A preparation method and application of alginate-based high entropy metal oxide

Alginate-based high-entropy metal oxide electrocatalyst is prepared by chelating sodium alginate with transition metal ions and reacting low-temperature hydrothermal heat, which solves the problems of high cost of precious metal oxides and poor stability of traditional materials, and achieves high catalytic activity and Stability, suitable for large-scale industrial applications.

CN115928134BActive Publication Date: 2024-12-06QINGDAO UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211418410.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-14
Publication Date
2024-12-06
Estimated Expiration
2042-11-14

AI Technical Summary

Technical Problem

In the prior art, the high cost and resource scarcity of precious metal oxide catalysts hinder large-scale industrial applications, and traditional electrocatalytic materials are prone to agglomeration and dissolution under long-term use, and their service life is limited.

Method used

Alginate-based high-entropy metal oxide electrocatalyst is prepared under low temperature conditions by chelating sodium alginate with transition metal ions through hydrothermal reaction and tube furnace carbonization method, forming nanosphere morphology and combining carbon materials to improve Specific capacity and stability.

Benefits of technology

The prepared alginate-based high-entropy metal oxide has high catalytic activity and good stability, which is better than commercial Ir/C and RuO2 catalysts, and exhibits high overpotential properties under alkaline conditions, is cheap and has rich raw materials. Suitable for large-scale development and utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115928134B_ABST
    Figure CN115928134B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of an alginate-based high-entropy metal oxide. The invention uses sodium alginate, which is abundant in source, as a raw material, chelates transition metal ions, and adopts two methods, hydrothermal reaction and tubular furnace carbonization, to prepare an alginate-based high-entropy metal oxide electrocatalyst with high OER catalytic activity under low temperature conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of water electrolysis, and in particular to a preparation method of an alginate-based high-entropy metal oxide and an application thereof. Background Art

[0002] With the rapid development of society and the sharp increase in population, the demand for energy is increasing day by day. Human beings continue to exploit and consume fossil energy, leading to serious environmental problems and energy crises. In order to reduce the use of fossil fuels and achieve sustainable development, on the one hand, we should develop and utilize renewable clean energy, such as solar energy, wind energy, hydropower, geothermal energy and tidal energy. On the other hand, we should develop clean and environmentally friendly new energy storage and conversion technologies, such as water electrolysis and fuel cells. Hydrogen, as a renewable energy source, has the characteristics of zero carbon emissions, high calorific value, easy storage and transportation, and abundant resources. The only product after hydrogen combustion is water, which will not cause any pollution to the environment. Therefore, hydrogen energy is recognized as a new energy that can replace traditional fossil fuels and is one of the candidates for the next generation of clean energy. The main sources of hydrogen are coal, oil and natural gas, but the preparation of hydrogen energy through these fossil fuels will produce a large amount of CO2 emissions, causing a greenhouse effect. Electrochemical water decomposition is an effective hydrogen production process with a simple process, high hydrogen yield and no harmful byproducts, which has attracted more and more attention. In industrial production, the most commonly used are noble metal oxide catalysts such as RuO2 and IrO2, but their high cost and resource scarcity seriously hinder large-scale industrial applications. Therefore, it is crucial to develop anode oxygen evolution catalyst materials that are abundant in resources, low in price, simple in preparation process, excellent in catalytic performance and good in stability. In comparison, transition metal oxides are considered to be the most likely materials to replace noble metal electrocatalysts today because of their wide sources, low prices and good OER catalytic performance.

[0003] High entropy oxides are a new type of oxide system that has just been developed in recent years. They have broken through the design concept of traditional doped oxides and have attracted widespread attention from the scientific community due to their unique properties. Due to the synergistic effect of various metal and non-metal elements, there are many components and the components are arranged in a chaotic manner, which makes it easy to form a single-phase solid solution structure. Therefore, they usually show better application performance than traditional metal oxides, such as high strength, high toughness, good high / low temperature performance, good electrical properties, etc. In particular, they have great application prospects in energy preparation and storage and electrocatalytic materials.

