Preparation method of H-CoFe-CNT micro-nano composite material and zinc air battery

Through the use of H-CoFe-CNT micro-nano composite materials, the problem of bubble blockage during charging of zinc air batteries is solved, the hydrophobicity and reaction interface of the battery are improved, the discharge performance and stability of zinc air batteries are improved, and the discharge performance and stability of zinc air batteries are improved, and the High peak power density and long-term cycle stability.

CN118993038APending Publication Date: 2024-11-22CHINA THREE GORGES UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410922448.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Traditional rechargeable zinc air batteries are reduced in efficiency due to bubble blocking the contact between catalyst and reactants during charging, and the use of hydrophobic coatings may reduce the specific surface area and active sites, affecting battery performance.

Method used

Using H-CoFe-CNT micro-nano composite material as air electrodes, a dual-function oxygen electrocatalyst with a hollow hydrophobic structure was prepared by CVD pyrolysis, and the hydrophobicity and reactant transport were improved by using the hierarchical structure of carbon nanotubes to form a favorable three-dimensional Phase reaction interface.

Benefits of technology

It improves the discharge performance and cycle stability of zinc air batteries, improves the peak power density and stability, and achieves efficient charging performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993038A_ABST
    Figure CN118993038A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of chargeable and dischargeable zinc air batteries, and particularly relates to an H-CoFe-CNT micro-nano composite material and a preparation method and application thereof on the air cathode side. The preparation method comprises the following steps: by taking cobalt salt, zinc salt, 2-methylimidazole and cetyltrimethylammonium bromide (CTAB) as reaction raw materials, growing at room temperature, etching and adsorbing Fe < 2 + > to obtain a hollow CoFeZn-MOF nano box; then under the assistance of dicyandiamide, the H-CoFe-CNT micro-nano composite material with a 3D micro-nano hierarchical structure, high catalytic activity and relatively good hydrophobicity is obtained. The prepared H-CoFe-CNT composite carbon material is used as a cathode and assembled with a zinc anode to form a liquid zinc-air battery, the liquid zinc-air battery shows an open-circuit voltage of 1.53 V, the discharge peak power density can reach 230 mW / cm < 2 >, and the liquid zinc-air battery can be stably and circularly charged and discharged for more than 2000 hours. The open-circuit voltage of the assembled quasi-solid-state zinc air battery is up to 1.50 V, and the discharge peak power density is up to 610 mWcm < 2 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparation of rechargeable zinc-air batteries, and the air cathode side specifically relates to the technical field of preparation of new energy materials. Background Art

[0002] The rapid development of the global economy and the escalating environmental damage caused by fossil fuels have made it imperative to cope with the tremendous pressure brought about by energy demand. In this context, the advancement of clean energy and energy storage devices is of vital importance. Among the series of technologies being explored, alkaline metal-air batteries have attracted increasing attention due to their high energy density and potential to provide sustainable energy solutions. The anodes of these batteries are composed of various metals such as lithium, sodium, magnesium, aluminum, potassium, zinc, and iron. Rechargeable zinc-air batteries (ZABs) have become attractive energy conversion and storage devices due to their high theoretical energy density, low cost, and good safety. The discharge and charge efficiencies of ZABs are mainly determined by the oxygen reduction reaction (ORR) and oxygen evolution reaction (OER) with electrocatalysts as air electrodes.

[0003] Mass transfer efficiency and promotion of reaction molecule / ion diffusion also play an important role in achieving excellent fast charging ZABs. Since a large amount of O2 is generated during the charging process, bubbles may block the contact between the catalyst and the reactants, so constructing a hydrophobic, oxygen-philic surface of the air electrode is considered to be an effective strategy. The traditional method is to use polytetrafluoroethylene (PTFE) coating to increase the hydrophobic property of the air electrode. However, it may drastically reduce the specific surface area and even block the active sites, thereby affecting the efficiency of the ZAB. Therefore, how to form a favorable three-phase boundary for ZABs by tailoring a suitable catalyst surface without using any hydrophobic coating is crucial to the fast charging performance of ZABs.

