Rare earth-aluminum phosphite and preparation method, application and composition thereof

By adding aluminum sources and rare earth compounds to the phosphorous acid solution to generate rare earth-aluminum phosphite, the problems of poor fire and thermal stability of existing inorganic phosphorus-based flame retardants during processing are solved, and the flame retardant of polymers is improved Performance and impact strength reduce corrosion.

CN118992995AActive Publication Date: 2024-11-22BAOTOU RESEARCH INSTITUTE OF RARE EARTHS

Patent Information

Application Number
CN202411067640.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-22
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

Existing inorganic phosphorus-based flame retardants such as aluminum hypophosphate are prone to fire during processing, have poor thermal stability and water solubility, and are insufficient in temperature resistance, making it difficult to meet the needs of high flame retardancy and low corrosion.

Method used

By adding an aluminum source slurry to the phosphite solution and adding a rare earth compound slurry, the reaction is to form a rare earth-aluminum phosphite, preferably the reaction temperature and time, and after filtration and drying, the rare earth-aluminum phosphite is obtained, which is used to improve the polymer Flame retardant performance.

Benefits of technology

It improves the flame retardant performance of the polymer, maintains high impact strength and low corrosion, and is suitable for polymers such as nylon and polybutylterephthalate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118992995A_ABST
    Figure CN118992995A_ABST
Patent Text Reader

Abstract

The invention discloses rare earth-aluminum phosphite as well as a preparation method, application and a composition thereof. The preparation method comprises the following steps: (1) dropwise adding an aluminum source slurry into a phosphorous acid solution to obtain an acidic aluminum phosphite slurry; (2) adding the rare earth compound slurry into the acidic aluminum phosphite slurry to obtain rare earth-aluminum phosphite; wherein an aluminum source in the aluminum source slurry is selected from one or more of aluminum hydroxide, pseudo-boehmite, gibbsite and boehmite; the rare earth compound is selected from one or more of rare earth oxide, rare earth hydroxide and rare earth carbonate. The rare earth-aluminum phosphite prepared by the method provided by the invention can effectively improve the flame retardant property of the polymer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a rare earth-aluminum phosphite and a preparation method, application and composition thereof. Background Art

[0002] Inorganic phosphorus flame retardants are favored by users because of their long-lasting flame retardant effect, good thermal stability, non-volatility, and halogen-free. Aluminum hypophosphite is a representative of inorganic phosphorus flame retardants, but it is easy to decompose during use and is prone to fire during processing, especially when the raw materials contain fibers.

[0003] CN116812894A discloses a phosphite material, the chemical formula of which is Al x Zn y (OH) z (HPO3)3·wH2O; wherein 1.5≤x≤2.5; 0<y≤1; 0<z≤1.5, and w is an integer of 0 to 4. The phosphite is a phosphite containing aluminum and zinc, contains hydroxyl groups and water, and has poor thermal stability.

[0004] CN11483991A discloses a method for preparing lanthanum phosphite, wherein lanthanum oxide and a catalyst are added to water, and the water temperature is maintained at 30-35°C to obtain a hydration reaction product. The catalyst is selected from formic acid, acetic acid, sulfuric acid or benzenesulfonic acid. The hydration reaction product is added to a reactor, phosphorous acid is continuously added dropwise, and the temperature of the reactor is maintained at 40-80°C. After the addition is completed, the reaction is kept warm for 2-5 hours to obtain a phosphite rare earth product. The phosphite rare earth product is filtered, dried, and crushed to obtain a finished lanthanum phosphite. The product obtained by this method is lanthanum phosphite, which has poor temperature resistance and high water solubility. Summary of the invention

[0005] In view of this, one object of the present invention is to provide a method for preparing a rare earth-aluminum phosphite. The rare earth-aluminum phosphite prepared by the method of the present invention can effectively improve the flame retardancy of a polymer. Furthermore, after the rare earth-aluminum phosphite prepared by the method of the present invention is added to a polymer, the resulting composition maintains a high impact strength and low corrosiveness. Another object of the present invention is to provide a rare earth-aluminum phosphite. Still another object of the present invention is to provide a use of a rare earth-aluminum phosphite. Still another object of the present invention is to provide a composition.