[0004] Carbon materials have the advantages of ultra-high specific surface area, good conductivity and outstanding stability, but the specific capacitance of carbon materials is generally poor. Metal oxides theoretically have better specific capacitance, but they will agglomerate and dissolve after working for a long time, and their service life is limited. Summary of the invention

[0005] In view of the problems existing in the above-mentioned prior art, the present invention provides a method for preparing an alginate-based high-entropy metal oxide and its application, using abundant sodium alginate as a raw material, chelating transition metal ions, and applying hydrothermal reaction and tubular furnace carbonization methods under low temperature conditions to prepare an alginate-based high-entropy metal oxide electrocatalyst with high OER catalytic activity.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A low-temperature preparation method of an alginate-based high-entropy metal oxide comprises the following steps:

[0008] 1) taking solid sodium alginate, adding water and stirring to obtain a sodium alginate solution, weighing at least three metal sources, adding water and stirring to prepare a metal salt solution;

[0009] 2) adding the sodium alginate solution dropwise into the metal salt solution, soaking and chelating to obtain a small spherical gel;

[0010] 3) placing the spherical gel in a high pressure reactor at 160-240° C. for 12 hours, washing, and freeze-drying the product to obtain a high entropy metal oxide;

[0011] The metal source includes iron salt, cobalt salt, nickel salt, zinc salt, copper salt, manganese salt, titanium salt and chromium salt.

[0012] Preferably, the step 3) can also be: washing the spherical gel, freeze-drying it, and placing it in a tubular furnace for 12 hours at 160-240° C. to obtain a high entropy metal oxide.

[0013] Preferably, the sodium alginate solution in step 1) is 1 wt %.

[0014] Preferably, in step 1), the metal sources are iron nitrate, cobalt nitrate and nickel nitrate respectively.

[0015] Preferably, the total amount of metal added to the metal salt solution in step 1) is 0.5M.

[0016] Preferably, the molar ratio of Fe, Co and Ni in the metal salt solution is 1:1:1.

[0017] Preferably, in step 2), the volume ratio of the sodium alginate solution to the metal salt solution is 3:5, and the soaking and chelating time is 4 hours.

[0018] Preferably, the freeze drying in step 3) is performed by freezing with liquid nitrogen and placing the mixture in a freeze dryer for 48 hours.

[0019] In addition, the present application also provides an application of an alginate-based high entropy metal oxide prepared by the above method as an electrocatalyst in water electrolysis.

[0020] The beneficial effects of the present invention are as follows:

[0021] 1. The present invention combines carbon materials with metal oxides, chelates sodium alginate with metal ions, fully reacts in a high-pressure reactor, and then freeze-dries to obtain nano-spherical morphology. The obtained alginate-based high-entropy metal oxide has both high specific capacity and stability, and high catalytic activity of OER performance under alkaline electrolyte. The raw materials used in the present invention are mainly sodium alginate, which has a wide range of sources, is green and environmentally friendly, and has high safety. The metal source is a transition metal, a non-precious metal, and is cheap. The resulting final product, a high-entropy metal oxide, has a low price, high catalytic activity, and good stability.

[0022] 2. The method of the present invention adjusts the metal doping ratio of different components to achieve excellent OER performance under alkaline conditions with a current density of 10 mA cm -2 When the overpotential of the alginate-based high entropy iron-cobalt-nickel oxide electrocatalyst produced by hydrothermal reaction under alkaline conditions is 329 mV, the overpotential of the alginate-based high entropy iron-cobalt-nickel oxide electrocatalyst produced by low-temperature carbonization in a tubular furnace under alkaline conditions is 231 mV, which is better than commercial Ir / C and RuO2 catalysts.

[0023] 3. The alginate-based high entropy metal oxide electrocatalyst prepared by the method of the present invention can be used as an excellent water electrolysis catalyst with high catalytic activity and good stability.

