High-strength ceramic core antibacterial pipe and preparation process thereof

By using antibacterial glass fiber and silver-loaded mesoporous silica material in ceramic core antibacterial tubes, combined with modified mullite fibers, the problems of poor stability of antibacterial agents and insufficient flame retardant performance in the prior art are solved, and high efficiency is achieved , long-lasting antibacterial effect and good thermal insulation performance.

CN118991149AActive Publication Date: 2024-11-22JIANGXI HEHUI NEW BUILDING MATERIALS CO LTD

Patent Information

Application Number
CN202411088121.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

The antibacterial agents of existing porcelain core antibacterial pipes have poor stability and insufficient flame retardant and thermal insulation properties, resulting in a short-lasting antibacterial effect and limited scope of application.

Method used

Antibacterial glass fiber, silver-loaded mesoporous silica material combined with polypropylene resin, combined with modified mullite fibers, and prepared high-strength porcelain core antibacterial pipes through specific process treatment to ensure the antibacterial inner layer and heat-resistant outer layer. Synergistic efficiency.

Benefits of technology

It achieves efficient and long-lasting antibacterial properties, improves the flame retardant and thermal insulation of the pipe, extends the service life, and enhances the antibacterial ability against E. coli and Staphylococcus aureus.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of pipes, in particular to a high-strength ceramic core antibacterial pipe and a preparation process thereof. A high-strength ceramic core antibacterial pipe comprises the following parts: an antibacterial inner pipe and a heat-resistant outer pipe, the antibacterial inner pipe is prepared from antibacterial glass fibers, a silver-loaded mesoporous silica material and polypropylene resin, and the antibacterial glass fibers and the silver-loaded mesoporous silica material cooperate with each other to achieve a synergistic effect in the antibacterial inner pipe. The prepared high-strength ceramic core antibacterial pipe has strong antibacterial performance and strong antibacterial durability; the modified mullite fiber, the polypropylene resin and other auxiliaries are mixed to prepare the heat-resistant outer pipe, and the modified mullite fiber has the characteristics of high temperature resistance, low heat conductivity, flame retardance and the like, so that the heat-resistant outer pipe in the high-strength ceramic core antibacterial pipe has good flame retardance, heat insulation effect and thermal dimensional stability; the problem that the pipe is easily deformed and damaged due to heating is avoided, and the service life of the pipe is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pipes, and more particularly to a high-strength porcelain core antibacterial pipe and a preparation process thereof. Background Art

[0002] Ceramic core antibacterial pipe is a pipe material with antibacterial function. The surface of the pipe is attached with antibacterial agent, which can effectively inhibit the growth and reproduction of bacteria in the pipe. It can be widely used in drinking water, chemical, medicine, food and other fields.

[0003] The antimicrobial agents used in porcelain core antibacterial pipes are mainly divided into inorganic antimicrobial agents and organic antimicrobial agents. The commonly used inorganic antimicrobial agents are silver-based antimicrobial agents. This antimicrobial agent mainly loads nanosilver in a carrier by physical adsorption or chemical grafting, and then attaches the loaded carrier to the inner wall of the pipe, and achieves the bactericidal effect by slowly releasing Ag+. However, the current carriers of nanosilver are mainly traditional inorganic carriers such as zeolite, zirconium phosphate, and clay. The main bonding method is ion exchange, which has poor stability, resulting in the shedding and elution of the loaded Ag+, which greatly limits the antibacterial effect and application range of silver-based antimicrobial agents in porcelain core antibacterial pipes; while organic antimicrobial agents mainly include nitrogen-containing ion compounds, quaternary ammonium salt antimicrobial agents and guanidine antimicrobial agents. These organic antimicrobial agents are used in porcelain core antibacterial pipes, and generally have problems such as easy elution and easy decomposition at high temperature, which affects the antibacterial durability of organic antimicrobial agents in porcelain core antibacterial pipes, and it is necessary to regularly replenish antimicrobial agents or replace new pipes.

[0004] In addition, the outer layer of the porcelain core pipes currently sold on the market is usually made of polypropylene. Although polypropylene has many advantages such as light weight, corrosion resistance, long service life, easy installation, and reliable connection, polypropylene materials have poor flame retardant properties, poor dimensional stability, and a high linear expansion coefficient, which causes the porcelain core pipes to be easily deformed by heat, limiting the scope of application and service life of the porcelain core pipes. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a high-strength porcelain core antibacterial pipe and a preparation process thereof which has strong antibacterial performance and strong antibacterial durability and improves the flame retardancy and heat insulation performance of the porcelain core antibacterial pipe.

[0006] A high-strength porcelain core antibacterial pipe, characterized in that it comprises the following parts: an antibacterial inner pipe and a heat-resistant outer pipe;

[0007] The raw materials of the antibacterial inner tube include: antibacterial glass fiber, silver-loaded mesoporous silica material and polypropylene resin, wherein the mixing mass ratio of the antibacterial glass fiber, silver-loaded mesoporous silica material and polypropylene resin is (1-3): (1-3): (45-50);

[0008] The raw materials of the antibacterial glass fiber include: pretreated glass fiber and antibacterial treatment liquid, wherein the mass ratio of the pretreated glass fiber to the antibacterial treatment liquid is (1-10): (30-70), and the pretreated glass fiber is obtained by sequentially treating the glass fiber with hydrogen peroxide and a titanate coupling agent;

[0009] The raw materials of the antibacterial treatment liquid include: 20 to 48 parts by weight of organosilicon quaternary ammonium salt, 4 to 15 parts by weight of ethyl orthosilicate, 50 to 70 parts by weight of anhydrous ethanol and 80 to 130 parts by weight of deionized water;

[0010] The raw materials of the silver-loaded mesoporous silica material include: 5 to 18 parts by weight of surface amination mesoporous silica, 20 to 50 parts by weight of anhydrous ethanol and 20 to 50 parts by weight of a 0.5 mol / L silver nitrate solution, wherein the surface amination mesoporous silica is obtained by dissolving the mesoporous silica in anhydrous ethanol and then modifying it with a silane coupling agent KH-550;

[0011] The raw materials of the heat-resistant outer tube include: polypropylene resin, modified mullite fiber, masterbatch, compatibilizer, lubricant and antioxidant, wherein the mass ratio of the polypropylene resin, modified mullite fiber, masterbatch, compatibilizer, lubricant and antioxidant is (80-140): (20-40): (3-12): (3-8): (0.5-1.5): (0.5-1);

[0012] The raw materials of the modified mullite fiber include: pretreated mullite fiber and 10% by mass of silane coupling agent KH-550 aqueous solution, with a solid-liquid mass ratio of (1-8): (20-50);

[0013] The raw materials of the pretreated mullite fiber include: 30-40 parts by weight of mullite fiber, 60-120 parts by weight of acetone solution and 80-150 parts by weight of 1 mol / L sodium hydroxide solution.