[0006] The above purpose is achieved through the following technical solutions.

[0007] In one aspect, the present invention provides a method for preparing a rare earth-aluminum phosphite, comprising the following steps:

[0008] (1) adding an aluminum source slurry dropwise to a phosphorous acid solution to obtain an acidic aluminum phosphite slurry;

[0009] (2) adding the rare earth compound slurry to the acidic aluminum phosphite slurry to obtain rare earth-aluminum phosphite;

[0010] Wherein, the aluminum source in the aluminum source slurry is selected from one or more of aluminum hydroxide, pseudo-boehmite, gibbsite, and boehmite;

[0011] The rare earth compound is selected from one or more of rare earth oxides, rare earth hydroxides and rare earth carbonates.

[0012] According to the preparation method of the present invention, preferably, the rare earth compound is selected from one or more of lanthanum oxide, lanthanum hydroxide and lanthanum carbonate.

[0013] According to the preparation method of the present invention, preferably, in step (1), the reaction temperature is 50-140° C., and the reaction time is 1-8 h; in step (2), the reaction temperature is 50-140° C., and the reaction time is 1-8 h.

[0014] According to the preparation method of the present invention, preferably, the mass ratio of the aluminum source to the phosphorous acid is (3.5-6.5):16.88; the molar ratio of the rare earth element in the rare earth compound to the phosphorous acid is (0.2-0.7):2.

[0015] According to the preparation method of the present invention, preferably, step (2) comprises the following steps:

[0016] The rare earth compound slurry is added to the acidic aluminum phosphite slurry, and then reacted at 50-140° C. for 1-8 hours to obtain a reactant; the reactant is filtered and then dried at 100-150° C. to obtain a rare earth-aluminum phosphite.

[0017] According to the preparation method of the present invention, preferably, in the aluminum source slurry, the mass ratio of the aluminum source to water is (4-6):(6-9); in the phosphorous acid solution, the mass ratio of phosphorous acid to water is 16.88:(20-30); in the rare earth compound slurry, the mass ratio of the rare earth compound to water is 1:(0.7-2).

[0018] On the other hand, the present invention provides a rare earth-aluminum phosphite, which is obtained by the above preparation method.

[0019] In another aspect, the present invention provides use of the rare earth-aluminum phosphite in improving the flame retardant properties of polymers.

[0020] In yet another aspect, the present invention provides a composition comprising the rare earth-aluminum phosphite and aluminum alkyl phosphinate.

[0021] According to the composition of the present invention, preferably, the composition further comprises a polymer, and the polymer is selected from one or more of nylon, polybutylene terephthalate, polyethylene terephthalate, polyurethane, and acrylonitrile-styrene-butadiene copolymer.

[0022] The rare earth-aluminum phosphite prepared by the method of the present invention can effectively improve the flame retardancy of polymers. Furthermore, after the rare earth-aluminum phosphite prepared by the method of the present invention is added to a polymer, the resulting composition maintains high impact strength and low corrosiveness. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 and Figure 2 They are SEM images of the rare earth-aluminum phosphite obtained in Example 1 at different magnifications.

[0024] Figure 3 and Figure 4 They are SEM images of the rare earth-aluminum phosphite obtained in Example 2 at different magnifications.

[0025] Figure 5 and Figure 6 They are SEM images of the rare earth-aluminum phosphite obtained in Example 3 at different magnifications.

[0026] Figure 7 EDS pattern of the rare earth-aluminum phosphite obtained in Example 2.

[0027] Figure 8 The XRD diagram of the rare earth-aluminum phosphite obtained in Example 1-3. DETAILED DESCRIPTION

[0028] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0029] <Preparation method of rare earth-aluminum phosphite>

[0030] The preparation method of the present invention comprises the following steps: (1) preparing an acidic aluminum phosphite slurry; and (2) obtaining a rare earth-aluminum phosphite. Detailed description is given below.