[0024] 4. The alginate-based high-entropy metal oxide electrocatalyst prepared by the method of the present invention has a simple operation process, does not require high-temperature annealing, has a high yield, has abundant raw material reserves and low prices, and can be developed and utilized on a large scale. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a scanning electron microscope image of the alginate-based high entropy iron-cobalt-nickel oxide obtained in Example 1;

[0026] Figure 2 is a scanning electron microscope image of the alginate-based high entropy iron-cobalt-nickel oxide obtained in Example 4;

[0027] Figure 3 is a transmission electron microscopy image of the alginate-based high entropy iron-cobalt-nickel oxide obtained in Example 1;

[0028] Figure 4 is a transmission electron micrograph of the alginate-based high entropy iron-cobalt-nickel oxide obtained in Example 4;

[0029] Figure 5is the XRD spectra of the alginate-based high entropy metal oxides obtained in Examples 2, 3, and 4;

[0030] Figure 6 It is the alkaline OER linear scanning curve of the products of Example 1 and Comparative Examples 1 and 2 and commercial Ir / C and RuO2 measured by an electrochemical workstation;

[0031] Figure 7 It is the alkaline OER linear scan curve of the products of Example 4 and Comparative Examples 3 and 4 and commercial Ir / C and RuO2 measured using an electrochemical workstation. DETAILED DESCRIPTION

[0032] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention is clearly and completely described below in conjunction with the accompanying drawings of the present invention. Based on the embodiments in this application, other similar embodiments obtained by ordinary technicians in this field without making any creative work should all fall within the scope of protection of this application.

[0033] Example 1

[0034] 1) 1.2 g of sodium alginate was placed in 120 ml of secondary water and stirred thoroughly to obtain a 1 wt% sodium alginate solution. A certain amount of ferric nitrate, cobalt nitrate and nickel nitrate were weighed to prepare salt solutions, placed in 200 ml of secondary water and stirred thoroughly to obtain 0.5 M ferric nitrate, cobalt nitrate and nickel nitrate salt solutions (ferric nitrate: cobalt nitrate: nickel nitrate is 1:1:1).

[0035] 2) Add the prepared sodium alginate solution dropwise into the mixed solution of ferric nitrate, cobalt nitrate and nickel nitrate, and soak and chelate for 4 hours to obtain a small spherical gel.

[0036] 3) After the gel is soaked, the spherical gel is filtered out and fully washed with secondary water. The spherical gel is placed in a 100 ml high-pressure reactor, and 50 ml of secondary water is injected for hydrothermal reaction at 180° C. for 12 hours.

[0037] 4) washing the product in the high-pressure reactor with deionized water and ethanol to remove excess impurities, freezing the product at -18°C for 12 hours, and then drying it in a freeze dryer to obtain the final product, alginate-based high-entropy iron cobalt nickel oxide (FeCoNi / C).

[0038] The final product, alginate-based high entropy iron cobalt nickel oxide FeCoNi / C nanoparticles, obtained above was used as a water electrolysis catalyst for electrochemical testing using an electrochemical workstation.

[0039] Example 2

[0040] 1) 1.2 g of sodium alginate was placed in 120 ml of secondary water and stirred thoroughly to obtain a 1 wt% sodium alginate solution. A certain amount of ferric nitrate, zinc nitrate, manganese nitrate and titanium nitrate were weighed to prepare salt solutions, placed in 200 ml of secondary water and stirred thoroughly to obtain 0.5 M ferric nitrate, zinc nitrate, manganese nitrate and titanium nitrate salt solutions (ferric nitrate: zinc nitrate: manganese nitrate: titanium nitrate is 1:1:1:1).

[0041] 2) Add the prepared sodium alginate solution dropwise into the mixed solution of iron nitrate, zinc nitrate, manganese nitrate and titanium nitrate, and soak and chelate for 4 hours to obtain a small spherical gel.

[0042] 3) After the gel is soaked, the spherical gel is filtered out and fully washed with secondary water. The spherical gel is placed in a 100 ml high-pressure reactor, and 50 ml of secondary water is injected for hydrothermal reaction at 160° C. for 12 hours.

[0043] 4) washing the product in the autoclave with deionized water and ethanol to remove excess impurities, freezing the product at -18°C for 12 hours, and then drying it in a freeze dryer to obtain the final product, alginate-based high-entropy iron zinc manganese titanium oxide (FeZnMnTi / C).

[0044] The final product, alginate-based high entropy iron zinc manganese titanium oxide FeZnMnTi / C nanoparticles obtained above, was used as a water electrolysis catalyst for electrochemical testing using an electrochemical workstation.

