plated diamond grinding wheel prepared in Example 4;
[0033] Figure 8 This is a microscopic morphology of the grinding surface of the resin-based nickel-plated diamond grinding wheel prepared in Example 5;
[0034] Fig. 9 This is a microscopic morphology of the grinding surface of the resin-based nickel-plated diamond grinding wheel prepared in Example 6;
[0035] Fig.10 This is a microscopic morphology of the grinding surface of the resin-based nickel-plated diamond grinding wheel prepared in Comparative Example 4;
[0036] Fig.11 This is a microscopic morphology of the grinding surface of the resin-based nickel-plated diamond grinding wheel prepared in Comparative Example 5;
[0037] Fig.12 This is a microscopic morphology of the grinding surface of the resin-based nickel-plated diamond grinding wheel prepared in Comparative Example 6. DETAILED DESCRIPTION
[0038] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0039] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0040] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0041] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0042] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0043] The embodiment of the present invention provides a resin-based nickel-plated diamond grinding wheel, which comprises the following components by mass percentage: 15-40% nickel-plated diamond abrasive, 25-35% resin powder, 30-50% copper powder and 5-10% carbon fiber.
[0044] In a preferred embodiment of the present invention, the particle size of the nickel-plated diamond abrasive is 60-200 mesh, the particle size of the carbon fiber is 100-200 mesh, the particle size of the copper powder is 100-300 mesh, and the particle size of the resin powder is 100-180 mesh.
[0045] In a preferred embodiment of the present invention, the resin powder is polyimide resin powder, epoxy resin powder or phenolic resin powder. More preferably, the resin powder is thermosetting phenolic resin powder.
[0046] In a preferred embodiment of the present invention, the carbon fiber is recycled carbon fiber, which is obtained by secondary recycling by microwave pyrolysis (see: Guan Wenhan. Research on microwave pyrolysis behavior of carbon fiber sucker rod [D]. Kunming University of Science and Technology, 2023. DOI: 10.27200 / d.cnki.gkmlu.2023.000288.). Compared with the original carbon fiber, the tensile strength is slightly reduced, the elastic modulus remains unchanged, and more than 90% of the performance of the original carbon fiber is maintained.
[0047] The embodiment of the present invention further provides a method for preparing the resin-based nickel-plated diamond grinding wheel, comprising weighing each component according to mass percentage, mixing and tableting, and performing pre-curing and post-curing to obtain the resin-based nickel-plated diamond grinding wheel;
[0048] The post-curing is carried out by microwave heating.
[0049] The use of microwaves to post-cure the grinding wheel achieves the goals of short sintering time, simple operation, energy saving and environmental protection. At the same time, the diamond grinding wheel cured by microwave sintering has better comprehensive performance. Microwave curing heats the inside and outside of the raw material at the same time, which can reduce or eliminate temperature gradients and achieve more uniform curing. It can also reduce the internal stress generated during the curing process of the raw material, thereby reducing the risk of structural deformation. The uniform and rapid curing process helps to improve the comprehensive performance of the raw material.
[0050] In a preferred embodiment of the present invention, the post-curing temperature is 100-200° C. and the holding time is 2-10 hours.
[0051] In a preferred embodiment of the present invention, there is no limitation on the power of the microwaves during the microwave heating post-curing process, and it only needs to reach the corresponding post-curing temperature.
[0052] In a preferred embodiment of the present invention, the pre-curing temperature is 100-180° C., and the heat preservation time is 20-50 min.
[0053] In a preferred embodiment of the present invention, the following steps are specifically included:
[0054] The nickel-plated diamond abrasive and copper powder are soaked with a wetting agent and mixed evenly, and then resin powder and carbon fiber are added and mixed evenly to obtain a mixture, and then the mixture is poured into a mold for tableting to obtain a green sample, and the green sample is pre-cured and post-cured in sequence, and the post-cured sample is deburred and trimmed to obtain the resin-based nickel-plated diamond grinding wheel.
[0055] In a preferred embodiment of the present invention, the wetting agent is a phenolic resin liquid.