[0004] Here, the cathode material in the present invention is intended to prepare an economical and efficient hydrophobic bifunctional electrocatalyst - an efficient bifunctional oxygen electrocatalyst with a hollow hydrophobic structure after CVD pyrolysis. Thanks to the hierarchical structure of the grown carbon nanotubes, the prepared air electrode has a certain hydrophobicity, which helps to form a favorable three-phase reaction interface. The hollow structure further promotes the transport of the reactants, and the two together improve the discharge performance of ZABs. Summary of the invention

[0005] The present invention provides a H-CoFe-CNT micro-nano composite material and a preparation method and application thereof. The material has high bifunctional activity and suitable hydrophobicity, and the assembled liquid and quasi-solid zinc-air batteries have excellent peak power density and good cycle stability.

[0006] In order to achieve the above-mentioned invention object, the present invention adopts the following technical scheme: The specific steps include: a: Preparation of CoZn-MOF nanobox: CoZn-MOF was obtained by aging in a mixed solution consisting of cobalt salt, zinc salt, CTAB aqueous solution and 2-methylimidazole aqueous solution, followed by centrifugal washing and drying; b: Preparation of H-CoZn-MOF hollow nanobox: CoZn-MOF was ultrasonically dispersed in a methanol solution, and then tannic acid was added to the solution. After stirring and centrifugation, the H-CoZn-MOF hollow nanobox was obtained; c: Preparation of H-CoFeZn-MOF hollow nanobox: H-CoZn-MOF was placed in a solution of Fe 2+ Ultrasonic dispersion in ionic methanol solution and stirring and centrifugation were performed to obtain H-CoFeZn-MOF hollow nanoboxes; d: Preparation of H-CoFe-CNT: The H-CoFeZn-MOF hollow nanobox and dicyandiamide were placed in the downstream and upstream of the tube furnace, respectively, and the H-CoFe-CNT micro-nanocomposite material was obtained after annealing in an argon atmosphere.

[0007] Furthermore, in step a, the cobalt salt may be cobalt nitrate, cobalt chloride, or cobalt acetate, the concentration of the aqueous solution thereof is 0.05-0.1 g / L, the concentration of the 2-methylimidazole aqueous solution is 40-60 g / L, and the mixing volume ratio of the cobalt salt aqueous solution and the 2-methylimidazole aqueous solution in the mixed solution is 1 / 1-1 / 3; the stirring time is 0.5-2 h, and the powder is collected by centrifugation.

[0008] Furthermore, in the step b: the concentration of the methanol solution of tannic acid is 3-7 g / L; the stirring time is 5-20 min, and the powder is collected by centrifugation.

[0009] Furthermore, in step c: the iron salt can be ferrous chloride, ferrous sulfate, or ferrous acetate, and the concentration of the solution is 0.8-1.2 g / L; the stirring time is 15-30 min, and the powder is collected by centrifugation.

[0010] Furthermore, in the step d: the H-CoFeZn-MOF hollow nanobox and dicyandiamide are placed in the downstream and upstream of the tube furnace respectively, and calcined in an argon atmosphere, and then the temperature is increased to 800-1000° C. within 2-3 hours and kept warm for 1.5-2 hours, and then cooled naturally.

[0011] The H-CoFe-CNT micro-nano composite carbon material obtained by the above preparation method has oxygen reduction performance and oxygen precipitation performance, and is hydrophobic. The hydrophobic angle is greater than 130°, and more preferably the hydrophobic angle is greater than 150°.

[0012] The present invention also provides a liquid zinc-air battery, which is assembled using H-CoFe-CNT micro-nano composite carbon material as the air cathode side.

[0013] The present invention also provides a quasi-solid-state zinc-air battery, which is assembled using H-CoFe-CNT micro-nano composite carbon material as the air cathode side.

[0014] The solid electrolyte material is one of PVA electrolyte, PaNa electrolyte, biocellulose membrane electrolyte, and acrylic gel electrolyte.