[0014] Furthermore, a preparation process of a high-strength porcelain core antibacterial pipe is characterized by comprising the following steps:

[0015] S1: Preparation of antibacterial glass fiber, using organosilicon quaternary ammonium salt, ethyl orthosilicate, anhydrous ethanol and deionized water to mix to prepare an antibacterial treatment solution, using hydrogen peroxide and titanate coupling agent to pre-treat the glass fiber in turn, immersing the pre-treated glass fiber in the antibacterial treatment solution, stirring, standing, high temperature reaction, washing and drying to obtain the antibacterial glass fiber;

[0016] S2: Preparation of silver-loaded mesoporous silica material, after dissolving mesoporous silica in anhydrous ethanol, dropwise adding silane coupling agent KH-550, stirring and refluxing, filtering and washing to obtain surface-aminated mesoporous silica, after dissolving surface-aminated mesoporous silica in anhydrous ethanol, adding silver nitrate solution, sealing and stirring in a dark place, filtering, washing and drying to obtain silver-loaded mesoporous silica material;

[0017] S3: Preparation of modified mullite fiber, the mullite fiber is placed in an acetone solution, after ultrasonic dispersion, washing and drying, the dried mullite fiber is placed in a sodium hydroxide solution, after heating, washing and drying, to obtain pretreated mullite fiber, the pretreated mullite fiber is placed in a silane coupling agent KH-550 aqueous solution, heated in a water bath for reaction, filtered, washed and dried, to obtain modified mullite fiber;

[0018] S4: Processing of pipe pellets and preparation of high-strength ceramic core antibacterial pipes. Antibacterial glass fiber, silver-loaded mesoporous silica material and polypropylene resin are mixed in proportion and granulated to obtain antibacterial inner layer pellets. Polypropylene resin, modified mullite fiber, masterbatch, compatibilizer, lubricant and antioxidant are mixed in proportion and granulated to obtain heat-resistant outer layer pellets. The antibacterial inner layer pellets and the heat-resistant outer layer pellets are extruded to form pipes respectively to obtain antibacterial inner pipes and heat-resistant outer pipes. After co-extrusion, molding and shaping, cooling, pulling and cutting, the antibacterial inner pipe and the heat-resistant outer pipe are obtained to obtain high-strength ceramic core antibacterial pipes.

[0019] Furthermore, the organosilicon quaternary ammonium salt is 3-(trimethoxysilyl)propyldimethyloctadecylammonium chloride, 3-(trimethoxysilyl)propyltrimethylammonium chloride, 3-(triethoxysilyl)propyldimethyloctadecylammonium chloride or 3-(trihydroxysilylpropyl)dimethyloctadecylammonium chloride.

[0020] Furthermore, step S1 of preparing antibacterial glass fiber specifically comprises the following steps:

[0021] S1.1: After 20 to 48 parts by weight of organosilicon quaternary ammonium salt, 4 to 15 parts by weight of ethyl orthosilicate and 50 to 70 parts by weight of anhydrous ethanol are stirred and mixed, 80 to 130 parts by weight of deionized water are added, and the mixture is stirred and reacted at 25 to 35° C. for 2 to 4 hours to obtain an antibacterial treatment solution;

[0022] S1.2: adding glass fiber to 0.1 mol / L hydrogen peroxide, wherein the solid-liquid mass ratio of the glass fiber to the 0.1 mol / L hydrogen peroxide is (1-7): (10-20), stirring at 60-85° C. for 15-30 min, then taking out the oxidized glass fiber, and completely immersing the oxidized glass fiber in a titanate coupling agent for 40-80 min, filtering, washing and drying to obtain a pretreated glass fiber;

[0023] S1.3: Completely immerse the pretreated glass fiber in the antibacterial treatment solution, the mass ratio of the pretreated glass fiber to the antibacterial treatment solution is (1-10): (30-70), stir for 20-40 minutes, and let stand at room temperature for 30-60 minutes. Then, take out the treated glass fiber and place it in an oven at 100-120°C for grafting reaction for 1-2 hours. After the reaction is completed, take out the reacted glass fiber, wash it with deionized water for 1-3 times, and then place it in an oven at 65-85°C for drying for 30-60 minutes to obtain antibacterial glass fiber.

[0024] Furthermore, the glass fiber has a length of 50 to 100 μm and a diameter of 10 to 30 μm.

[0025] Furthermore, step S2 of preparing silver-loaded mesoporous silica material specifically comprises the following steps:

[0026] S2.1: dissolving 12 to 21 parts by weight of mesoporous silica in 40 to 90 parts by weight of anhydrous ethanol, adding dropwise 15 to 24 parts by weight of silane coupling agent KH-550, stirring and refluxing for 8 to 12 hours to obtain a mixed solution, and then filtering and washing the mixed solution to obtain surface amino-modified mesoporous silica;

[0027] S2.2: Take 5 to 18 parts by weight of surface amino-modified mesoporous silica and dissolve them in 20 to 50 parts by weight of anhydrous ethanol, then add 20 to 50 parts by weight of a 0.5 mol / L silver nitrate solution, seal and stir for 3 to 4 hours in a light-proof manner, then filter, wash with 70% by volume ethanol, wash with deionized water and dry to obtain a silver-loaded mesoporous silica material.