[0045] Example 3

[0046] 1) Place 1.2 g of sodium alginate in 120 ml of secondary water and stir thoroughly to obtain a 1 wt% sodium alginate solution. Weigh a certain amount of ferric nitrate, cobalt nitrate, and chromium nitrate to prepare a salt solution, place it in 200 ml of secondary water and stir thoroughly to obtain a 0.5 M ferric nitrate, cobalt nitrate, and chromium nitrate salt solution (ferric nitrate: cobalt nitrate: chromium nitrate is 3:2:1).

[0047] 2) Add the prepared sodium alginate solution dropwise into the mixed solution of ferric nitrate, cobalt nitrate and chromium nitrate, and soak and chelate for 4 hours to obtain a small spherical gel.

[0048] 3) After the gel is soaked, the spherical gel is filtered out and fully washed with secondary water. The spherical gel is placed in a 100 ml high-pressure reactor, and 50 ml of secondary water is injected for hydrothermal reaction at 240° C. for 12 hours.

[0049] 4) washing the product in the autoclave with deionized water and ethanol to remove excess impurities, freezing the product at -18°C for 12 hours, and then drying it in a freeze dryer to obtain the final product, alginate-based high-entropy iron cobalt chromium oxide (FeCoCr / C).

[0050] The final product, alginate-based high-entropy iron cobalt chromium oxide FeCoCr / C nanoparticles, was used as a water electrolysis catalyst for electrochemical testing using an electrochemical workstation.

[0051] Example 4

[0052] 1) 1.2 g of sodium alginate was placed in 120 ml of secondary water and stirred thoroughly to obtain a 1 wt% sodium alginate solution. A certain amount of ferric nitrate, cobalt nitrate and nickel nitrate were weighed to prepare salt solutions, placed in 200 ml of secondary water and stirred thoroughly to obtain a 0.5 M mixed solution of ferric nitrate, cobalt nitrate and nickel nitrate (ferric nitrate: cobalt nitrate: nickel nitrate is 1:1:1).

[0053] 2) Add the prepared sodium alginate solution dropwise into the mixed solution of ferric nitrate, cobalt nitrate and nickel nitrate, and soak and chelate for 4 hours to obtain a small spherical gel.

[0054] 3) The spherical gel was filtered out, washed thoroughly with deionized water to remove excess water, and then the spherical gel was rapidly frozen with liquid nitrogen and placed in a freeze dryer for 48 hours.

[0055] 4) placing the product of step 3) in a tube furnace, and low-temperature carbonizing in air at 180° C. for 12 hours at a heating rate of 5° C. per minute to obtain the final product, alginate-based high-entropy iron-cobalt-nickel oxide (FeCoNi / C).

[0056] The final product, alginate-based high entropy iron cobalt nickel oxide FeCoNi / C nanoparticles, obtained above was used as a water electrolysis catalyst for electrochemical testing using an electrochemical workstation.

[0057] Comparative Example 1

[0058] 1.2 g of sodium alginate was placed in 120 ml of secondary water and stirred thoroughly to obtain a 1 wt% sodium alginate solution. A certain amount of ferric nitrate was weighed to prepare a salt solution, placed in 200 ml of secondary water and stirred thoroughly to obtain a 0.5 M ferric nitrate salt solution.

[0059] The prepared sodium alginate solution is added dropwise into the ferric nitrate solution, and small spherical gel is obtained by soaking and chelating.

[0060] After the gel was soaked for 4 hours, the spherical gel was filtered out and washed thoroughly with secondary water. The spherical gel was placed in a 100 ml high-pressure reactor, injected with 50 ml of secondary water, and subjected to hydrothermal reaction at 180 degrees Celsius for 12 hours.

[0061] The product in the reactor was washed with deionized water and ethanol to remove excess impurities, and the product was frozen at -18 degrees Celsius for 12 hours and then dried in a freeze dryer to obtain the final product, alginate-based iron oxide (Fe / C).

[0062] The final product, alginate-based iron oxide Fe / C nanoparticles, obtained above was used as a water electrolysis catalyst for electrochemical testing using an electrochemical workstation.