[0015] Compared with the prior art, the present invention has the following beneficial effects: The H-CoFe-CNT three-dimensional micro-nano composite material has a composite structure in which carbon nanotubes are grown in situ in a hollow carbon cage. The product has a uniform morphology. This microstructure has a certain hydrophobicity, which is greater than 130°, preferably greater than 150°. The cobalt-iron alloy particles wrapped in carbon nanotubes have good OER performance, and the iron particles and the carbon layer core-shell structure have excellent ORR performance. The half-wave potential is 0.909V, which is comparable to conventional transition metal single-atom catalysts. This composite material combines the advantages of the three and has high bifunctional activity. Due to the improvement of hydrophobicity, it can be exposed to more air in the electrolyte, which significantly improves its discharge polarization and further improves the power density of ZABs.

[0016] The preparation method of the H-CoFe-CNT three-dimensional micro-nano composite air electrode of the present invention has the advantages of high repeatability, simple synthesis process, and easy control. The prepared H-CoFe-CNT micro-nano composite material has high bifunctional activity, and the liquid ZABs used as cathode assembly show high power density (200mWcm 2 Above), high stability (2000h@5mA / cm 2 Applied to the air electrode of rechargeable quasi-solid-state zinc-air battery with a power density of 600mWcm 2 above. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is the XRD pattern of the product prepared in Example 1-4.

[0018] Figure 2 The following are SEM images and contact angle photographs of the product prepared in Example 1.

[0019] Figure 3 The following are SEM images and contact angle photographs of the product prepared in Example 2.

[0020] Figure 4 The following are SEM images and contact angle photographs of the product prepared in Example 3.

[0021] Figure 5 The following are SEM images and contact angle photographs of the product prepared in Example 3.

[0022] Figure 6 is a TEM image of H-CoFe-CNT prepared in Example 4.

[0023] Figure 7 Graph showing the ORR polarization curves of the ORR / OER bifunctional oxygen electrocatalysts prepared in Examples 1-4 of the present invention.

[0024] Figure 8 Graph showing the OER polarization curves of the ORR / OER bifunctional oxygen electrocatalysts prepared in Examples 1-4 of the present invention.

[0025] Fig. 9 This is a performance diagram of the ORR stability test of the H-CoFe-CNT micro-nano composite material and Pt / C+RuO2 prepared in Example 4.

[0026] Fig.10 This is a comparison of the LSV curves of the H-CoFe-CNT micro-nano composite material prepared in Example 4 and Pt / C+RuO2 before and after the ORR stability test.

[0027] Fig.11 This is an open circuit voltage performance diagram of the bifunctional oxygen electrocatalyst prepared in Example 4 of the present invention used in a liquid zinc-air battery.

[0028] Fig.12 This is a discharge polarization curve of the bifunctional oxygen electrocatalyst prepared in Example 4 of the present invention used in a liquid zinc-air battery.

[0029] Fig.13 This is a test chart of the charge and discharge cycle stability of the bifunctional oxygen electrocatalyst prepared in Example 4 for liquid zinc-air batteries.

[0030] Fig.14 This is an open circuit voltage diagram of the bifunctional oxygen electrocatalyst prepared in Example 4 used in a quasi-solid-state zinc-air battery.

[0031] Fig.15 This is a discharge polarization curve of the bifunctional oxygen electrocatalyst prepared in Example 4 of the present invention used in a liquid zinc-air battery.

[0032] Fig.16 This is a photo of the bifunctional oxygen electrocatalyst prepared in Example 4 of the present invention being used in a quasi-solid-state zinc-air battery to drive a small fan. DETAILED DESCRIPTION

[0033] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0034] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0035] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.

[0036] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0037] Example 1 (a) Preparation of CoZn-MOF 30 mg of cobalt nitrate (Co(NO3)2·6H2O), 1.5 g of zinc nitrate hexahydrate (Zn(NO3)2·6H2O) and 15 mg of CTAB were dissolved in 100 mL of deionized water, mixed with 300 mL of deionized water dissolved with 22.7 g of 2-methylimidazole (2-MIM), aged at room temperature for 30 min, and the purple solution was rinsed several times by centrifugation with deionized water and methanol at 6500 rpm and dried at 80°C for 12 h.

