Preparation method of manganous-manganic oxide for positive electrode material of lithium ion battery

By generating a nickel-cobalt-manganese hydroxide coating layer on the surface of manganese tetroxide, forming core-shell structured manganese tetroxide particles, the problem of high compaction density and cycle performance that existing preparation methods cannot meet for lithium-ion battery cathode materials is solved, and the structural stability and electrochemical performance of the material are improved.

CN118993153APending Publication Date: 2024-11-22GUANGXI MANGANESE NEW ENERGY TECH DEV CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411201462.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing methods for preparing manganese tetroxide cannot meet the requirements for high compaction density and cycle performance of lithium-ion battery cathode materials. Traditional methods suffer from problems such as high cost, low purity, high impurities, and poor physical properties.

Method used

Manganese tetroxide slurry was prepared by co-precipitation and a nickel cobalt manganese hydroxide coating layer was formed on its surface to form core-shell structured manganese tetroxide particles. When used as a manganese source to prepare lithium manganese oxide, the nickel cobalt manganese hydroxide coating on the surface improves the structural stability and electrochemical performance of the material.

Benefits of technology

Significantly improved the compaction density and cycle performance of lithium-ion battery cathode materials, the ternary material of nickel-cobalt-manganese oxide increased the specific capacity, suppressed the contact between lithium manganese oxide and electrolyte, and improved the electrochemical performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993153A_ABST
    Figure CN118993153A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of manganous-manganic oxide for a positive electrode material of a lithium ion battery, and belongs to the field of preparation of manganous-manganic oxide. The preparation method comprises the following steps: (1) taking manganese sulfate, sodium hydroxide and EDTA (Ethylene Diamine Tetraacetic Acid) as raw materials, and preparing manganous-manganic oxide slurry by adopting a coprecipitation method; (2) preparing cobalt salt, manganese salt and nickel salt into a nickel-cobalt-manganese mixed salt solution by using water; (3) taking the manganous-manganic oxide slurry as a base solution, transferring the manganous-manganic oxide slurry into a reaction kettle, stirring, simultaneously pumping the nickel-cobalt-manganese mixed salt solution, a sodium hydroxide aqueous solution and ammonia water into the reaction kettle in a parallel flow feeding manner, stirring for reaction, standing after reaction, and separating to obtain a precipitate; and (4) washing and drying the precipitate to obtain the manganous-manganic oxide for the positive electrode material of the lithium ion battery. When the prepared manganous-manganic oxide is used for preparing the lithium ion battery positive electrode material, the compaction density, the specific capacity and the cycle performance of the positive electrode material can be remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of trimanganese tetraoxide preparation, and in particular to a method for preparing trimanganese tetraoxide for positive electrode materials of lithium ion batteries. Background Art

[0002] Manganese tetraoxide is also known as black manganese ore in nature. Its theoretical manganese content is 72.03%. It is mainly used as a basic raw material in industries such as electronic products and new energy power batteries. Manganese tetraoxide products can be divided into electronic grade and battery grade. Electronic grade manganese tetraoxide is a key raw material for the production of manganese-zinc ferrite, which is mainly used in transformers, filters, inductors and other products; battery grade manganese tetraoxide is mainly used in lithium battery manganese positive electrode materials, including lithium manganate, lithium iron manganese phosphate and sodium ion battery layered oxides.

[0003] In recent years, with the development of green industries such as new energy vehicles, lithium manganate, as a positive electrode material for power lithium-ion batteries, has attracted more and more attention due to its advantages such as low price, good safety performance and no pollution to the environment. The traditional method for producing lithium manganate is mainly the high-temperature solid phase method. This method uses electrolytic manganese dioxide as a manganese source, adds lithium carbonate and corresponding additives, and is made by solid phase sintering. However, the battery materials prepared by lithium manganate produced by this method have problems such as low gram capacity, poor cycle performance, and poor high temperature performance. Studies have shown that compared with manganese dioxide, lithium manganate prepared using spherical manganese tetraoxide as raw material has better performance. Both manganese tetraoxide and lithium manganate have spinel structures. When lithium manganate is prepared with manganese tetraoxide, no drastic structural changes will occur, and the material structure is more stable; the prepared lithium manganate has better electrochemical properties, and the gram capacity, high temperature performance, and cycle performance have been significantly improved: Therefore, using manganese tetraoxide instead of electrolytic manganese dioxide to produce lithium manganate is the current development trend.