[0056] In a preferred embodiment of the present invention, the tabletting pressure is 20-50 MPa, and the pressure holding time is 10-30 min.
[0057] In a preferred embodiment of the present invention, the tablets are formed by cold pressing using an oil pressure tablet press.
[0058] All raw materials used in the embodiments of the present invention are commercially available, wherein the nickel content in the nickel-plated diamond is 10wt%-40wt%.
[0059] The technical solution of the present invention is further illustrated by the following embodiments.
[0060] Example 1
[0061] A resin-based nickel-plated diamond grinding wheel is prepared from the following components by mass percentage: 37% nickel-plated diamond abrasive, 25% 2123 thermosetting phenolic resin powder, 30% copper powder, and 8% carbon fiber; the particle size of the nickel-plated diamond abrasive is 140-170 meshes, the particle size of the copper powder is 300 meshes, the particle size of the carbon fiber is 100 meshes, and the particle size of the resin powder is 180 meshes.
[0062] A method for preparing a resin-based nickel-plated diamond grinding wheel comprises the following steps:
[0063] (1) Mixing
[0064] Weigh the components according to the above mass percentages, wet the nickel-plated diamond abrasive and copper powder with a wetting agent (phenolic resin solution, the addition amount is 0.03% of the total mass of the nickel-plated diamond abrasive and copper powder) and mix them evenly, and mix and stir for 30 minutes to obtain a mixture A;
[0065] (2) Mixing again
[0066] The resin powder, carbon fiber and mixed material A are mixed evenly, and the mixing and grinding time is 10 minutes to obtain mixed material B;
[0067] (3) Tablet pressing
[0068] Pour the mixture B evenly into the mold and use a hydraulic tablet press to cold press the mixture at a pressure of 20 MPa for 10 minutes to obtain a green sample.
[0069] (4) Pre-curing
[0070] The green sample was placed in a drying oven for pre-curing. The pre-curing temperature was set to 160°C and kept at this temperature for 20 minutes. After the end of the heat preservation, it was allowed to cool naturally to below 40°C and taken out to obtain a pre-cured sample.
[0071] (5) Post-curing
[0072] The pre-cured sample was placed in a microwave oven for post-curing, the post-curing temperature was set to 170°C, and kept at this temperature for 4 hours. After the end of the heat preservation, it was allowed to cool naturally to below 40°C, and it was taken out to obtain a post-cured sample;
[0073] (6) Trimming and forming
[0074] The post-cured sample was deburred and trimmed to obtain a resin-based nickel-plated diamond grinding wheel.
[0075] Example 2
[0076] A resin-based nickel-plated diamond grinding wheel is prepared from the following components by mass percentage: 37% nickel-plated diamond abrasive, 25% 2123 thermosetting phenolic resin powder, 30% copper powder, and 8% carbon fiber; the particle size of the nickel-plated diamond abrasive is 140-170 meshes, the particle size of the copper powder is 300 meshes, the particle size of the carbon fiber is 100 meshes, and the particle size of the resin powder is 180 meshes.
[0077] A method for preparing a resin-based nickel-plated diamond grinding wheel comprises the following steps:
[0078] (1) Mixing
[0079] Weigh the components according to the above mass percentages, wet the nickel-plated diamond abrasive and copper powder with a wetting agent (phenolic resin solution, the addition amount is 0.03% of the total mass of the nickel-plated diamond abrasive and copper powder) and mix them evenly, and mix and stir for 30 minutes to obtain a mixture A;
[0080] (2) Mixing again
[0081] The resin powder, carbon fiber and mixed material A are mixed evenly, and the mixing and grinding time is 10 minutes to obtain mixed material B;
[0082] (3) Tablet pressing
[0083] Pour the mixture B evenly into the mold and use a hydraulic tablet press to cold press the mixture at a pressure of 20 MPa for 10 minutes to obtain a green sample.
[0084] (4) Pre-curing
[0085] The green sample was placed in a drying oven for pre-curing. The pre-curing temperature was set to 160°C and kept at this temperature for 20 minutes. After the end of the heat preservation, it was allowed to cool naturally to below 40°C and taken out to obtain a pre-cured sample.