[0038] (b) Preparation of H-CoZn-MOF The prepared CoZn-MOF was dispersed in a methanol solution, tannic acid (concentration of 5 mg / ml) was added, stirred for 10 min, centrifuged to collect the powder, and dried at 80°C for 12 h.

[0039] (c) Preparation of H-Co-C The prepared purple powder of H-CoZn-MOF is placed downstream of the corundum boat and dicyandiamide is placed upstream. The corundum boat is placed in a tubular furnace for calcination. The calcination atmosphere is argon, the calcination temperature is 800-1000°C, the heating time is 2-3h, and the insulation time is 1.5-2h. After the tubular furnace is cooled naturally, the H-Co-C material is obtained.

[0040] Example 2 (a) Preparation of CoZn-MOF 30 mg of cobalt nitrate (Co(NO3)2·6H2O), 1.5 g of zinc nitrate hexahydrate (Zn(NO3)2·6H2O) and 15 mg of CTAB were dissolved in 100 mL of deionized water, mixed with 300 mL of deionized water dissolved with 22.7 g of 2-methylimidazole (2-MIM), aged at room temperature for 30 min, and the purple solution was rinsed several times by centrifugation with deionized water and methanol at 6500 rpm and dried at 80°C for 12 h.

[0041] (b) Preparation of H-CoZn-MOF The prepared CoZn-MOF was dispersed in a methanol solution, tannic acid (concentration of 5 mg / ml) was added, stirred for 10 min, centrifuged to collect the powder, and dried at 80°C for 12 h.

[0042] (c) Preparation of H-CoFeZn-MOF The prepared H-CoZn-MOF was dispersed in methanol solution and Fe 2+ (concentration is 1 mg / ml), stir for 20 min, collect the powder by centrifugation, and dry at 80°C for 12 h.

[0043] (d) Preparation of H-CoFe The prepared H-CoFeZn-MOF is placed in a tubular furnace for calcination. The calcination atmosphere is argon, the calcination temperature is 800-1000°C, the heating time is 2-3h, the insulation time is 1.5-2h, and after the tubular furnace is cooled naturally, the H-CoFe material is obtained.

[0044] Example 3 (a) Preparation of CoZn-MOF 30 mg of cobalt nitrate (Co(NO3)2·6H2O), 1.5 g of zinc nitrate hexahydrate (Zn(NO3)2·6H2O) and 15 mg of CTAB were dissolved in 100 mL of deionized water, mixed with 300 mL of deionized water dissolved with 22.7 g of 2-methylimidazole (2-MIM), aged at room temperature for 30 min, and the purple solution was rinsed several times by centrifugation with deionized water and methanol at 6500 rpm and dried at 80°C for 12 h.

[0045] (b) Preparation of CoFeZn-MOF The prepared CoZn-MOF was dispersed in methanol solution and Fe 2+ (concentration is 1 mg / ml), stir for 20 min, collect the powder by centrifugation, and dry at 80°C for 12 h.

[0046] (c) Preparation of CoFe-CNT The prepared CoFeZn-MOF is placed downstream of the corundum boat and dicyandiamide is placed upstream. The corundum boat is placed in a tubular furnace for calcination. The calcination atmosphere is argon, the calcination temperature is 800-1000°C, the heating time is 2-3h, the insulation time is 1.5-2h, and after the tubular furnace is cooled naturally, the CoFe-CNT material is obtained.

[0047] Example 4 (a) Preparation of CoZn-MOF 30 mg of cobalt nitrate (Co(NO3)2·6H2O), 1.5 g of zinc nitrate hexahydrate (Zn(NO3)2·6H2O) and 15 mg of CTAB were dissolved in 100 mL of deionized water, mixed with 300 mL of deionized water dissolved with 22.7 g of 2-methylimidazole (2-MIM), aged at room temperature for 30 min, and the purple solution was rinsed several times by centrifugation with deionized water and methanol at 6500 rpm and dried at 80°C for 12 h.