[0004] At present, the preparation methods of manganese tetraoxide mainly include metal manganese method, manganese salt method, roasting method, etc. In China, manganese tetraoxide is mostly prepared by metal manganese powder suspension oxidation method. This process is relatively mature, but the production cost is high. The manganese salt method mainly uses manganese sulfate and manganese chloride as raw materials, and reacts with alkaline solution under certain conditions to finally prepare manganese tetraoxide products; the raw materials of this method are cheap and easy to operate, but the subsequent lithium manganate products have low compaction density and poor cycle performance. The roasting method mainly uses manganese carbonate as raw material, and roasts at 850-1100℃ to obtain manganese tetraoxide; this method has strict process requirements, and after high-temperature roasting, manganese tetraoxide has the disadvantages of high impurities, low purity and poor physical properties. There is no public report that related companies use this method to produce and sell manganese tetraoxide. In recent years, the battery industry has put forward higher requirements for the product quality of manganese tetraoxide, and the manganese tetraoxide produced by the above commonly used preparation methods can no longer meet the relevant requirements. Summary of the invention

[0005] The purpose of the present invention is to solve the above-mentioned problems existing in the prior art and to provide a method for preparing manganese tetraoxide for positive electrode materials of lithium ion batteries. The manganese tetraoxide prepared by the present invention is used to prepare positive electrode materials of lithium ion batteries, which can significantly improve the compaction density, specific capacity and cycle performance of the positive electrode materials.

[0006] In order to achieve the above object, the technical solution of the present invention is as follows:

[0007] A method for preparing manganese tetraoxide for lithium ion battery positive electrode material comprises the following steps:

[0008] (1) using manganese sulfate, sodium hydroxide and EDTA as raw materials, and adopting a coprecipitation method to prepare a manganese tetraoxide slurry, wherein the manganese tetraoxide slurry contains manganese tetraoxide particles, and the D50 of the manganese tetraoxide particles is 5-15 μm;

[0009] (2) preparing a nickel-cobalt-manganese mixed salt solution with water, wherein the cobalt ion concentration of the nickel-cobalt-manganese mixed salt solution is 0.3-0.8 mol / L, the manganese ion concentration of the nickel-cobalt-manganese mixed salt solution is 0.5-1.5 mol / L, and the nickel ion concentration of the nickel-cobalt-manganese mixed salt solution is 0.5-1.5 mol / L; preparing a sodium hydroxide aqueous solution with a concentration of 100-250 g / L;

[0010] (3) transferring the manganese tetraoxide slurry as the base liquid into a reactor and stirring, pumping a nickel-cobalt-manganese mixed salt solution, a sodium hydroxide aqueous solution, and ammonia water into the reactor in a parallel feeding manner and stirring for reaction, wherein the total mass of the pumped nickel-cobalt-manganese ions, the mass of the sodium hydroxide, and the mass of the ammonia water are in a ratio of 0.2-1.0:1-2:0.01-0.05, and during the stirring reaction, a nickel-cobalt-manganese hydroxide coating layer is gradually generated on the outer surface of the manganese tetraoxide particles, and after 1-10 hours of feeding, the mixture is allowed to stand for 5-15 hours, and a precipitate is separated;

[0011] (4) Washing and drying the precipitate to obtain manganese tetraoxide for positive electrode material of lithium ion battery.

[0012] Furthermore, the step (1) specifically comprises the following steps: dissolving manganese sulfate in deionized water to prepare a manganese sulfate solution with a divalent manganese ion concentration of 60-90 g / L; dissolving sodium hydroxide in deionized water to prepare a sodium hydroxide solution with a concentration of 120-130 g / L, adding EDTA to the sodium hydroxide solution to form a complex precipitant, wherein the concentration of EDTA in the complex precipitant is 1-10 g / L; adding deionized water as a base liquid to the reactor, heating to 50-80 ℃, then stir at a speed of 200-300r / min and introduce air, and continuously drop the reaction materials, manganese sulfate solution and complex precipitant, into the reactor at a molar ratio of manganese ion to sodium hydroxide of 0.3-0.5:1 for precipitation reaction, and the reaction conditions are controlled as follows: reaction temperature is 50-80℃, reaction pH is 8-10, and stirring speed is 200-300r / min. After the reaction materials are added dropwise, the above reaction conditions are continued to stir and react for 1-2h to obtain manganese tetraoxide slurry.