[0031] Steps for preparing acid aluminum phosphite slurry

[0032] Aluminum source slurry is added dropwise to the phosphorous acid solution to obtain acidic aluminum phosphite slurry.

[0033] The phosphorous acid solution includes phosphorous acid and water. The mass ratio of phosphorous acid to water may be 16.88:(20-30); preferably 16.88:(22-28). In some embodiments, the mass ratio of phosphorous acid to water is 16.88:(24-26). Phosphorous acid may be mixed with water to form a phosphorous acid solution.

[0034] The aluminum source in the aluminum source slurry can be selected from one or more of aluminum hydroxide, pseudo-boehmite, gibbsite, and boehmite. In some embodiments, the aluminum source is aluminum hydroxide. In other embodiments, the aluminum source is pseudo-boehmite. In still other embodiments, the aluminum source is gibbsite.

[0035] The aluminum source slurry includes an aluminum source and water. The mass ratio of the aluminum source to water can be (4-6): (6-9); preferably (4.5-5.5): (6.5-8.5); more preferably (5-5.2): (7-8).

[0036] The aluminum source may be dispersed in water to form an aluminum source slurry.

[0037] The mass ratio of the aluminum source to the phosphorous acid may be (3.5-6.5):16.88; preferably (4.5-5.5):16.88; more preferably (5.1-5.2):16.88.

[0038] The reaction temperature may be 50 to 140°C; preferably 70 to 110°C; more preferably 80 to 90°C.

[0039] The reaction time can be 1 to 8 hours, preferably 2 to 6 hours, and more preferably 2 to 4 hours. The reaction time is calculated from the completion of the dropwise addition of the aluminum source slurry.

[0040] The phosphorous acid solution may be first heated to 50 to 140° C., preferably 70 to 110° C., and more preferably 80 to 90° C., and then the aluminum source slurry may be added dropwise thereto.

[0041] Steps for obtaining rare earth-aluminum phosphites

[0042] The rare earth compound slurry is added into the acidic aluminum phosphite slurry to obtain the rare earth-aluminum phosphite.

[0043] The rare earth compound may be selected from one or more of rare earth oxides, rare earth hydroxides, and rare earth carbonates. The rare earth element in the rare earth compound may be selected from one or more of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium, and yttrium. Preferably, the rare earth element in the rare earth compound is selected from one or more of lanthanum and cerium. The rare earth compound may be selected from one or more of lanthanum oxide, lanthanum hydroxide, and lanthanum carbonate. According to one embodiment of the present invention, the rare earth compound is lanthanum oxide.

[0044] The rare earth compound slurry comprises the rare earth compound and water. The mass ratio of the rare earth compound to water may be 1:(0.7-2), preferably 1:(1-1.8), and more preferably 1:(1.3-1.6).

[0045] The rare earth compound and water may be stirred at 50 to 140° C., preferably 70 to 120° C., more preferably 80 to 100° C. for 1 to 6 hours, preferably 2 to 4 hours, to obtain a rare earth compound slurry.

[0046] The rare earth compound slurry can be pumped into the acidic aluminum phosphite slurry. For example, a peristaltic pump is used to pump the rare earth compound slurry into the acidic aluminum phosphite slurry.

[0047] The molar ratio of the rare earth element in the rare earth compound to the phosphorous acid may be (0.2-0.7):2; preferably (0.3-0.6):2; and more preferably (0.32-0.4):2.

[0048] The reaction temperature may be 50 to 140°C; preferably 70 to 120°C; more preferably 80 to 100°C.

[0049] The reaction time may be 1 to 8 hours, preferably 2 to 6 hours, and more preferably 3 to 5 hours.

[0050] The reaction can be carried out under stirring.

[0051] Specifically, the rare earth compound slurry is added to the acidic aluminum phosphite slurry, and then reacted at 50-140° C. for 1-8 hours to obtain a reactant; the reactant is filtered and then dried at 100-150° C. to obtain a rare earth-aluminum phosphite.