[0086] (5) Post-curing
[0087] The pre-cured sample was placed in a microwave oven for post-curing, the post-curing temperature was set to 170°C, and kept at this temperature for 6 hours. After the end of the heat preservation, it was allowed to cool naturally to below 40°C, and it was taken out to obtain a post-cured sample;
[0088] (6) Trimming and forming
[0089] The post-cured sample was deburred and trimmed to obtain a resin-based nickel-plated diamond grinding wheel.
[0090] Example 3
[0091] A resin-based nickel-plated diamond grinding wheel is prepared from the following components by mass percentage: 37% nickel-plated diamond abrasive, 25% 2123 thermosetting phenolic resin powder, 30% copper powder, and 8% carbon fiber; the particle size of the nickel-plated diamond abrasive is 140-170 meshes, the particle size of the copper powder is 300 meshes, the particle size of the carbon fiber is 100 meshes, and the particle size of the resin powder is 180 meshes.
[0092] A method for preparing a resin-based nickel-plated diamond grinding wheel comprises the following steps:
[0093] (1) Mixing
[0094] Weigh the components according to the above mass percentages, wet the nickel-plated diamond abrasive and copper powder with a wetting agent (phenolic resin solution, the addition amount is 0.03% of the total mass of the nickel-plated diamond abrasive and copper powder) and mix them evenly, and mix and stir for 30 minutes to obtain a mixture A;
[0095] (2) Mixing again
[0096] The resin powder, carbon fiber and mixed material A are mixed evenly, and the mixing and grinding time is 10 minutes to obtain mixed material B;
[0097] (3) Tablet pressing
[0098] Pour the mixture B evenly into the mold and use a hydraulic tablet press to cold press the mixture at a pressure of 20 MPa for 10 minutes to obtain a green sample.
[0099] (4) Pre-curing
[0100] The green sample was placed in a drying oven for pre-curing. The pre-curing temperature was set to 160°C and kept at this temperature for 20 minutes. After the end of the heat preservation, it was allowed to cool naturally to below 40°C and taken out to obtain a pre-cured sample.
[0101] (5) Post-curing
[0102] The pre-cured sample was placed in a microwave oven for post-curing. The post-curing temperature was set to 170°C and kept at this temperature for 8 hours. After the heat preservation, it was allowed to cool naturally to below 40°C and taken out to obtain a post-cured sample.
[0103] (6) Trimming and forming
[0104] The post-cured sample was deburred and trimmed to obtain a resin-based nickel-plated diamond grinding wheel.
[0105] Example 4
[0106] A resin-based nickel-plated diamond grinding wheel is prepared from the following components by mass percentage: 40% nickel-plated diamond abrasive, 25% 2123 thermosetting phenolic resin powder, 30% copper powder, and 5% carbon fiber; the particle size of the nickel-plated diamond abrasive is 170-200 meshes, the particle size of the copper powder is 100 meshes, the particle size of the carbon fiber is 200 meshes, and the particle size of the resin powder is 100 meshes.
[0107] A method for preparing a resin-based nickel-plated diamond grinding wheel comprises the following steps:
[0108] (1) Mixing
[0109] Weigh the components according to the above mass percentages, wet the nickel-plated diamond abrasive and copper powder with a wetting agent (phenolic resin solution, the addition amount is 0.03% of the total mass of the nickel-plated diamond abrasive and copper powder) and mix them evenly, and mix and stir for 30 minutes to obtain a mixture A;
[0110] (2) Mixing again
[0111] The resin powder, carbon fiber and mixed material A are mixed evenly, and the mixing and grinding time is 10 minutes to obtain mixed material B;
[0112] (3) Tablet pressing
[0113] Pour the mixture B evenly into the mold and use a hydraulic tablet press to cold press the mixture at a pressure of 40 MPa for 30 minutes to obtain a green sample.