[0028] Furthermore, step S3 of preparing modified mullite fiber specifically comprises the following steps:

[0029] S3.1: 30 to 40 parts by weight of mullite fiber are placed in 60 to 120 parts by weight of acetone solution, ultrasonically dispersed for 1 to 2 hours, washed and dried, and the dried mullite fiber is placed in 80 to 150 parts by weight of a 1 mol / L sodium hydroxide solution, heated at 70 to 80°C for 1 to 2 hours, washed and dried to obtain pretreated mullite fiber;

[0030] S3.2: Place the pretreated mullite fiber into a 10% by mass aqueous solution of silane coupling agent KH-550, the solid-liquid mass ratio of the pretreated mullite fiber to the 10% by mass aqueous solution of silane coupling agent KH-550 is (1-8): (20-50), heat in a water bath at 50-65°C for 2-4 hours, filter after heating, wash with deionized water for 2-5 times, and dry to obtain modified mullite fiber.

[0031] Furthermore, step S4 of processing pipe granules and preparing high-strength ceramic core antibacterial pipes specifically includes the following steps:

[0032] S4.1: Mix the antibacterial glass fiber, the silver-loaded mesoporous silica material and the polypropylene resin in a proportion of (1-3): (1-3): (45-50), stir and mix them with a high-speed stirrer for 5-10 minutes, and then extrude and granulate them with a twin-screw extruder at an extrusion temperature of 180-230° C. to obtain an antibacterial inner layer pellet;

[0033] S4.2: Mix polypropylene resin, modified mullite fiber, masterbatch, compatibilizer, lubricant and antioxidant in proportion, the mixing mass ratio of polypropylene resin, modified mullite fiber, masterbatch, compatibilizer, lubricant and antioxidant is (80-140): (20-40): (3-12): (3-8): (0.5-1.5): (0.5-1), stir and mix with a high-speed stirrer for 5-10 minutes, and then extrude and granulate with a twin-screw extruder at an extrusion temperature of 200-230° C. to obtain heat-resistant outer layer pellets;

[0034] S4.3: putting the antibacterial inner layer pellets into a single screw extruder to extrude to obtain an antibacterial inner tube;

[0035] S4.4: feeding the heat-resistant outer layer pellets into another single screw extruder for extrusion to obtain a heat-resistant outer tube;

[0036] S4.5: The antibacterial inner tube and the heat-resistant outer tube are loaded into the co-extrusion equipment for co-extrusion, and the extruded material is placed in a molding die for molding. After shaping, cooling, pulling and cutting, a high-strength ceramic core antibacterial tube is obtained.

[0037] Furthermore, the compatibilizer is polypropylene grafted maleic anhydride, dibutyl maleate, acrylamide or glycidyl methacrylate, the lubricant is fatty acid amide, stearate or polyethylene wax, and the antioxidant is antioxidant DLTP, antioxidant 1010 or antioxidant 168.

[0038] Furthermore, the extrusion temperature of the single screw extruder in step S4.3 is 180-240°C and the rotation speed is 40-60 r / min, and the extrusion temperature of the single screw extruder in step S4.4 is 180-240°C and the rotation speed is 60-90 r / min.

[0039] The present invention has the following advantages:

[0040] 1. In the present invention, by preparing antibacterial glass fiber, quaternary ammonium salt molecules are grafted onto the surface of the glass fiber, so that the grafted modified glass fiber has antibacterial properties against Escherichia coli and Staphylococcus aureus, and can maintain good antibacterial stability, thus overcoming the problem of poor durability such as easy elution and decomposition when the organic antibacterial agent is directly applied to the pipe.

[0041] 2. In the present invention, silver ions are loaded on the surface of aminated mesoporous silica, so that Ag+ can be evenly and stably distributed on the surface of mesoporous silica, thereby improving the antibacterial durability while ensuring the antibacterial performance, which helps to solve the problems of poor loading stability of nanosilver and poor antibacterial durability of traditional carriers.

[0042] 3. In the present invention, antibacterial inner layer granules are prepared using antibacterial glass fiber, silver-loaded mesoporous silica material and polypropylene resin, and then the antibacterial inner layer granules are used to prepare an antibacterial inner tube. The antibacterial glass fiber and silver-loaded mesoporous silica material cooperate with each other and can play a synergistic role in the antibacterial inner tube, so that the prepared high-strength porcelain core antibacterial tube has a high-efficiency and long-lasting antibacterial effect, and has an effective antibacterial effect on Escherichia coli and Staphylococcus aureus.

[0043] 4. In the present invention, modified mullite fiber, polypropylene resin and other additives are mixed to prepare heat-resistant outer layer granules, and then the heat-resistant outer layer granules are used to prepare a heat-resistant outer tube. The modified mullite fiber has the characteristics of high temperature resistance, low thermal conductivity and flame retardancy, which can improve the flame retardancy, thermal insulation effect and thermal dimensional stability of high-strength porcelain core antibacterial pipes, reduce the normal use of pipes affected by thermal deformation of pipes, thereby improving the application range and service life of high-strength porcelain core antibacterial pipes. DETAILED DESCRIPTION

[0044] In order to enable persons skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention.

[0045] Example 1

[0046] A preparation process of a high-strength porcelain core antibacterial pipe comprises the following steps:

[0047] S1: Preparation of antibacterial glass fiber,

[0048] S1.1: After 48 parts by weight of 3-(trimethoxysilyl)propyldimethyloctadecylammonium chloride, 15 parts by weight of ethyl orthosilicate and 70 parts by weight of anhydrous ethanol are stirred and mixed, 130 parts by weight of deionized water are added, and the mixture is stirred and reacted at 35° C. for 4 hours to obtain an antibacterial treatment solution;

[0049] S1.2: adding glass fiber to 0.1 mol / L hydrogen peroxide, wherein the length of the glass fiber is 60 μm, the diameter is 20 μm, and the solid-liquid mass ratio of the glass fiber to the 0.1 mol / L hydrogen peroxide is 7:20, stirring at 85°C for 30 minutes, then taking out the oxidized glass fiber, and completely immersing the oxidized glass fiber in a titanate coupling agent for 80 minutes, filtering, washing and drying to obtain a pretreated glass fiber;