[0052] The drying temperature may be 100 to 150° C., preferably 110 to 140° C., and more preferably 120 to 130° C. The drying may be carried out by oven drying, vacuum drying, flash drying, ribbon drying, or the like.

[0053] <Rare earth-aluminum phosphites and their uses>

[0054] The rare earth-aluminum phosphite of the present invention is prepared by the above method and can improve the flame retardant property of polymer.

[0055] Therefore, the present invention also provides the use of the rare earth-aluminum phosphite in improving the flame retardant properties of polymers.

[0056] The polymer may be selected from one or more of nylon, polybutylene terephthalate, polyethylene terephthalate, polyurethane, and acrylonitrile-styrene-butadiene copolymer. Preferably, the polymer is nylon. Nylon may be selected from one or more of PA6, PA66, PA11, and PA12. According to one embodiment of the present invention, nylon is a mixture of PA6 and PA66. The mass ratio of PA6 to PA66 may be 10:(20-60); preferably 10:(30-50); more preferably 10:(35-45).

[0057] <Composition>

[0058] The composition of the present invention comprises the above rare earth-aluminum phosphite and alkyl aluminum phosphinate. The present invention finds that compounding the above rare earth-aluminum phosphite with alkyl aluminum phosphinate has a better flame retardant effect.

[0059] The alkyl phosphinate in the alkyl phosphinate aluminum can be represented by formula (I):

[0060]

[0061] Wherein, R1 and R2 are independently selected from H, C1-C6 alkyl, and at least one of R1 and R2 is not H. Preferably, R1 and R2 are independently selected from C1-C3 alkyl.

[0062] Examples of alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, n-pentyl, isopentyl, neopentyl, n-hexyl, 2-methylpentyl, 3-methylpentyl, 2,3-dimethylbutyl, 2,2-dimethylbutyl.

[0063] According to one embodiment of the present invention, the alkyl aluminum phosphinate is diethyl aluminum phosphinate.

[0064] The amount of rare earth-aluminum phosphite used can be 1 to 6 parts by weight, preferably 2 to 5 parts by weight, more preferably 3 to 4 parts by weight, and most preferably 3 to 3.2 parts by weight.

[0065] The amount of alkyl aluminum phosphinate used may be 8 to 18 parts by weight, preferably 10 to 16 parts by weight, more preferably 12 to 15 parts by weight, and most preferably 12 to 13 parts by weight.

[0066] The composition of the present invention may further include a polymer. In certain embodiments, the composition may further include one or more of an antioxidant, a lubricant, a masterbatch and glass fiber.

[0067] The polymer may be selected from one or more of nylon, polybutylene terephthalate, polyethylene terephthalate, polyurethane, and acrylonitrile-styrene-butadiene copolymer. Preferably, the polymer is nylon. Nylon may be selected from one or more of PA6, PA66, PA11, and PA12. According to one embodiment of the present invention, nylon is a mixture of PA6 and PA66. The mass ratio of PA6 to PA66 may be 10:(20-60); preferably 10:(30-50); more preferably 10:(35-45).

[0068] The amount of the polymer used may be 30 to 70 parts by weight, preferably 40 to 60 parts by weight, more preferably 50 to 55 parts by weight, and more preferably 52 to 53 parts by weight.

[0069] The amount of the antioxidant can be 0.1 to 1.5 parts by weight, preferably 0.3 to 1 parts by weight, and more preferably 0.5 to 0.8 parts by weight. The antioxidant can be a mixture of antioxidant 1098 and antioxidant 608. The mass ratio of antioxidant 1098 to antioxidant 608 can be 2:(1 to 5), and preferably 2:(3 to 4).

[0070] The amount of the lubricant can be 0.1 to 1 part by weight, preferably 0.2 to 0.8 part by weight, and more preferably 0.3 to 0.5 part by weight. The lubricant can be wax powder. According to one embodiment of the present invention, the lubricant is AC540A produced by Honeywell.

[0071] The amount of the masterbatch can be 0.3 to 3 parts by weight, preferably 0.5 to 2 parts by weight, and more preferably 1 to 1.5 parts by weight. A black masterbatch is preferred.