[0114] (4) Pre-curing
[0115] The green sample was placed in a drying oven for pre-curing. The pre-curing temperature was set to 100°C and kept at this temperature for 50 minutes. After the end of the heat preservation, it was allowed to cool naturally to below 40°C and taken out to obtain a pre-cured sample.
[0116] (5) Post-curing
[0117] The pre-cured sample was placed in a microwave oven for post-curing. The post-curing temperature was set to 200°C and kept at this temperature for 2 hours. After the end of the heat preservation, it was allowed to cool naturally to below 40°C and taken out to obtain a post-cured sample.
[0118] (6) Trimming and forming
[0119] The post-cured sample was deburred and trimmed to obtain a resin-based nickel-plated diamond grinding wheel.
[0120] Example 5
[0121] A resin-based nickel-plated diamond grinding wheel is prepared from the following components by mass percentage: 15% nickel-plated diamond abrasive, 25% 2123 thermosetting phenolic resin powder, 50% copper powder, and 10% carbon fiber; the nickel-plated diamond abrasive has a particle size of 170-200 meshes, the copper powder has a particle size of 100 meshes, the carbon fiber has a particle size of 200 meshes, and the resin powder has a particle size of 100 meshes.
[0122] A method for preparing a resin-based nickel-plated diamond grinding wheel comprises the following steps:
[0123] (1) Mixing
[0124] Weigh the components according to the above mass percentages, wet the nickel-plated diamond abrasive and copper powder with a wetting agent (phenolic resin solution, the addition amount is 0.03% of the total mass of the nickel-plated diamond abrasive and copper powder) and mix them evenly, and mix and stir for 30 minutes to obtain a mixture A;
[0125] (2) Mixing again
[0126] The resin powder, carbon fiber and mixed material A are mixed evenly, and the mixing and grinding time is 10 minutes to obtain mixed material B;
[0127] (3) Tablet pressing
[0128] Pour the mixture B evenly into the mold and use a hydraulic tablet press to cold press the mixture at a pressure of 50 MPa for 20 minutes to obtain a green sample.
[0129] (4) Pre-curing
[0130] The green sample was placed in a drying oven for pre-curing. The pre-curing temperature was set to 180°C and kept at this temperature for 20 minutes. After the end of the heat preservation, it was allowed to cool naturally to below 40°C and taken out to obtain a pre-cured sample.
[0131] (5) Post-curing
[0132] The pre-cured sample was placed in a microwave oven for post-curing. The post-curing temperature was set to 100°C and kept at this temperature for 8 hours. After the end of the heat preservation, it was allowed to cool naturally to below 40°C and taken out to obtain a post-cured sample.
[0133] (6) Trimming and forming
[0134] The post-cured sample was deburred and trimmed to obtain a resin-based nickel-plated diamond grinding wheel.
[0135] Example 6
[0136] The same as Example 4, except that a resin-based nickel-plated diamond grinding wheel is prepared from the following components by mass percentage: 20% nickel-plated diamond abrasive, 35% 2123 type thermosetting phenolic resin powder, 35% copper powder, and 10% carbon fiber. The preparation method is the same as Example 4.
[0137] Comparative Example 1
[0138] The same as Example 1, except that the post-curing step is different, which is conventional heating, specifically:
[0139] The pre-cured sample was placed in a constant temperature drying oven for post-curing. The post-curing temperature was set to 170°C and kept at this temperature for 4 hours. After the insulation was completed, it was allowed to cool naturally to below 40°C and was taken out to obtain a post-cured sample.
[0140] Comparative Example 2
[0141] Same as Example 2, except that the post-curing step is different, which is conventional heating, specifically:
[0142] The pre-cured sample was placed in a constant temperature drying oven for post-curing. The post-curing temperature was set to 170°C and kept at this temperature for 6 hours. After the insulation was completed, it was allowed to cool naturally to below 40°C and was taken out to obtain a post-cured sample.
[0143] Comparative Example 3
[0144] Same as Example 3, except that the post-curing step is different, which is conventional heating, specifically:
[0145] The pre-cured sample was placed in a constant temperature drying oven for post-curing. The post-curing temperature was set to 170°C and kept at this temperature for 8 hours. After the insulation was completed, it was allowed to cool naturally to below 40°C and was taken out to obtain a post-cured sample.