[0013] Furthermore, in step (2), the cobalt salt is one or more of cobalt sulfate, cobalt nitrate, cobalt carbonate, and cobalt chloride; the manganese salt is one or more of manganese sulfate, manganese nitrate, manganese carbonate, and manganese chloride; and the nickel salt is one or more of nickel sulfate, nickel nitrate, and nickel chloride.

[0014] Furthermore, in step (3), the reaction conditions are as follows: the stirring speed is 1000-2000 r / min, the reaction temperature is controlled at 40-60° C., and the pH is adjusted at 7.5-10.0.

[0015] Furthermore, in step (3), after the nickel-cobalt-manganese hydroxide coating layer added to the trimanganese tetraoxide particles has a thickness of 1.0-3.0 μm, the mixture is allowed to stand and separated to obtain a precipitate.

[0016] The present invention also provides application of manganese tetraoxide prepared by the preparation method in lithium ion batteries, wherein the manganese tetraoxide is used as a manganese source to prepare a positive electrode material for a lithium ion battery, specifically, the manganese tetraoxide is mixed with a lithium source, calcined, ground, and sieved to obtain the positive electrode material for a lithium ion battery; the molar ratio of lithium in the lithium source to the total molar ratio of nickel, cobalt, and manganese in the manganese tetraoxide is 0.60-0.75:1; and the lithium source is one or a combination of two or more of lithium nitrate, lithium hydroxide, lithium carbonate, and lithium oxalate.

[0017] The beneficial effects of the present invention are as follows:

[0018] The compaction density of lithium manganate prepared by using spherical manganese tetraoxide produced by the metal manganese method and the manganese salt method as the manganese source is generally low. First, this is because the particle size distribution of spherical manganese tetraoxide is relatively concentrated. Since the lithium manganate product basically inherits the particle size characteristics of the manganese source, the particle size distribution of the prepared lithium manganate is also too concentrated; another important reason is that the primary grains of the lithium manganate product are octahedral structures. In the battery manufacturing process, the positive electrode material needs to be coated on the pole piece and rolled. The octahedral cone grains of lithium manganate will cause great damage to the pole piece, resulting in a low compaction density. The present invention first uses a precipitation method to prepare the manganese tetraoxide kernel, and by controlling the raw material feeding amount, reaction temperature, reaction pH value, stirring speed, etc., a certain thickness of nickel-cobalt-manganese hydroxide is generated on the surface of the manganese tetraoxide to form a core-shell structure manganese tetraoxide. When the core-shell structured manganese tetraoxide is used as a manganese source to prepare lithium manganate, the nickel-cobalt-manganese hydroxide coated on the surface will generate a nickel-cobalt-manganese-lithium ternary material. Since the primary grains of the nickel-cobalt-manganese-lithium ternary material are relatively round, the damage to the pole piece is small, thereby effectively improving the compaction density. In addition, the nickel-cobalt-manganese-lithium ternary material generated on the surface isolates the contact between the lithium manganate and the electrolyte, inhibits the disproportionation reaction of trivalent manganese and the Jan-Taylor effect, thereby effectively improving the cycle performance of the prepared lithium-ion battery positive electrode material. At the same time, since the nickel-cobalt-manganese-lithium ternary material has a high specific capacity, the nickel-cobalt-manganese-lithium ternary material generated on the surface can also improve the specific capacity of the prepared lithium-ion battery positive electrode material as a whole.

[0019] The compaction density of lithium manganese oxide, a positive electrode material of lithium ion battery prepared from manganese tetraoxide prepared by the present invention, reaches 3.0g / cm 3 The 1C discharge capacity of the prepared battery can reach more than 130 mAh / g, and the 100-week cycle retention rate can reach more than 95%. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a SEM image of the lithium-ion battery positive electrode material made of manganese tetraoxide prepared in Example 1;

[0021] Figure 2 This is a SEM image of the lithium-ion battery positive electrode material made of manganese tetraoxide prepared in Comparative Example 1. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0023] Example 1

[0024] A method for preparing manganese tetraoxide for lithium ion battery positive electrode material comprises the following steps:

[0025] (1) Manganese sulfate, sodium hydroxide and EDTA are used as raw materials to prepare manganese tetraoxide slurry by coprecipitation method. The specific operation is as follows: manganese sulfate is dissolved in deionized water to prepare a manganese sulfate solution with a divalent manganese ion concentration of 85 g / L; sodium hydroxide is dissolved in deionized water to prepare a sodium hydroxide solution with a concentration of 125 g / L, EDTA is added to the sodium hydroxide solution to form a complex precipitant, and the concentration of EDTA in the complex precipitant is 5 g / L; deionized water is added to the reactor as a base liquid, heated to 70°C and then heated at 250r. / min, stirring and introducing air, continuously dropping the reaction materials manganese sulfate solution and complex precipitant into the reactor at a molar ratio of manganese ion to sodium hydroxide of 0.4:1 for precipitation reaction, and controlling the reaction conditions as follows: reaction temperature of 70°C, reaction pH of 9, stirring speed of 250r / min, and continuing to stir and react under the above reaction conditions for 1.5h after the dropwise addition of the reaction materials, to obtain manganese tetraoxide slurry, wherein the manganese tetraoxide slurry contains manganese tetraoxide particles, and the D50 of the manganese tetraoxide particles is 7.5μm;

[0026] (2) preparing a nickel-cobalt-manganese mixed salt solution with cobalt sulfate, manganese sulfate and nickel sulfate using water, wherein the cobalt ion concentration of the nickel-cobalt-manganese mixed salt solution is 0.58 mol / L, the manganese ion concentration of the nickel-cobalt-manganese mixed salt solution is 0.8 mol / L, and the nickel ion concentration of the nickel-cobalt-manganese mixed salt solution is 1 mol / L; preparing a sodium hydroxide aqueous solution with a concentration of 180 g / L;

[0027] (3) The manganese tetraoxide slurry is transferred into the reactor as the base liquid and stirred, and the nickel-cobalt-manganese mixed salt solution, sodium hydroxide aqueous solution and ammonia water are simultaneously pumped into the reactor in a parallel feeding manner and stirred for reaction. The total mass of the nickel-cobalt-manganese ions pumped in, the mass of the sodium hydroxide, and the mass of the ammonia water are in a ratio of 0.5:1.2:0.03. During the stirring reaction, the reaction conditions are as follows: the stirring speed is 1500 r / min, the reaction temperature is controlled at 50°C, the pH is adjusted to 8.0, and a nickel-cobalt-manganese hydroxide coating layer is gradually generated on the outer surface of the manganese tetraoxide particles. After 4 hours of feeding, the nickel-cobalt-manganese hydroxide coating layer of the manganese tetraoxide particles is 2.3 μm thick. After standing for 10 hours, a precipitate is separated.

[0028] (4) Washing and drying the precipitate to obtain manganese tetraoxide for positive electrode material of lithium ion battery.

[0029] Example 2

[0030] A method for preparing manganese tetraoxide for lithium ion battery positive electrode material comprises the following steps:

[0031] (1) Manganese sulfate, sodium hydroxide and EDTA are used as raw materials to prepare manganese tetraoxide slurry by coprecipitation method. The specific operation is as follows: manganese sulfate is dissolved in deionized water to prepare a manganese sulfate solution with a divalent manganese ion concentration of 70 g / L; sodium hydroxide is dissolved in deionized water to prepare a sodium hydroxide solution with a concentration of 120 g / L, EDTA is added to the sodium hydroxide solution to form a complex precipitant, and the concentration of EDTA in the complex precipitant is 3 g / L; deionized water is added to the reactor as the base liquid, heated to 60°C and then heated at 300°C. r / min and stirred and air was introduced, and the reaction materials manganese sulfate solution and complex precipitant were continuously dripped into the reactor at a molar ratio of manganese ion to sodium hydroxide of 0.3:1 for precipitation reaction, and the reaction conditions were controlled as follows: reaction temperature was 60°C, reaction pH was 8, and stirring speed was 300r / min. After the reaction materials were dripped, the above reaction conditions were continued to stir and react for 2h to obtain manganese tetraoxide slurry, and the obtained manganese tetraoxide slurry contained manganese tetraoxide particles, and the D50 of the manganese tetraoxide particles was 8.4μm;

[0032] (2) preparing a nickel-cobalt-manganese mixed salt solution with cobalt nitrate, manganese sulfate and nickel nitrate using water, wherein the cobalt ion concentration of the nickel-cobalt-manganese mixed salt solution is 0.4 mol / L, the manganese ion concentration of the nickel-cobalt-manganese mixed salt solution is 0.6 mol / L, and the nickel ion concentration of the nickel-cobalt-manganese mixed salt solution is 0.8 mol / L; preparing a sodium hydroxide aqueous solution with a concentration of 250 g / L;