[0048] (b) Preparation of H-CoZn-MOF The prepared CoZn-MOF was dispersed in a methanol solution, tannic acid (concentration of 5 mg / ml) was added, stirred for 10 min, centrifuged to collect the powder, and dried at 80°C for 12 h.

[0049] (c) Preparation of H-CoFeZn-MOF The prepared H-CoFeZn-MOF was dispersed in methanol solution and Fe 2+ (concentration is 1 mg / ml), stir for 20 min, collect the powder by centrifugation, and dry at 80°C for 12 h.

[0050] (d) Preparation of H-CoFe-CNT The prepared H-CoFeZn-MOF is placed downstream of the corundum boat and dicyandiamide is placed upstream. The corundum boat is placed in a tubular furnace for calcination. The calcination atmosphere is argon, the calcination temperature is 800-1000°C, the heating time is 2-3h, the insulation time is 1.5-2h, and after the tubular furnace is cooled naturally, the H-CoFe-CNT material is obtained.

[0051] The prepared bifunctional oxygen electrocatalyst was subjected to scanning electron microscopy analysis, contact angle test, X-ray diffraction analysis, transmission electron microscopy analysis, ORR, OER, ORR stability test, liquid zinc-air battery open circuit voltage test, liquid zinc-air battery discharge polarization performance test, liquid zinc-air battery charge and discharge cycle stability test, quasi-solid-state zinc-air battery open circuit voltage test, quasi-solid-state zinc-air battery discharge polarization performance test, quasi-solid-state zinc-air battery charge and discharge cycle stability test, and the results are as follows: Figure 1-Figure 16 shown.

[0052] X-ray diffraction results ( Figure 1 ) shows that the physical phase in Example 1 is metallic cobalt. When the iron element is introduced, the physical phase of Example 4 is transformed into metallic iron and cobalt-iron alloy (Co3Fe7). SEM images show that Example 1 presents a regular hexahedral structure with a size of about 400nm, and a contact angle of 134° with deionized water. Example 4 presents a hierarchical structure of epitaxially grown carbon nanotubes on a cubic structure, and the corresponding contact angle increases to 151°, creating favorable conditions for providing a three-phase reaction interface. As a comparison, Examples 2 and 3 respectively show that the introduction of dicyandiamide-assisted thermal decomposition and the formation of cobalt-iron alloys both promote the growth of carbon nanotubes to a certain extent, and also increase the contact angle of the material with deionized water to a certain extent. Figure 6 It shows that the interior of Example 4 is hollow, and carbon nanotubes grow both inside and outside the carbon cage, which is beneficial to the transmission and diffusion of the reaction substances.

[0053] Figure 7 It shows that the H-CoFe-CNT prepared in Example 4 has an excellent half-wave potential (0.909 V), which is slightly higher than Pt / C (0.88 V) and is comparable to conventional Fe-NC catalysts. Figure 9-10 The ORR stability of Example 4 was further tested. After 7200s of chronoamperometry test, the current retention rate was 95%, and the oxygen reduction LSV decay was significantly smaller than that of Pt / C. Figure 8 It shows that the bifunctional catalyst H-CoFe-CNT also has good OER activity.

[0054] Figure 11-13 The results show that after the bifunctional oxygen electrocatalyst prepared in Example 4 is used as the positive electrode material to assemble a liquid zinc-air battery, the open circuit voltage is 1.53 V and the peak power density can reach 255 mW / cm 2 , the assembled liquid zinc-air battery operated stably for more than 2,000 hours.

[0055] Figure 14-16 The results show that after the bifunctional oxygen electrocatalyst prepared in Example 4 was used as the positive electrode material to assemble a quasi-solid-state zinc-air battery, the open circuit voltage was 1.50 V and the peak power density was as high as 610 mW / cm 2 .

[0056] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for a person skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to replace some of the technical features therein by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions claimed to be protected by the present invention.