[0050] S1.3: The pretreated glass fiber is completely immersed in the antibacterial treatment liquid, the mass ratio of the pretreated glass fiber to the antibacterial treatment is 1:7, after stirring for 40 minutes, it is allowed to stand at room temperature for 60 minutes, then the treated glass fiber is taken out and placed in an oven at 120°C for grafting reaction for 2 hours, after the reaction is completed, the reacted glass fiber is taken out, washed with deionized water for 3 times, and then placed in an oven at 85°C for drying for 60 minutes to obtain the antibacterial glass fiber;

[0051] S2: Preparation of silver-loaded mesoporous silica materials,

[0052] S2.1: 21 parts by weight of mesoporous silica was dissolved in 90 parts by weight of anhydrous ethanol, 24 parts by weight of silane coupling agent KH-550 was added dropwise, and the mixture was stirred and refluxed for 12 hours to obtain a mixed solution, and then the mixed solution was filtered and washed to remove excess silane coupling agent KH-550 to obtain surface amino mesoporous silica;

[0053] S2.2: 18 parts by weight of surface amino-modified mesoporous silica were dissolved in 50 parts by weight of anhydrous ethanol, and then 50 parts by weight of a 0.5 mol / L silver nitrate solution was added, the mixture was sealed and stirred for 4 hours in a dark place, and then filtered, washed with 70% ethanol by volume, washed with deionized water and dried to obtain a silver-loaded mesoporous silica material;

[0054] S3: Preparation of modified mullite fiber,

[0055] S3.1: 40 parts by weight of mullite fiber are dispersed loosely and placed in 120 parts by weight of acetone solution, ultrasonically dispersed for 2 hours, washed and dried, and the dried mullite fiber is placed in 150 parts by weight of a 1 mol / L sodium hydroxide solution, heated at 80°C for 2 hours, washed and dried to obtain pretreated mullite fiber;

[0056] S3.2: The pretreated mullite fiber is placed in a 10% by mass aqueous solution of silane coupling agent KH-550, the solid-liquid mass ratio of the pretreated mullite fiber to the 10% by mass aqueous solution of silane coupling agent KH-550 is 4:25, heated in a water bath at 65°C for 4h, filtered after heating, washed with deionized water 5 times, and dried to obtain modified mullite fiber;

[0057] S4: Pipe material processing and high-strength ceramic core antibacterial pipe preparation,

[0058] S4.1: Mix the antibacterial glass fiber, the silver-loaded mesoporous silica material and the polypropylene resin in a proportion of 3:3:50, stir and mix them with a high-speed stirrer for 10 minutes, and then extrude and granulate them with a twin-screw extruder at an extrusion temperature of 230° C. to obtain an antibacterial inner layer pellet;

[0059] S4.2: Mix polypropylene resin, modified mullite fiber, masterbatch, polypropylene grafted maleic anhydride, stearate and antioxidant DLTP in proportion, the mass ratio of polypropylene resin, modified mullite fiber, masterbatch, polypropylene grafted maleic anhydride, stearate and antioxidant DLTP is 140:40:12:8:1.5:1, stir and mix with a high-speed mixer for 10 minutes, and then extrude and granulate with a twin-screw extruder at an extrusion temperature of 230°C to obtain heat-resistant outer layer pellets;

[0060] S4.3: The antibacterial inner layer pellets are put into a single screw extruder for extrusion at a temperature of 240° C. and a rotation speed of 60 r / min to obtain an antibacterial inner tube;

[0061] S4.4: The heat-resistant outer layer pellets are fed into another single-screw extruder for extrusion at a temperature of 240° C. and a rotation speed of 90 r / min to obtain a heat-resistant outer tube;

[0062] S4.5: The antibacterial inner tube and the heat-resistant outer tube are loaded into the co-extrusion equipment for co-extrusion, and the extruded material is placed in a molding die for molding. After shaping, cooling, pulling and cutting, a high-strength ceramic core antibacterial tube is obtained.

[0063] Example 2

[0064] A preparation process of a high-strength porcelain core antibacterial pipe comprises the following steps:

[0065] S1: Preparation of antibacterial glass fiber,

[0066] S1.1: After 48 parts by weight of 3-(trimethoxysilyl)propyldimethyloctadecylammonium chloride, 15 parts by weight of ethyl orthosilicate and 70 parts by weight of anhydrous ethanol are stirred and mixed, 130 parts by weight of deionized water are added, and the mixture is stirred and reacted at 25° C. for 2 hours to obtain an antibacterial treatment solution;

[0067] S1.2: adding glass fiber to 0.1 mol / L hydrogen peroxide, wherein the length of the glass fiber is 60 μm, the diameter is 20 μm, and the solid-liquid mass ratio of the glass fiber to the 0.1 mol / L hydrogen peroxide is 7:20, stirring at 60°C for 15 minutes, then taking out the oxidized glass fiber, and completely immersing the oxidized glass fiber in a titanate coupling agent for 40 minutes, filtering, washing and drying to obtain a pretreated glass fiber;

[0068] S1.3: The pretreated glass fiber is completely immersed in the antibacterial treatment liquid, the mass ratio of the pretreated glass fiber to the antibacterial treatment is 1:7, after stirring for 20 minutes, it is allowed to stand at room temperature for 30 minutes, then the treated glass fiber is taken out and placed in an oven at 100°C for grafting reaction for 1 hour, after the reaction is completed, the reacted glass fiber is taken out, washed twice with deionized water, and then placed in an oven at 65°C for drying for 30 minutes to obtain the antibacterial glass fiber;

[0069] S2: Preparation of silver-loaded mesoporous silica materials,

[0070] S2.1: 21 parts by weight of mesoporous silica were dissolved in 90 parts by weight of anhydrous ethanol, 24 parts by weight of silane coupling agent KH-550 were added dropwise, and the mixture was stirred and refluxed for 8 hours to obtain a mixed solution, and then the mixed solution was filtered and washed to remove excess silane coupling agent KH-550 to obtain surface amino-modified mesoporous silica;