[0033] (3) The manganese tetraoxide slurry is transferred into a reactor as the base liquid and stirred, and the nickel-cobalt-manganese mixed salt solution, sodium hydroxide aqueous solution and ammonia water are simultaneously pumped into the reactor in a parallel feeding manner and stirred for reaction, and the total mass ratio of the pumped nickel-cobalt-manganese ions, the mass of sodium hydroxide and the mass of ammonia water is 0.2:1:0.01. During the stirring reaction, the reaction conditions are as follows: the stirring speed is 1000 r / min, the reaction temperature is controlled at 60°C, the pH is adjusted to 7.5, and a nickel-cobalt-manganese hydroxide coating layer is gradually generated on the outer surface of the manganese tetraoxide particles. After the nickel-cobalt-manganese hydroxide coating layer of the manganese tetraoxide particles is added to a thickness of 1.8 μm, it is allowed to stand for 5 hours and a precipitate is separated.

[0034] (4) Washing and drying the precipitate to obtain manganese tetraoxide for positive electrode material of lithium ion battery.

[0035] Example 3

[0036] A method for preparing manganese tetraoxide for lithium ion battery positive electrode material comprises the following steps:

[0037] (1) Manganese sulfate, sodium hydroxide and EDTA are used as raw materials to prepare manganese tetraoxide slurry by coprecipitation method. The specific operation is as follows: manganese sulfate is dissolved in deionized water to prepare a manganese sulfate solution with a divalent manganese ion concentration of 90 g / L; sodium hydroxide is dissolved in deionized water to prepare a sodium hydroxide solution with a concentration of 130 g / L, EDTA is added to the sodium hydroxide solution to form a complex precipitant, and the concentration of EDTA in the complex precipitant is 7 g / L; deionized water is added to the reactor as a base liquid, heated to 80°C and then heated at 200°C. r / min, stirring and introducing air, and continuously dropping the reaction materials, manganese sulfate solution and complex precipitant, into the reactor at a molar ratio of manganese ion to sodium hydroxide of 0.5:1 for precipitation reaction, and the reaction conditions are controlled as follows: reaction temperature is 80°C, reaction pH is 10, and stirring speed is 200r / min. After the reaction materials are added dropwise, the above reaction conditions are maintained for stirring and reaction for 1h to obtain manganese tetraoxide slurry, wherein the manganese tetraoxide slurry contains manganese tetraoxide particles, and the D50 of the manganese tetraoxide particles is 10μm;

[0038] (2) preparing a nickel-cobalt-manganese mixed salt solution with water, wherein the cobalt ion concentration of the nickel-cobalt-manganese mixed salt solution is 0.6 mol / L, the manganese ion concentration of the nickel-cobalt-manganese mixed salt solution is 1.2 mol / L, and the nickel ion concentration of the nickel-cobalt-manganese mixed salt solution is 1.5 mol / L; preparing a sodium hydroxide aqueous solution with a concentration of 100 g / L;

[0039] (3) The manganese tetraoxide slurry is transferred into a reactor as the base liquid and stirred, and the nickel-cobalt-manganese mixed salt solution, sodium hydroxide aqueous solution and ammonia water are simultaneously pumped into the reactor in a parallel feeding manner and stirred for reaction, and the total mass ratio of the pumped nickel-cobalt-manganese ions, the mass of sodium hydroxide and the mass of ammonia water is 1.0:2:0.05. During the stirring reaction, the reaction conditions are as follows: the stirring speed is 2000 r / min, the reaction temperature is controlled at 40°C, the pH is adjusted to 9.0, and a nickel-cobalt-manganese hydroxide coating layer is gradually generated on the outer surface of the manganese tetraoxide particles. After the nickel-cobalt-manganese hydroxide coating layer of the manganese tetraoxide particles is added to a thickness of 2.6 μm, it is allowed to stand for 15 hours and a precipitate is separated.

[0040] (4) Washing and drying the precipitate to obtain manganese tetraoxide for positive electrode material of lithium ion battery.