[0063] Comparative Example 2

[0064] Place 1.2 g of sodium alginate in 120 ml of secondary water and stir thoroughly to obtain a 1 wt% sodium alginate solution. Weigh a certain amount of ferric nitrate and cobalt nitrate to prepare a salt solution, place it in 200 ml of secondary water and stir thoroughly to obtain a 0.5 M ferric nitrate and cobalt nitrate salt solution (ferric nitrate: cobalt nitrate is 1:1).

[0065] The prepared sodium alginate solution is added dropwise into the mixed solution of ferric nitrate and cobalt nitrate, and the small spherical gel is obtained by soaking and chelating.

[0066] After the gel was soaked for 4 hours, the spherical gel was filtered out and washed thoroughly with secondary water. The spherical gel was placed in a 100 ml high-pressure reactor, injected with 50 ml of secondary water, and subjected to hydrothermal reaction at 180 degrees Celsius for 12 hours.

[0067] The product in the reactor was washed with deionized water and ethanol to remove excess impurities, and the product was frozen at -18 degrees Celsius for 12 hours and then dried in a freeze dryer to obtain the final product, alginate-based iron cobalt oxide (FeCo / C).

[0068] The final product, alginate-based iron cobalt oxide FeCo / C nanoparticles, obtained above was used as a water electrolysis catalyst for electrochemical testing using an electrochemical workstation.

[0069] Comparative Example 3

[0070] 1.2 g of sodium alginate was placed in 120 ml of secondary water and stirred thoroughly to obtain a 1 wt% sodium alginate solution. A certain amount of ferric nitrate was weighed to prepare a salt solution, placed in 200 ml of secondary water and stirred thoroughly to obtain a 0.5 M ferric nitrate salt solution.

[0071] The prepared sodium alginate solution is added dropwise into the ferric nitrate solution, and small spherical gel is obtained by soaking and chelating.

[0072] The spherical gel was filtered out, washed thoroughly with deionized water to remove excess water, and then the spherical gel was rapidly frozen with liquid nitrogen and placed in a freeze dryer for 48 hours.

[0073] The product was placed in a tube furnace and carbonized in air at low temperature at 180°C for 12 hours with a heating rate of 5°C per minute to obtain the final product, alginate-based high entropy iron oxide (Fe / C).

[0074] The final product, alginate-based iron cobalt oxide Fe / C nanoparticles, obtained above was used as a water electrolysis catalyst for electrochemical testing using an electrochemical workstation.

[0075] Comparative Example 4

[0076] Place 1.2 g of sodium alginate in 120 ml of secondary water and stir thoroughly to obtain a 1 wt% sodium alginate solution. Weigh a certain amount of ferric nitrate and cobalt nitrate to prepare a salt solution, place it in 200 ml of secondary water and stir thoroughly to obtain a 0.5 M ferric nitrate and cobalt nitrate salt solution (ferric nitrate: cobalt nitrate is 1:1).

[0077] The prepared sodium alginate solution is added dropwise into the mixed solution of ferric nitrate and cobalt nitrate, and the small spherical gel is obtained by soaking and chelating.

[0078] The spherical gel was filtered out, washed thoroughly with deionized water to remove excess water, and then the spherical gel was rapidly frozen with liquid nitrogen and placed in a freeze dryer for 48 hours.

[0079] The product was placed in a tube furnace and carbonized in air at low temperature at 180°C for 12 hours with a heating rate of 5°C per minute to obtain the final product, alginate-based high entropy iron cobalt oxide (FeCo / C).

[0080] The final product, alginate-based iron cobalt oxide FeCo / C nanoparticles, obtained above was used as a water electrolysis catalyst for electrochemical testing using an electrochemical workstation.

[0081] Figure 1 This is a scanning electron microscope image of the alginate-based high entropy iron-cobalt-nickel oxide obtained in Example 1. It can be clearly seen that the alginate-based high entropy iron-cobalt-nickel oxide has a nanoparticle morphology, is relatively evenly dispersed, and has a particle size of less than 100 nanometers.