[0072] The amount of glass fiber used may be 10 to 50 parts by weight, preferably 20 to 40 parts by weight, and more preferably 30 to 35 parts by weight.

[0073] The composition of the present invention can be prepared by the following method: extruding the raw material through a twin-screw extruder to obtain a molding material, cooling the molding material, and then granulating to obtain the composition.

[0074] Here are the raw materials:

[0075] The PA6 grade is 2400J and was purchased from Hangzhou Juheshun New Materials Co., Ltd.

[0076] The PA66 grade is EPR24, which was purchased from Pingdingshan Shenma Engineering Plastics Co., Ltd.

[0077] The glass fiber grade is ECS301UW, which was purchased from Chongqing International Composite Materials Co., Ltd.

[0078] Aluminum diethylphosphinate was purchased from Qingdao Oupure New Materials Co., Ltd.

[0079] Aluminum phosphite was purchased from Shenzhen Ruishixing Technology Co., Ltd.

[0080] Lubricant AC540A was purchased from Honeywell.

[0081] The black masterbatch was PA3785, purchased from Cabot Corporation of the United States.

[0082] Here is the test method:

[0083] If the following test methods require processing into test pieces, the composition shall be dried and then processed into test pieces on an injection molding machine at 280°C, unless otherwise specified.

[0084] UL94: HB grade is evaluated by horizontal burning test, and V0-V2 grade is evaluated by 500W (125mm) vertical burning test.

[0085] Notched impact strength: tested using the method specified in ISO 179-1.

[0086] Example 1

[0087] 5.2 kg of aluminum hydroxide and 8.0 kg of water are dispersed into aluminum source slurry. 16.88 kg of phosphorous acid is mixed with 25.32 kg of water to obtain phosphorous acid solution. The phosphorous acid solution is heated to 80°C, and then the aluminum source slurry is added dropwise thereto; after the aluminum source slurry is added dropwise, the reaction is carried out at 80°C for 2 hours to obtain acidic aluminum phosphite slurry.

[0088] 5.61 kg of lanthanum oxide and 8.5 kg of water were stirred at 80°C for 3 hours to obtain a rare earth compound slurry. The rare earth compound slurry was pumped into the acidic aluminum phosphite slurry, and then reacted at 80°C with stirring for 3 hours to obtain a reactant. The reactant was cooled and filtered, and then dried at 120°C to obtain a rare earth-aluminum phosphite.

[0089] Figure 1 and Figure 2 The SEM image of the rare earth-aluminum phosphite obtained in this example is shown in FIG. Figure 1 and Figure 2 It can be seen that the rare earth-aluminum phosphite of this embodiment includes long strip-shaped grains and irregular block-shaped grains; the two types of grains are dispersed or aggregated together.

[0090] According to the TG curve, the thermal weight loss temperature of 1 wt% of the rare earth-aluminum phosphite of this embodiment is 433.7°C.

[0091] Example 2

[0092] 5.0 kg of pseudo-boehmite and 7.25 kg of water are dispersed into aluminum source slurry. 16.88 kg of phosphorous acid is mixed with 25.62 kg of water to obtain phosphorous acid solution. The phosphorous acid solution is heated to 95°C, and then the aluminum source slurry is added dropwise thereto; after the aluminum source slurry is added dropwise, the reaction is carried out at 95°C for 2 hours to obtain acidic aluminum phosphite slurry.

[0093] 5.59 kg of lanthanum oxide and 5.72 kg of water were stirred at 80°C for 3 hours to obtain a rare earth compound slurry. The rare earth compound slurry was pumped into the acidic aluminum phosphite slurry, and reacted at 80°C with stirring for 3 hours to obtain a reactant. The reactant was cooled and filtered, and then dried at 120°C to obtain a rare earth-aluminum phosphite.