[0071] S2.2: 18 parts by weight of surface amino-modified mesoporous silica were dissolved in 50 parts by weight of anhydrous ethanol, and then 50 parts by weight of a 0.5 mol / L silver nitrate solution was added, and the mixture was sealed and stirred for 3 hours in a dark place, and then filtered, washed with 70% ethanol by volume, washed with deionized water, and dried to obtain a silver-loaded mesoporous silica material;

[0072] S3: Preparation of modified mullite fiber,

[0073] S3.1: 40 parts by weight of mullite fiber are dispersed loosely and placed in 120 parts by weight of acetone solution, ultrasonically dispersed for 1 hour, washed and dried, and the dried mullite fiber is placed in 150 parts by weight of a 1 mol / L sodium hydroxide solution, heated at 70°C for 1 hour, washed and dried to obtain pretreated mullite fiber;

[0074] S3.2: The pretreated mullite fiber is placed in a 10% by mass silane coupling agent KH-550 aqueous solution, the solid-liquid mass ratio of the pretreated mullite fiber to the 10% by mass silane coupling agent KH-550 aqueous solution is 4:25, heated in a 50°C water bath for 2h, after the heating is completed, filtered, washed twice with deionized water, and dried to obtain modified mullite fiber;

[0075] S4: Pipe material processing and high-strength ceramic core antibacterial pipe preparation,

[0076] S4.1: Mix the antibacterial glass fiber, the silver-loaded mesoporous silica material and the polypropylene resin in a proportion of 3:3:50, stir and mix them with a high-speed stirrer for 5 minutes, and then extrude and granulate them with a twin-screw extruder at an extrusion temperature of 180° C. to obtain an antibacterial inner layer pellet;

[0077] S4.2: Mix polypropylene resin, modified mullite fiber, masterbatch, polypropylene grafted maleic anhydride, stearate and antioxidant DLTP in proportion, the mass ratio of polypropylene resin, modified mullite fiber, masterbatch, polypropylene grafted maleic anhydride, stearate and antioxidant DLTP is 140:40:12:8:1.5:1, stir and mix with a high-speed mixer for 10 minutes, and then extrude and granulate with a twin-screw extruder at an extrusion temperature of 200°C to obtain heat-resistant outer layer pellets;

[0078] S4.3: The antibacterial inner layer pellets are put into a single screw extruder for extrusion at a temperature of 180° C. and a rotation speed of 40 r / min to obtain an antibacterial inner tube;

[0079] S4.4: The heat-resistant outer layer pellets are fed into another single-screw extruder for extrusion at an extrusion temperature of 180°C and a rotation speed of 60 r / min to obtain a heat-resistant outer tube;

[0080] S4.5: The antibacterial inner tube and the heat-resistant outer tube are loaded into the co-extrusion equipment for co-extrusion, and the extruded material is placed in a molding die for molding. After shaping, cooling, pulling and cutting, a high-strength ceramic core antibacterial tube is obtained.

[0081] Example 3

[0082] A preparation process of a high-strength porcelain core antibacterial pipe comprises the following steps:

[0083] S1: Preparation of antibacterial glass fiber,

[0084] S1.1: 20 parts by weight of 3-(trimethoxysilyl)propyldimethyloctadecylammonium chloride, 4 parts by weight of ethyl orthosilicate and 50 parts by weight of anhydrous ethanol were stirred and mixed, and then 80 parts by weight of deionized water were added, and the mixture was stirred and reacted at 35° C. for 4 hours to obtain an antibacterial treatment solution;

[0085] S1.2: adding glass fiber to 0.1 mol / L hydrogen peroxide, wherein the length of the glass fiber is 60 μm, the diameter is 20 μm, and the solid-liquid mass ratio of the glass fiber to the 0.1 mol / L hydrogen peroxide is 1:10, stirring at 85°C for 30 minutes, then taking out the oxidized glass fiber, and completely immersing the oxidized glass fiber in a titanate coupling agent for 80 minutes, filtering, washing and drying to obtain a pretreated glass fiber;

[0086] S1.3: The pretreated glass fiber is completely immersed in the antibacterial treatment liquid, the mass ratio of the pretreated glass fiber to the antibacterial treatment is 1:30, after stirring for 40 minutes, it is allowed to stand at room temperature for 60 minutes, then the treated glass fiber is taken out and placed in an oven at 120°C for grafting reaction for 2 hours, after the reaction is completed, the reacted glass fiber is taken out, washed with deionized water for 3 times, and then placed in an oven at 85°C for drying for 60 minutes to obtain the antibacterial glass fiber;

[0087] S2: Preparation of silver-loaded mesoporous silica materials,

[0088] S2.1: 12 parts by weight of mesoporous silica was dissolved in 40 parts by weight of anhydrous ethanol, 15 parts by weight of silane coupling agent KH-550 was added dropwise, and the mixture was stirred and refluxed for 12 hours to obtain a mixed solution, and then the mixed solution was filtered and washed to remove excess silane coupling agent KH-550 to obtain surface amino mesoporous silica;

[0089] S2.2: Take 5 parts by weight of surface amino mesoporous silica and dissolve it in 20 parts by weight of anhydrous ethanol, then add 20 parts by weight of a 0.5 mol / L silver nitrate solution, seal and stir for 4 hours in a dark place, then filter, wash with 70% ethanol by volume, wash with deionized water and dry to obtain a silver-loaded mesoporous silica material;

[0090] S3: Preparation of modified mullite fiber,

[0091] S3.1: 30 parts by weight of mullite fiber are dispersed loosely and placed in 60 parts by weight of acetone solution, ultrasonically dispersed for 2 hours, washed and dried, and the dried mullite fiber is placed in 80 parts by weight of 1 mol / L sodium hydroxide solution, heated at 80°C for 2 hours, washed and dried to obtain pretreated mullite fiber;

[0092] S3.2: The pretreated mullite fiber is placed in a 10% by mass silane coupling agent KH-550 aqueous solution, the solid-liquid mass ratio of the pretreated mullite fiber to the 10% by mass silane coupling agent KH-550 aqueous solution is 1:20, heated in a water bath at 65°C for 4 hours, filtered after heating, washed with deionized water 5 times, and dried to obtain modified mullite fiber;

[0093] S4: Pipe material processing and high-strength ceramic core antibacterial pipe preparation,