[0082] Figure 2 This is a scanning electron microscope image of the alginate-based high-entropy iron-cobalt-nickel oxide obtained in Example 4. It can be clearly seen that its morphology is nanosheets, which is significantly different from the morphology of Example 1. The dispersion is relatively uniform, and some nanosheets are stacked into a block structure.

[0083] Figure 3 This is a transmission electron microscope image of the alginate-based high-entropy iron-cobalt-nickel oxide obtained in Example 1, which is a high-resolution TEM image (HRTEM). Metal nanoparticles (lattice fringe spacing of 0.20 nm) can be clearly observed, with relatively continuous lattice fringes and a carbon layer coated at the boundary.

[0084] Figure 4It is a transmission electron microscope image of the alginate-based high entropy iron cobalt nickel oxide obtained in Example 4, which is a high-resolution TEM image (HRTEM). Metal nanoparticles (lattice fringe spacing of 0.26nm) can be clearly observed. The discontinuity of the lattice fringes is due to the fact that the alginate-based high entropy iron cobalt nickel oxide produced in Example 4 has an ultrafine lattice structure, and some lattice disordered areas are caused by the stacking of ultrafine lattice structures, and no carbon layer is seen at the boundary.

[0085] Figure 5 It is the XRD spectrum of the alginate-based high entropy metal oxide obtained in Examples 2, 3, and 4. The main diffraction peaks can correspond well to the crystal planes of spinel (111), (220), (331), and (222), which are consistent with the stoichiometric ratios of elements such as Fe, Co, and Ni.

[0086] Figure 6 The alkaline OER linear scan curves of the product of Example 1, the products of Comparative Examples 1 and 2, and commercial Ir / C and RuO2 measured using an electrochemical workstation. The current density is 10 mA cm -2 When the overpotential of the alginate-based high entropy iron-cobalt-nickel oxide electrocatalyst produced by hydrothermal reaction under alkaline conditions is 329 mV. Under the same conditions, the overpotential of the commercial Ir / C catalyst is 468 mV, and the overpotential of the commercial RuO2 catalyst is 497 mV, which is better than the commercial Ir / C and RuO2 catalysts.

[0087] Figure 7 The alkaline OER linear scan curves of the product of Example 4, the products of Comparative Examples 3 and 4, and commercial Ir / C and RuO2 measured by an electrochemical workstation. The current density is 10 mA cm -2 When the overpotential of the alginate-based high entropy iron-cobalt-nickel oxide electrocatalyst produced by low-temperature carbonization in a tubular furnace under alkaline conditions was 231 mV. Under the same conditions, the overpotential of the commercial Ir / C catalyst was 468 mV, and the overpotential of the commercial RuO2 catalyst was 497 mV, which was better than that of the commercial Ir / C and RuO2 catalysts.

[0088] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A low-temperature preparation method of alginate-based high-entropy metal oxide, characterized in that: Here are the steps: 1) 1.2 g of sodium alginate was placed in 120 ml of secondary water and stirred thoroughly to obtain a 1 wt% sodium alginate solution, and a certain amount of iron nitrate, cobalt nitrate, and nickel nitrate were weighed to prepare salt solutions, placed in 200 ml of secondary water, and stirred thoroughly to obtain a 0.5 M mixed solution of iron nitrate, cobalt nitrate, and nickel nitrate, wherein the molar ratio of Fe, Co, and Ni is 1:1:1; 2) adding the prepared sodium alginate solution dropwise into the mixed solution of iron nitrate, cobalt nitrate and nickel nitrate, and soaking and chelating for 4 hours to obtain a small spherical gel; 3) Filter out the spherical gel, wash it thoroughly with deionized water to remove excess water, and then quickly freeze the spherical gel with liquid nitrogen and place it in a freeze dryer for 48 hours; 4) placing the product of step 3) in a tubular furnace, low-temperature carbonizing in air, treating at 180° C. for 12 hours at a heating rate of 5° C. per minute, to obtain alginate-based high-entropy iron-cobalt-nickel oxide.

Citation Information

Patent Citations

  • Biomass carbon / ferrocobalt dual-metal-oxide double-functional oxide catalyst as well as preparation method and application thereof

    CN105609795A