[0094] Figure 3 and Figure 4 The SEM image of the rare earth-aluminum phosphite obtained in this example is shown in FIG. Figure 3 and Figure 4 It can be seen that the rare earth-aluminum phosphite of this embodiment includes long strip-shaped grains and irregular block-shaped grains; the two types of grains are dispersed or aggregated together.

[0095] According to the TG curve, the thermal weight loss temperature of 1 wt% of the rare earth-aluminum phosphite of this embodiment is 391.7°C.

[0096] Figure 7 This is the EDS diagram of the rare earth-aluminum phosphite of this embodiment. Figure 7 It can be seen that the deposits grown on the surface of the rare earth diethyl hypophosphite are aluminum-containing compounds, which also contain elements such as phosphorus and oxygen, and can be inferred to be diethyl aluminum hypophosphite.

[0097] Example 3

[0098] 5.3 kg of gibbsite and 7 kg of water were dispersed into aluminum source slurry. 16.88 kg of phosphorous acid was mixed with 22.12 kg of water to obtain phosphorous acid solution. The phosphorous acid solution was heated to 100°C, and then the aluminum source slurry was added dropwise thereto; after the aluminum source slurry was added dropwise, the mixture was reacted at 100°C for 4 hours to obtain acidic aluminum phosphite slurry.

[0099] 8.40 kg of lanthanum oxide and 8.68 kg of water were stirred at 80°C for 3 hours to obtain a rare earth compound slurry. The rare earth compound slurry was pumped into the acidic aluminum phosphite slurry, and reacted at 80°C with stirring for 5 hours to obtain a reactant. The reactant was cooled and filtered, and then dried at 120°C to obtain a rare earth-aluminum phosphite.

[0100] Figure 5 and Figure 6 The SEM image of the rare earth-aluminum phosphite obtained in this example is shown in FIG. Figure 5and Figure 6 It can be seen that the rare earth-aluminum phosphite of this embodiment includes long strip-shaped grains and irregular block-shaped grains; the two types of grains are dispersed or aggregated together.

[0101] According to the TG curve, the thermal weight loss temperature of 1 wt% of the rare earth-aluminum phosphite of this embodiment is 471.7°C.

[0102] Figure 8 The XRD diagram of the rare earth-aluminum phosphite obtained in Example 1-3 is shown in FIG. Figure 8 It can be seen that the diffraction peak positions and peak heights of the rare earth-aluminum phosphites obtained in Examples 1-3 are substantially consistent, and the crystal phase structures of the rare earth-aluminum phosphites obtained in each example are the same.

[0103] Examples 4 to 6 Comparative Examples 1 to 2

[0104] PA66 and PA6 are placed in a twin-screw extruder (model: KTS35 / 44D); aluminum diethylphosphinate, phosphite, 0.2 parts by weight of antioxidant 1098, 0.3 parts by weight of antioxidant 608, 0.3 parts by weight of AC540A and 1 part by weight of black masterbatch are mixed, and then added into the twin-screw extruder from a first side feed port at 260°C; 30 parts by weight of glass fiber are added into the twin-screw extruder through a second side feed port; and the molding material is extruded through the twin-screw extruder to obtain a molding material. The molding material is cooled in a water bath, and then granulated to obtain a composition.

[0105] The types and amounts of some raw materials are shown in Table 1, and the properties of the composition are shown in Table 1.

[0106] Table 1

[0107]

[0108] Note: Each set of UL94 tests is conducted five times. A*X means that the results of grade A are X times out of five tests.

[0109] Corrosion test

[0110] PA66 and PA6 are placed in a twin-screw extruder (model: KTS35 / 44D); a brass block with a mass of m1 is set on the die head of the twin-screw extruder; aluminum diethylphosphinate, phosphite, antioxidant 1098, antioxidant 608, AC540A and black masterbatch are mixed and then added to the twin-screw extruder from the first side feed port at 260°C; glass fiber is added to the twin-screw extruder through the second side feed port; and the molding material is extruded through the twin-screw extruder to obtain the molding material. The molding material is cooled in a water bath and then granulated.

[0111] The total weight of the raw materials (PA66, PA6, aluminum diethylphosphinate, phosphite, antioxidant 1098, antioxidant 608, AC540A, black masterbatch and glass fiber) is 25 kg.