[0094] S4.1: Mix the antibacterial glass fiber, the silver-loaded mesoporous silica material and the polypropylene resin in a proportion of 1:1:45, stir and mix them with a high-speed stirrer for 10 minutes, and then extrude and granulate them with a twin-screw extruder at an extrusion temperature of 230° C. to obtain an antibacterial inner layer pellet;

[0095] S4.2: Mix polypropylene resin, modified mullite fiber, masterbatch, polypropylene grafted maleic anhydride, stearate and antioxidant DLTP in proportion, the mixing mass ratio of polypropylene resin, modified mullite fiber, masterbatch, polypropylene grafted maleic anhydride, stearate and antioxidant DLTP is 80:20:3:3:0.5:0.5, stir and mix with a high-speed stirrer for 10 minutes, and then extrude and granulate with a twin-screw extruder at an extrusion temperature of 230°C to obtain heat-resistant outer layer pellets;

[0096] S4.3: The antibacterial inner layer pellets are put into a single screw extruder for extrusion at a temperature of 240° C. and a rotation speed of 60 r / min to obtain an antibacterial inner tube;

[0097] S4.4: The heat-resistant outer layer pellets are fed into another single-screw extruder for extrusion at a temperature of 240° C. and a rotation speed of 90 r / min to obtain a heat-resistant outer tube;

[0098] S4.5: The antibacterial inner tube and the heat-resistant outer tube are loaded into the co-extrusion equipment for co-extrusion, and the extruded material is placed in a molding die for molding. After shaping, cooling, pulling and cutting, a high-strength ceramic core antibacterial tube is obtained.

[0099] Comparative Example 1

[0100] Compared with Example 1, the difference of Comparative Example 1 is that the antibacterial glass fiber in step S4.1 is removed, and the other steps remain unchanged to prepare a high-strength porcelain core antibacterial pipe, which is recorded as Comparative Example 1.

[0101] Comparative Example 2

[0102] Compared with Example 1, the difference of Comparative Example 2 is that the silver-loaded mesoporous silica material in step S4.1 is removed, and the other steps remain unchanged to prepare a high-strength ceramic core antibacterial tubing, which is recorded as Comparative Example 2.

[0103] Comparative Example 3

[0104] Compared with Example 1, the difference of Comparative Example 3 is that the antibacterial glass fiber in step S4.1 is replaced by organosilicon quaternary ammonium salt, and the other steps remain unchanged to prepare a high-strength porcelain core antibacterial pipe, which is recorded as Comparative Example 3.

[0105] Comparative Example 4

[0106] Compared with Example 1, the difference of Comparative Example 4 is that the modified mullite fiber in step S4.2 is removed, and the other steps remain unchanged to prepare a high-strength ceramic core antibacterial tubing, which is recorded as Comparative Example 4.

[0107] One high-strength porcelain core antibacterial pipe prepared in Examples 1-3 and Comparative Examples 1-3 was selected as a sample, and the sample was cut from the center and cut into 5 cm pipe sheets as test samples. According to the method specified in the standard JC / T939-2004 "Antibacterial Performance of Antibacterial Plastic Pipes for Construction", the test samples were tested for antibacterial performance and antibacterial durability, wherein the durability test was to immerse the test samples in a deionized water bath at a temperature of 50°C for 24 hours, and then test their antibacterial performance against Escherichia coli and Staphylococcus aureus. The results are shown in Table 1.

[0108] Table 1: Antibacterial performance and antibacterial durability test results

[0109]

[0110] As shown in Table 1, the high-strength ceramic core antibacterial pipes prepared in Examples 1-3 have an antibacterial rate of more than 99% against Escherichia coli and Staphylococcus aureus, and after being treated with a durable immersion, the antibacterial rate can still be maintained at more than 99%, and have strong antibacterial performance and strong antibacterial durability. In contrast, although the high-strength ceramic core antibacterial pipes in Comparative Examples 1-3 also have antibacterial performance, the antibacterial rate and the antibacterial rate after durability treatment are less than the high-strength ceramic core antibacterial pipes in Examples 1-3, indicating that adding antibacterial glass fiber or silver-loaded mesoporous silica material to the antibacterial inner tube of the high-strength ceramic core antibacterial pipe can play an antibacterial role against Escherichia coli and Staphylococcus aureus, but the antibacterial effect of the two in combination can play a synergistic role, so that the high-strength ceramic core antibacterial pipe has a strong antibacterial performance. In addition, after the durability immersion treatment, the antibacterial effect of the test samples of Comparative Examples 2-3 on Escherichia coli and Staphylococcus aureus decreased significantly, indicating that by adding silver-loaded mesoporous silica material and loading silicone quaternary ammonium salt in glass fiber, it can help improve the antibacterial durability of high-strength ceramic core antibacterial pipes against Escherichia coli and Staphylococcus aureus, so that the high-strength ceramic core antibacterial pipes have efficient and long-lasting antibacterial effects.

[0111] The flame retardancy, thermal insulation and linear expansion coefficient of the high-strength porcelain core antibacterial pipes prepared in Examples 1-3 and Comparative Example 4 were tested, wherein the flame retardancy was tested using the GB / T2406.2-2009 method, the thermal insulation was tested using the GB / T5990 method, and the linear expansion coefficient was tested using the GB / T1036 method. The test results are shown in Table 2.

[0112] Table 2: Test results of flame retardancy, thermal insulation and linear expansion coefficient

[0113] Group Oxygen index LOI (%) Thermal conductivity (W / (m*K)) Linear expansion coefficient (μm / (m*℃)) Example 1 36.24 0.07 2.5 Example 2 35.68 0.1 2.9 Example 3 36.06 0.08 2.7 Comparative Example 4 32.51 0.14 5.6

[0114] As can be seen from Table 2, the oxygen index test results of the high-strength porcelain core antibacterial pipes prepared in Examples 1-3 are greater than that of Comparative Example 4, while the thermal conductivity and linear expansion coefficient test results are less than those of Comparative Example 3, indicating that the high-strength porcelain core antibacterial pipes in Examples 1-3 have good flame retardant properties, thermal insulation properties and thermal dimensional stability. The addition of modified mullite fibers can effectively improve the linear expansion coefficient and thermal conductivity of the high-strength porcelain core antibacterial pipes, thereby reducing deformation of the pipes after being heated.