[0146] Comparative Example 4
[0147] Same as Example 1, except that the nickel-plated diamond abrasive is replaced with ordinary diamond abrasive (purchased from Weihong Abrasives and Grinding Tools Factory, Changge City, Henan Province), and the preparation method is the same as Example 1.
[0148] Comparative Example 5
[0149] The same as Example 1, except that the post-curing temperature is set to 250° C. and maintained at this temperature for 2 hours.
[0150] Comparative Example 6
[0151] The same as Example 1, except that the post-curing temperature is set to 50° C. and kept at this temperature for 10 hours.
[0152] Performance Testing
[0153] (1) Grinding ratio measurement
[0154] According to the polycrystalline diamond wear ratio determination method, the diamond grinding wheel and a specific workpiece are rubbed against each other on a specified device to measure the grinding ratio. The selected workpiece is a 80-mesh green silicon carbide standard grinding wheel. The measurement results are shown in Table 1.
[0155] Table 1 Grinding ratio measurement results
[0156] Grinding ratio Example 1 9.58 Example 2 10.62 Example 3 10.23 Example 4 8.75 Example 5 8.16 Example 6 9.83 Comparative Example 1 5.80 Comparative Example 2 7.94 Comparative Example 3 7.71 Comparative Example 4 7.13 Comparative Example 5 7.91 Comparative Example 6 6.08
[0157] (2) Scanning electron microscopy characterization
[0158] After grinding with a standard grinding wheel, the samples prepared in Examples 1-3 and Comparative Examples 1-3 were observed using a scanning electron microscope.
[0159] The microstructure of the grinding surface of the resin-based nickel-plated diamond grinding wheel is shown in Figure 1-6 It can be seen that the abrasive grains in the resin-based nickel-plated diamond grinding wheel of Example 1 are tightly combined with the resin binder, and the diamond abrasive grains are intact after grinding, and the structure is well maintained ( Figure 1 ), in the resin-based nickel-plated diamond grinding wheel of Example 2, the diamond abrasive grains are tightly wrapped with the resin-based binder, and the morphology of the diamond abrasive grains is intact ( Figure 2 ), the abrasive grains in the resin-based nickel-plated diamond grinding wheel of Example 3 are tightly combined with the resin binder, and the abrasive grain morphology is good ( Figure 3 ), the abrasive grains in the resin-based nickel-plated diamond grinding wheel of comparative example 1 will have gaps with the resin binder ( Figure 4 ), in comparative example 2, the abrasive grains in the resin-based nickel-plated diamond grinding wheel are closely combined with the resin binder, but there are gaps between the abrasive grains, and some diamond abrasive grains will be broken after grinding. ( Figure 5 ), in comparative example 3, the abrasive grains in the resin-based nickel-plated diamond grinding wheel are tightly wrapped with the resin binder, and the diamond abrasive grains are broken after grinding ( Figure 6 ).
[0160] It can be seen that after comparing the curing by conventional heating (Comparative Examples 1-3) and microwave heating (Examples 1-3), it can be found that after microwave heating curing, the grinding ratio of the resin-based diamond grinding wheel is higher, the performance of the grinding wheel is better, the abrasive grains in the diamond grinding wheel are more closely combined with the resin binder, and the shape of the diamond abrasive grains is more complete.