[0112] The mass of the brass block on the die after granulation was measured and recorded as m2. The loss of the brass block was calculated according to the formula (m1-m2) / m1, and the corrosiveness of the composition was judged according to the loss of the brass block.

[0113] The selection and proportion of each raw material are shown in Table 2, and the corrosiveness is shown in Table 2.

[0114] Table 2

[0115]

[0116] It can be seen from Table 1 and Table 2 that the rare earth-aluminum phosphite of the present invention can achieve better flame retardant effect than the compounding of aluminum phosphite and aluminum diethylphosphinate, and can make nylon maintain higher notched impact strength and lower corrosiveness.

[0117] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.

Claims

1. A method for preparing a rare earth-aluminum phosphite, characterized in that: The steps include: (1) adding an aluminum source slurry dropwise to a phosphorous acid solution to obtain an acidic aluminum phosphite slurry; (2) adding the rare earth compound slurry to the acidic aluminum phosphite slurry to obtain rare earth-aluminum phosphite; Wherein, the aluminum source in the aluminum source slurry is selected from one or more of aluminum hydroxide, pseudo-boehmite, gibbsite, and boehmite; The rare earth compound is selected from one or more of rare earth oxides, rare earth hydroxides and rare earth carbonates.

2. The preparation method according to claim 1, characterized in that: The rare earth compound is selected from one or more of lanthanum oxide, lanthanum hydroxide and lanthanum carbonate.

3. The preparation method according to claim 1, characterized in that: In step (1), the reaction temperature is 50-140° C. and the reaction time is 1-8 h; in step (2), the reaction temperature is 50-140° C. and the reaction time is 1-8 h.

4. The preparation method according to claim 1, characterized in that: The mass ratio of the aluminum source to the phosphorous acid is (3.5-6.5):16.88; the molar ratio of the rare earth element in the rare earth compound to the phosphorous acid is (0.2-0.7):

2.

5. The preparation method according to claim 1, characterized in that: Step (2) comprises the following steps: The rare earth compound slurry is added to the acidic aluminum phosphite slurry, and then reacted at 50-140° C. for 1-8 hours to obtain a reactant; the reactant is filtered and then dried at 100-150° C. to obtain a rare earth-aluminum phosphite.

6. The preparation method according to claim 1, characterized in that: In the aluminum source slurry, the mass ratio of the aluminum source to water is (4-6):(6-9); in the phosphorous acid solution, the mass ratio of phosphorous acid to water is 16.88:(20-30); in the rare earth compound slurry, the mass ratio of the rare earth compound to water is 1:(0.7-2).

7. A rare earth-aluminum phosphite, characterized in that: The rare earth-aluminum phosphite is obtained by the preparation method according to any one of claims 1 to 6.

8. Use of the rare earth-aluminum phosphite according to claim 7 in improving the flame retardant properties of polymers.

9. A composition, characterized in that The composition comprises the rare earth-aluminum phosphite of claim 7 and aluminum alkyl phosphinate.

10. The composition according to claim 9, characterized in that The composition further comprises a polymer, and the polymer is selected from one or more of nylon, polybutylene terephthalate, polyethylene terephthalate, polyurethane, and acrylonitrile-styrene-butadiene copolymer.

Citation Information

Patent Citations

  • Rare earth metal hypophosphite and preparation method and application of rare earth metal hypophosphite

    CN102838098A

  • Flame retardant-stabilizer combination for thermoplastic polymers

    CN103154110A

  • Mixtures of aluminium hydrogenphosphites with aluminium salts, process for the production thereof and the use thereof

    CN104114485A

  • Mixtures of aluminium phosphite with sparingly soluble aluminium salts and foreign ions, process for the production thereof and the use thereof

    CN104114486A

  • Halogen-free solid flame retardant mixture and use thereof

    CN105940085A

Cited By

  • Method for preparing high-purity and high-thermal-stability aluminum phosphite through continuous flow

    CN121470444A