[0115] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all such improvements and changes should fall within the scope of protection of the appended claims of the present invention. Parts not described in detail in this specification belong to the prior art known to those skilled in the art.

Claims

1. A high-strength porcelain core antibacterial pipe, It is characterized in that It includes the following parts: antibacterial inner tube and heat-resistant outer tube; The raw materials of the antibacterial inner tube include: antibacterial glass fiber, silver-loaded mesoporous silica material and polypropylene resin, wherein the mixing mass ratio of the antibacterial glass fiber, silver-loaded mesoporous silica material and polypropylene resin is (1-3): (1-3): (45-50); The raw materials of the antibacterial glass fiber include: pretreated glass fiber and antibacterial treatment liquid, wherein the mass ratio of the pretreated glass fiber to the antibacterial treatment liquid is (1-10): (30-70), and the pretreated glass fiber is obtained by sequentially treating the glass fiber with hydrogen peroxide and a titanate coupling agent; The raw materials of the antibacterial treatment liquid include: 20 to 48 parts by weight of organosilicon quaternary ammonium salt, 4 to 15 parts by weight of ethyl orthosilicate, 50 to 70 parts by weight of anhydrous ethanol and 80 to 130 parts by weight of deionized water; The raw materials of the silver-loaded mesoporous silica material include: 5 to 18 parts by weight of surface amination mesoporous silica, 20 to 50 parts by weight of anhydrous ethanol and 20 to 50 parts by weight of a 0.5 mol / L silver nitrate solution, wherein the surface amination mesoporous silica is obtained by dissolving the mesoporous silica in anhydrous ethanol and then modifying it with a silane coupling agent KH-550; The raw materials of the heat-resistant outer tube include: polypropylene resin, modified mullite fiber, masterbatch, compatibilizer, lubricant and antioxidant, wherein the mass ratio of the polypropylene resin, modified mullite fiber, masterbatch, compatibilizer, lubricant and antioxidant is (80-140): (20-40): (3-12): (3-8): (0.5-1.5): (0.5-1); The raw materials of the modified mullite fiber include: pretreated mullite fiber and 10% by mass of silane coupling agent KH-550 aqueous solution, with a solid-liquid mass ratio of (1-8): (20-50); The raw materials of the pretreated mullite fiber include: 30-40 parts by weight of mullite fiber, 60-120 parts by weight of acetone solution and 80-150 parts by weight of 1 mol / L sodium hydroxide solution.

2. A preparation process of the high-strength ceramic core antibacterial pipe according to claim 1, It is characterized in that The following steps are involved: S1: Preparation of antibacterial glass fiber, using organosilicon quaternary ammonium salt, ethyl orthosilicate, anhydrous ethanol and deionized water to mix to prepare an antibacterial treatment solution, using hydrogen peroxide and titanate coupling agent to pre-treat the glass fiber in turn, immersing the pre-treated glass fiber in the antibacterial treatment solution, stirring, standing, high temperature reaction, washing and drying to obtain the antibacterial glass fiber; S2: Preparation of silver-loaded mesoporous silica material, after dissolving mesoporous silica in anhydrous ethanol, dropwise adding silane coupling agent KH-550, stirring and refluxing, filtering and washing to obtain surface-aminated mesoporous silica, after dissolving surface-aminated mesoporous silica in anhydrous ethanol, adding silver nitrate solution, sealing and stirring in a dark place, filtering, washing and drying to obtain silver-loaded mesoporous silica material; S3: Preparation of modified mullite fiber, the mullite fiber is placed in an acetone solution, after ultrasonic dispersion, washing and drying, the dried mullite fiber is placed in a sodium hydroxide solution, after heating, washing and drying, to obtain pretreated mullite fiber, the pretreated mullite fiber is placed in a silane coupling agent KH-550 aqueous solution, heated in a water bath for reaction, filtered, washed and dried, to obtain modified mullite fiber; S4: Processing of pipe pellets and preparation of high-strength ceramic core antibacterial pipes. Antibacterial glass fiber, silver-loaded mesoporous silica material and polypropylene resin are mixed in proportion and granulated to obtain antibacterial inner layer pellets. Polypropylene resin, modified mullite fiber, masterbatch, compatibilizer, lubricant and antioxidant are mixed in proportion and granulated to obtain heat-resistant outer layer pellets. The antibacterial inner layer pellets and the heat-resistant outer layer pellets are extruded to form pipes respectively to obtain antibacterial inner pipes and heat-resistant outer pipes. After co-extrusion, molding and shaping, cooling, pulling and cutting, the antibacterial inner pipe and the heat-resistant outer pipe are obtained to obtain high-strength ceramic core antibacterial pipes.

3. A preparation process for a high-strength porcelain core antibacterial pipe according to claim 2, It is characterized in that The organosilicon quaternary ammonium salt is 3-(trimethoxysilyl)propyldimethyloctadecylammonium chloride, 3-(trimethoxysilyl)propyltrimethylammonium chloride, 3-(triethoxysilyl)propyldimethyloctadecylammonium chloride or 3-(trihydroxysilylpropyl)dimethyloctadecylammonium chloride.

4. A preparation process for a high-strength ceramic core antibacterial pipe according to claim 2, It is characterized in that Step S1: Preparation of antibacterial glass fiber, specifically comprising the following steps: S1.1: After 20 to 48 parts by weight of organosilicon quaternary ammonium salt, 4 to 15 parts by weight of ethyl orthosilicate and 50 to 70 parts by weight of anhydrous ethanol are stirred and mixed, 80 to 130 parts by weight of deionized water are added, and the mixture is stirred and reacted at 25 to 35° C. for 2 to 4 hours to obtain an antibacterial treatment solution; S1.2: adding glass fiber to 0.1 mol / L hydrogen peroxide, wherein the solid-liquid mass ratio of the glass fiber to the 0.1 mol / L hydrogen peroxide is (1-7): (10-20), stirring at 60-85° C. for 15-30 min, then taking out the oxidized glass fiber, and completely immersing the oxidized glass fiber in a titanate coupling agent for 40-80 min, filtering, washing and drying to obtain a pretreated glass fiber; S1.3: Completely immerse the pretreated glass fiber in the antibacterial treatment solution, the mass ratio of the pretreated glass fiber to the antibacterial treatment solution is (1-10): (30-70), stir for 20-40 minutes, and let stand at room temperature for 30-60 minutes. Then, take out the treated glass fiber and place it in an oven at 100-120°C for grafting reaction for 1-2 hours. After the reaction is completed, take out the reacted glass fiber, wash it with deionized water for 1-3 times, and then place it in an oven at 65-85°C for drying for 30-60 minutes to obtain antibacterial glass fiber.