Claims

1. A method for preparing a H-CoFe-CNT micro-nano composite material, characterized in that: The following steps are involved: (a) Preparation of CoZn-MOF nanobox: The CoZn-MOF nanobox was aged in a mixed solution of cobalt salt, zinc salt, CTAB aqueous solution and 2-methylimidazole aqueous solution, and then centrifuged, washed and dried to obtain the CoZn-MOF nanobox; (b) Preparation of H-CoZn-MOF hollow nanoboxes: CoZn-MOF was ultrasonically dispersed in a methanol solution, and then tannic acid was added to the solution. After stirring and centrifugation, H-CoZn-MOF hollow nanoboxes were obtained. (c) Preparation of H-CoFeZn-MOF hollow nanobox: H-CoZn-MOF was ultrasonically dispersed in a methanol solution containing iron salt, and then stirred and centrifuged to obtain the H-CoFe-MOF hollow nanobox; (d) Preparation of H-CoFe-CNT: The H-CoFeZn-MOF hollow nanobox and dicyandiamide were placed in the downstream and upstream of the tube furnace respectively, and the H-CoFe-CNT micro-nano composite carbon material was obtained after annealing in an argon atmosphere.

2. The method for preparing the H-CoFe-CNT micro-nano composite material according to claim 1, characterized in that: In the step (a), the cobalt salt is cobalt nitrate, cobalt chloride, or cobalt acetate, the concentration of the cobalt salt aqueous solution is 0.05 to 0.1 g / L, the concentration of the 2-methylimidazole aqueous solution is 40 to 60 g / L, and the mixing volume ratio of the cobalt salt aqueous solution to the 2-methylimidazole aqueous solution in the mixed solution is 1 / 1 to 1 / 3.

3. The method for preparing the H-CoFe-CNT micro-nano composite carbon material according to claim 1, characterized in that: In the step (b), the concentration of the methanol solution of tannic acid is 3-7 g / L.

4. The method for preparing the H-CoFe-CNT micro-nano composite carbon material according to claim 1, characterized in that: In the step (c), the iron salt may be ferrous chloride, ferrous sulfate, or ferrous acetate, and the concentration of the solution thereof is 0.8-1.2 g / L.

5. The method for preparing the H-CoFe-CNT micro-nano composite carbon material according to claim 1, characterized in that: The step (d) specifically includes: placing the H-CoFeZn-MOF hollow nanobox and dicyandiamide in the downstream and upstream of a tube furnace respectively, placing them in an argon atmosphere for calcination, then raising the temperature to 800-1000° C. within 2-3 hours and keeping the temperature for 1.5-2 hours, and naturally cooling down to obtain an H-CoFe-CNT micro-nano composite carbon material.

6. The H-CoFe-CNT micro-nano composite carbon material prepared by the preparation method according to any one of claims 1 to 5, characterized in that: The H-CoFe-CNT micro-nano composite material has oxygen reduction performance and oxygen precipitation performance, and is hydrophobic. The hydrophobic angle is greater than 130°, and more preferably the hydrophobic angle is greater than 150°.

7. A liquid zinc-air battery, characterized in that: The H-CoFe-CNT micro-nano composite carbon material prepared by the preparation method according to any one of claims 1 to 5 is assembled as the air cathode side.

8. A quasi-solid-state zinc-air battery, characterized in that: The H-CoFe-CNT micro-nano composite carbon material prepared by the preparation method according to any one of claims 1 to 5 is assembled as the air cathode side.

9. The quasi-solid-state zinc-air battery according to claim 8, characterized in that: The solid electrolyte material is one of PVA electrolyte, PaNa electrolyte, biocellulose membrane electrolyte, and acrylic gel electrolyte.

Citation Information

Cited By

  • Preparation method and application of flexible self-supporting cobalt-nitrogen-carbon composite catalyst

    CN119695179A

  • Preparation method and application of a flexible self-supporting cobalt-nitrogen-carbon composite catalyst

    CN119695179B