[0041] Comparative Example 1

[0042] A method for preparing manganese tetraoxide comprises the following steps:

[0043] Manganese sulfate is dissolved in deionized water to prepare a manganese sulfate solution with a divalent manganese ion concentration of 85 g / L; sodium hydroxide is dissolved in deionized water to prepare a sodium hydroxide solution with a concentration of 125 g / L, EDTA is added to the sodium hydroxide solution to form a complex precipitant, and the concentration of EDTA in the complex precipitant is 5 g / L; deionized water is added to the reactor as a base liquid, and the reaction kettle is heated to 70°C, stirred at a speed of 250 r / min, and air is introduced, and the reaction materials manganese sulfate solution and the complex precipitant are mixed according to the manganese ion concentration. The molar ratio of sodium hydroxide to sodium hydroxide is 0.4:1 and is continuously dripped into the reactor for precipitation reaction. The reaction conditions are controlled as follows: the reaction temperature is 70°C, the reaction pH is 9, and the stirring speed is 250r / min. After the reaction materials are added dropwise, the above reaction conditions are continued to stir and react for 1.5h to obtain manganese tetraoxide slurry. The obtained manganese tetraoxide slurry contains manganese tetraoxide particles, and the D50 of the manganese tetraoxide particles is 7.5μm. After standing for 30min, it is filtered, and the precipitate is washed and dried to obtain manganese tetraoxide.

[0044] Comparative Example 2

[0045] A method for preparing manganese tetraoxide comprises the following steps:

[0046] (1) Manganese sulfate, sodium hydroxide and EDTA are used as raw materials to prepare manganese tetraoxide slurry by coprecipitation method. The specific operation is as follows: manganese sulfate is dissolved in deionized water to prepare a manganese sulfate solution with a divalent manganese ion concentration of 85 g / L; sodium hydroxide is dissolved in deionized water to prepare a sodium hydroxide solution with a concentration of 125 g / L, EDTA is added to the sodium hydroxide solution to form a complex precipitant, and the concentration of EDTA in the complex precipitant is 5 g / L; deionized water is added to the reactor as a base liquid, heated to 70°C and then heated at 250r. / min, stirring and introducing air, continuously dropping the reaction materials manganese sulfate solution and complex precipitant into the reactor at a molar ratio of manganese ion to sodium hydroxide of 0.4:1 for precipitation reaction, and controlling the reaction conditions as follows: reaction temperature of 70°C, reaction pH of 9, stirring speed of 250r / min, and continuing to stir and react under the above reaction conditions for 1.5h after the dropwise addition of the reaction materials, to obtain manganese tetraoxide slurry, wherein the manganese tetraoxide slurry contains manganese tetraoxide particles, and the D50 of the manganese tetraoxide particles is 7.5μm;

[0047] (2) preparing a nickel-cobalt-manganese mixed salt solution with cobalt sulfate, manganese sulfate and nickel sulfate using water, wherein the cobalt ion concentration of the nickel-cobalt-manganese mixed salt solution is 0.58 mol / L, the manganese ion concentration of the nickel-cobalt-manganese mixed salt solution is 0.8 mol / L, and the nickel ion concentration of the nickel-cobalt-manganese mixed salt solution is 1 mol / L; preparing a sodium hydroxide aqueous solution with a concentration of 180 g / L;

[0048] (3) The manganese tetraoxide slurry is transferred into a reactor as the base liquid and stirred, and the nickel-cobalt-manganese mixed salt solution, sodium hydroxide aqueous solution and ammonia water are simultaneously pumped into the reactor in a parallel feeding manner and stirred for reaction, and the total mass ratio of the pumped nickel-cobalt-manganese ions, the mass of sodium hydroxide and the mass of ammonia water is 0.5:1.2:0.03. During the stirring reaction, the reaction conditions are as follows: the stirring speed is 1500 r / min, the reaction temperature is controlled at 50°C, the pH is adjusted to 8.0, and a nickel-cobalt-manganese hydroxide coating layer is gradually generated on the outer surface of the manganese tetraoxide particles. When the nickel-cobalt-manganese hydroxide coating layer of the manganese tetraoxide particles is 0.6 μm, the reaction is stopped and the mixture is allowed to stand for 10 hours to separate and obtain a precipitate.

[0049] (4) Washing and drying the precipitate to obtain manganese tetraoxide for positive electrode material of lithium ion battery.

[0050] Application Examples

[0051] The manganese tetraoxide prepared in Examples 1-3 and Comparative Examples 1-2 was made into lithium ion battery positive electrode materials and lithium ion batteries according to the following process and their performance was tested.