5. A preparation process for a high-strength ceramic core antibacterial pipe according to claim 4, It is characterized in that The length of the glass fiber is 50 to 100 μm and the diameter is 10 to 30 μm.

6. A process for preparing a high-strength ceramic core antibacterial pipe according to claim 2, It is characterized in that Step S2: Preparation of silver-loaded mesoporous silica material, specifically comprising the following steps: S2.1: dissolving 12 to 21 parts by weight of mesoporous silica in 40 to 90 parts by weight of anhydrous ethanol, adding dropwise 15 to 24 parts by weight of silane coupling agent KH-550, stirring and refluxing for 8 to 12 hours to obtain a mixed solution, and then filtering and washing the mixed solution to obtain surface amino-modified mesoporous silica; S2.2: Take 5 to 18 parts by weight of surface amino-modified mesoporous silica and dissolve them in 20 to 50 parts by weight of anhydrous ethanol, then add 20 to 50 parts by weight of a 0.5 mol / L silver nitrate solution, seal and stir for 3 to 4 hours in a light-proof manner, then filter, wash with 70% by volume ethanol, wash with deionized water and dry to obtain a silver-loaded mesoporous silica material.

7. The preparation process of a high-strength ceramic core antibacterial pipe according to claim 2, It is characterized in that Step S3: Preparation of modified mullite fiber, specifically comprising the following steps: S3.1: 30 to 40 parts by weight of mullite fiber are placed in 60 to 120 parts by weight of acetone solution, ultrasonically dispersed for 1 to 2 hours, washed and dried, and the dried mullite fiber is placed in 80 to 150 parts by weight of a 1 mol / L sodium hydroxide solution, heated at 70 to 80°C for 1 to 2 hours, washed and dried to obtain pretreated mullite fiber; S3.2: The pretreated mullite fiber is placed in a 10% by mass silane coupling agent KH-550 aqueous solution, and the solid-liquid mass ratio of the pretreated mullite fiber to the 10% by mass silane coupling agent KH-550 aqueous solution is (1 to 8): (20-50), heated in a water bath at 50-65°C for 2-4h. After heating, filtered, washed with deionized water for 2-5 times, and dried to obtain modified mullite fiber.

8. The preparation process of a high-strength ceramic core antibacterial pipe according to claim 2, It is characterized in that Step S4 is processing the pipe granules and preparing the high-strength ceramic core antibacterial pipe, which specifically includes the following steps: S4.1: Mix the antibacterial glass fiber, the silver-loaded mesoporous silica material and the polypropylene resin in a proportion of (1-3): (1-3): (45-50), stir and mix them with a high-speed stirrer for 5-10 minutes, and then extrude and granulate them with a twin-screw extruder at an extrusion temperature of 180-230° C. to obtain an antibacterial inner layer pellet; S4.2: Mix polypropylene resin, modified mullite fiber, masterbatch, compatibilizer, lubricant and antioxidant in proportion, the mixing mass ratio of polypropylene resin, modified mullite fiber, masterbatch, compatibilizer, lubricant and antioxidant is (80-140): (20-40): (3-12): (3-8): (0.5-1.5): (0.5-1), stir and mix with a high-speed stirrer for 5-10 minutes, and then extrude and granulate with a twin-screw extruder at an extrusion temperature of 200-230° C. to obtain heat-resistant outer layer pellets; S4.3: putting the antibacterial inner layer pellets into a single screw extruder to extrude to obtain an antibacterial inner tube; S4.4: feeding the heat-resistant outer layer pellets into another single screw extruder for extrusion to obtain a heat-resistant outer tube; S4.5: The antibacterial inner tube and the heat-resistant outer tube are loaded into the co-extrusion equipment for co-extrusion, and the extruded material is placed in a molding die for molding. After shaping, cooling, pulling and cutting, a high-strength ceramic core antibacterial tube is obtained.

9. A process for preparing a high-strength ceramic core antibacterial pipe according to claim 8, It is characterized in that The compatibilizer is polypropylene grafted maleic anhydride, dibutyl maleate, acrylamide or glycidyl methacrylate, the lubricant is fatty acid amide, stearate or polyethylene wax, and the antioxidant is antioxidant DLTP, antioxidant 1010 or antioxidant 168.

10. A process for preparing a high-strength ceramic core antibacterial pipe according to claim 9, It is characterized in that The single screw extruder in step S4.3 has an extrusion temperature of 180-240°C and a rotation speed of 40-60 r / min. The single screw extruder in step S4.4 has an extrusion temperature of 180-240°C and a rotation speed of 60-90 r / min.

Citation Information

Patent Citations

  • Antibacterial mildew-proof 3D-printing polypropylene wire material and preparation method thereof

    CN109705454A

  • PPR pipe as well as preparation method and application thereof

    CN117267480A

  • POLYMER COMPOSITION (a) PROVIDED WITH ANTISTATICITY, ANTIBACTERIAL PROPERTIES, AND LUMINOSITY IN THE DARK, MOLDING AND COVER MATERIAL USING THE POLYMER COMPOSITION (a), AND MOUNTING METHOD OF COVER MATERIAL ON OUTSIDE SURFACE OF METALLIC ARTICLE

    JP2016055533A

Cited By

  • Antibacterial mildew-proof polypropylene modified material and preparation method thereof

    CN121182066A

  • Antibacterial and mildew-proof polypropylene modified material and preparation method thereof