[0161] After grinding with the standard grinding wheel, the microscopic morphology of the grinding surface of the resin-based nickel-plated diamond grinding wheel and the resin-based ordinary diamond grinding wheel prepared in Examples 4-6 and Comparative Examples 4-6 was observed by scanning electron microscope. The results are shown in FIG. Figure 7-12 It can be seen that the abrasive grains in the resin-based nickel-plated diamond grinding wheel of Example 4 are closely combined with the resin binder, and the diamond grains are intact (see Figure 7 ); The abrasive grains in the resin-based nickel-plated diamond grinding wheel of Example 5 are tightly wrapped with the resin-based binder, but a hole structure appears after grinding, and there are fine cracks on the diamond surface and slight breakage (see Figure 8 ); The abrasive grains in the resin-based nickel-plated diamond grinding wheel of Example 6 are tightly wrapped with the resin binder, and the diamond grains at the grinding surface are intact (see Fig. 9 ); Comparative Example 4 has obvious gaps between the abrasive grains and the resin-based binder in the resin-based ordinary diamond grinding wheel, and the diamond grains are severely broken after grinding (see Fig.10 ); The abrasive grains in the resin-based nickel-plated diamond grinding wheel in Comparative Example 5 are closely combined with the resin binder, the grinding surface is relatively flat, and the diamond particles are relatively complete (see Fig.11 ); In comparative example 6, there is a large gap between the abrasive grains in the resin-based nickel-plated diamond grinding wheel and the resin-based binder when wrapped, and the diamond particles are relatively complete (see Fig.12 ).
[0162] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A resin-based nickel-plated diamond grinding wheel, characterized in that: The invention comprises the following components by mass percentage: 15-40% of nickel-plated diamond abrasive, 25-35% of resin powder, 30-50% of copper powder and 5-10% of carbon fiber.
2. The resin-based nickel-plated diamond grinding wheel according to claim 1, characterized in that: The particle size of the nickel-plated diamond abrasive is 60-200 meshes, the particle size of the carbon fiber is 100-200 meshes, the particle size of the copper powder is 100-300 meshes, and the particle size of the resin powder is 100-180 meshes.
3. The resin-based nickel-plated diamond grinding wheel according to claim 1, characterized in that: The resin powder can be polyimide resin powder, epoxy resin powder or phenolic resin powder.
4. A method for preparing the resin-based nickel-plated diamond grinding wheel according to any one of claims 1 to 3, characterized in that: After weighing each component according to mass percentage, mixing and tableting, and performing pre-curing and post-curing, the resin-based nickel-plated diamond grinding wheel is obtained; The post-curing is carried out by microwave heating.
5. The method for preparing a resin-based nickel-plated diamond grinding wheel according to claim 4, characterized in that: The post-curing temperature is 100-200° C., and the heat preservation time is 2-10 hours.
6. The method for preparing a resin-based nickel-plated diamond grinding wheel according to claim 4, characterized in that: The pre-curing temperature is 100-180° C., and the heat preservation time is 20-50 minutes.
7. The method for preparing a resin-based nickel-plated diamond grinding wheel according to claim 4, characterized in that: The specific steps include: The nickel-plated diamond abrasive and copper powder are soaked with a wetting agent and mixed evenly, and then resin powder and carbon fiber are added and mixed evenly to obtain a mixture, and then the mixture is poured into a mold for tableting to obtain a green sample, and the green sample is pre-cured and post-cured in sequence, and the post-cured sample is deburred and trimmed to obtain the resin-based nickel-plated diamond grinding wheel.
8. The method for preparing a resin-based nickel-plated diamond grinding wheel according to claim 7, characterized in that: The wetting agent is phenolic resin liquid.
9. The method for preparing a resin-based nickel-plated diamond grinding wheel according to claim 7, characterized in that: The tabletting pressure is 20-50 MPa, and the pressure holding time is 10-30 min.
Citation Information
Patent Citations
Grinding wheel with magnetic-field-assisted orderly-distributed nickel-plated diamonds and manufacturing method thereof
CN106002654A
Super-hard grinding wheel for hard alloy blade peripheral grinding and manufacturing method thereof
CN110202490A
Grinding wheel applied to external grinding of silicon carbide crystal bar and preparation method
CN111300289A
Ultrathin and ultra-hard resin grinding wheel for high-speed cutting and preparation method of ultrathin and ultra-hard resin grinding wheel
CN113231970A
Retired carbon fiber reinforced resin sheet grinding wheel uniformly cured by microwaves and preparation method of retired carbon fiber reinforced resin sheet grinding wheel
CN115781536A
Cited By
Diamond surface treatment process with high holding strength