[0052] The manganese tetraoxide prepared in each group was mixed with lithium carbonate, the total molar ratio of lithium in the lithium carbonate to nickel, cobalt and manganese in the manganese tetraoxide was 0.7:1, and the mixture was evenly mixed by a ball mill at a speed of 1500r / min, forward rotation for 0.5h, and reverse rotation for 0.5h, and then placed in a tube furnace, and heated to 600°C and kept warm for 4h under an oxygen atmosphere at a flow rate of 60mL / min, and then heated to 900°C and kept warm for 10h, with a heating rate of 5°C / min, and then naturally cooled to room temperature with the furnace temperature, and the sintered material was taken out and ground and passed through a 200-mesh sieve to obtain a positive electrode material for a lithium-ion battery. The obtained positive electrode material for a lithium-ion battery was tested, and the test results of D50, coating thickness and compaction density are shown in Table 1, and the above results are all averaged.

[0053] like Figure 1 As shown, it is a SEM image of the lithium-ion battery positive electrode material made of manganese tetraoxide prepared in Example 1. It can be seen from the figure that the primary grains on the surface of the particles are relatively round, which can effectively improve the compaction density.

[0054] like Figure 2 As shown, it is a SEM image of the lithium-ion battery positive electrode material made of manganese tetraoxide prepared in Comparative Example 1. It can be seen from the figure that the primary grains on the surface of the particles are octahedral cones, resulting in a low compaction density.

[0055] Weigh the positive electrode materials of lithium-ion batteries made of manganese tetraoxide, acetylene black and PVDF binder in a mass ratio of 8:1:1. First, dissolve the PVDF powder with N-methylpyrrolidone to make a binder with a mass concentration of 5%. Then, add the positive electrode materials of lithium-ion batteries and acetylene black to the binder and grind them evenly. Then, apply them on aluminum foil, put them in a vacuum oven to dry, and cut them into discs with a diameter of 10 mm with a slicer. Press them to get the positive electrode sheets. With metal lithium sheet as the negative electrode, Celgard2320 as the diaphragm, and 1 mol / L LiPF6 / ethylene carbonate + dimethyl carbonate (volume ratio 1:1) as the electrolyte, CR2032 button-type simulated batteries were assembled in a glove box filled with argon. After the assembled CR2032 type simulated battery was left at room temperature for 6 hours, it was tested in the charge and discharge voltage range of 3.0-4.2V. It was first activated at a rate of 0.1C for three cycles, and then the rate was increased to 1C for 100 constant current charge and discharge cycles. The test results are shown in Table 1.

[0056] Table 1

[0057]

[0058] From the data in Table 1, it can be seen that the compacted density of the lithium manganate material prepared from the manganese tetraoxide of Examples 1-3 is 3.0 g / cm 3 As described above, the compaction density is high and it is more suitable for preparing lithium-ion batteries; however, since the manganese tetraoxide in Comparative Examples 1 and 2 is not coated with nickel-cobalt-manganese hydroxide or the coating thickness is not appropriate, the compaction density of the prepared lithium manganate material is greatly reduced, and the performance of the lithium battery prepared by using it as the positive electrode material is significantly reduced.

[0059] The lithium ion battery prepared by the trimanganese tetraoxide prepared by Examples 1-3 of the present invention has significantly improved 1C discharge specific capacity and 100 cycle retention rate compared with the lithium ion battery prepared by the trimanganese tetraoxide of Comparative Examples 1-2. The present invention prepares trimanganese tetraoxide of a certain particle size first, and then coats the surface of the trimanganese tetraoxide with a layer of nickel, cobalt and manganese hydroxide of a suitable thickness, and the prepared trimanganese tetraoxide is applied to a lithium battery, which can effectively improve the specific capacity and cycle performance of the lithium ion battery.

[0060] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art may make some modifications and improvements without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be based on the definition of the claims.

Claims

1. A method for preparing manganese tetraoxide for positive electrode material of lithium ion battery, It is characterized in that The steps include: (1) using manganese sulfate, sodium hydroxide and EDTA as raw materials, and adopting a coprecipitation method to prepare a manganese tetraoxide slurry, wherein the manganese tetraoxide slurry contains manganese tetraoxide particles, and the D50 of the manganese tetraoxide particles is 5-15 μm; (2) preparing a nickel-cobalt-manganese mixed salt solution with water, wherein the cobalt ion concentration of the nickel-cobalt-manganese mixed salt solution is 0.3-0.8 mol / L, the manganese ion concentration of the nickel-cobalt-manganese mixed salt solution is 0.5-1.5 mol / L, and the nickel ion concentration of the nickel-cobalt-manganese mixed salt solution is 0.5-1.5 mol / L; preparing a sodium hydroxide aqueous solution with a concentration of 100-250 g / L; (3) transferring the manganese tetraoxide slurry as the base liquid into a reactor and stirring, pumping a nickel-cobalt-manganese mixed salt solution, a sodium hydroxide aqueous solution, and ammonia water into the reactor in a parallel feeding manner and stirring for reaction, wherein the total mass of the pumped nickel-cobalt-manganese ions, the mass of the sodium hydroxide, and the mass of the ammonia water are in a ratio of 0.2-1.0:1-2:0.01-0.05, and during the stirring reaction, a nickel-cobalt-manganese hydroxide coating layer is gradually generated on the outer surface of the manganese tetraoxide particles, and after 1-10 hours of feeding, the mixture is allowed to stand for 5-15 hours, and a precipitate is separated; (4) Washing and drying the precipitate to obtain manganese tetraoxide for positive electrode material of lithium ion battery.

2. A method for preparing manganese tetraoxide for positive electrode material of lithium ion battery according to claim 1, It is characterized in that The step (1) specifically comprises the following steps: dissolving manganese sulfate in deionized water to prepare a manganese sulfate solution with a divalent manganese ion concentration of 60-90 g / L; dissolving sodium hydroxide in deionized water to prepare a sodium hydroxide solution with a concentration of 120-130 g / L, adding EDTA to the sodium hydroxide solution and mixing to form a complex precipitant, wherein the concentration of EDTA in the complex precipitant is 1-10 g / L; adding deionized water as a base liquid to a reactor, heating to 50-80° C., stirring at a speed of 200-300 r / min and introducing air, and continuously dripping the reaction materials, the manganese sulfate solution and the complex precipitant, into the reactor at a molar ratio of manganese ions to sodium hydroxide of 0.3-0.5:1 to carry out precipitation reaction, wherein the reaction conditions are controlled as follows: the reaction temperature is 50-80° C., the reaction pH is 8-10, and the stirring speed is 200-300 r / min. After the dropwise addition of the reaction materials is completed, the above reaction conditions are continued to be stirred for 1-2 hours to obtain manganese tetraoxide slurry.

3. The method for preparing manganese tetraoxide for positive electrode material of lithium ion battery according to claim 1, Features: In step (2), the cobalt salt is one or more of cobalt sulfate, cobalt nitrate, cobalt carbonate, and cobalt chloride; the manganese salt is one or more of manganese sulfate, manganese nitrate, manganese carbonate, and manganese chloride; and the nickel salt is one or more of nickel sulfate, nickel nitrate, and nickel chloride.

4. The method for preparing manganese tetraoxide for positive electrode material of lithium ion battery according to claim 1, Features: In step (3), the reaction conditions are as follows: the stirring speed is 1000-2000 r / min, the reaction temperature is controlled at 40-60° C., and the pH is adjusted at 7.5-10.

0.

5. The method for preparing manganese tetraoxide for positive electrode material of lithium ion battery according to claim 1, Features: In step (3), after the nickel-cobalt-manganese hydroxide coating layer of the manganese tetraoxide particles is added to a thickness of 1.0-3.0 μm, the mixture is allowed to stand for 5-15 hours and a precipitate is obtained by separation.

6. Application of trimanganese tetraoxide prepared by the method for preparing trimanganese tetraoxide for a positive electrode material of a lithium ion battery according to any one of claims 1 to 5 in lithium ion batteries, Features: The trimanganese tetraoxide is used as a manganese source to prepare a positive electrode material for a lithium ion battery. Specifically, the trimanganese tetraoxide is mixed with a lithium source, calcined, ground, and sieved to obtain the positive electrode material for a lithium ion battery; the molar ratio of lithium in the lithium source to the total molar ratio of nickel, cobalt, and manganese in the trimanganese tetraoxide is 0.60-0.75:1; the lithium source is one or a combination of two or more of lithium nitrate, lithium hydroxide, lithium carbonate, and lithium oxalate.

Citation Information

Cited By

  • Manganese tetraoxide precursor as well as preparation method and application thereof

    CN121342088A