Cobalt-free nickel-manganese binary precursor material as well as preparation method and application thereof

By adding additives during the co-precipitation growth stage and using a reducing agent during the washing stage, the crystallinity and manganese oxide precipitation problems of cobalt-free nickel-manganese binary precursors were solved, thereby improving the electrochemical performance and cycle stability of the material.

CN118993168AActive Publication Date: 2024-11-22GEM CO LTD

Patent Information

Application Number
CN202410989321.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-22
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

Traditional cobalt-free nickel-manganese binary precursors suffer from poor crystallinity and easy precipitation of manganese oxides during preparation, which affects electrochemical performance and cycle stability. Existing improvement methods may introduce impurities or fail to completely suppress manganese oxide precipitation.

Method used

Additives are added during the growth stage of the co-precipitation reaction to regulate crystal growth, and a reducing agent is used in the washing stage of the post-treatment to inhibit the precipitation of manganese oxides. The preparation method includes adjusting the pH value and controlling the particle size, and using a combination of specific complexing agents and reducing agents for the washing process.

Benefits of technology

A cobalt-free nickel-manganese binary precursor with good crystallinity and no manganese oxide precipitation was obtained, which improved the electrochemical performance and cycle stability of the material and reduced the impurity content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993168A_ABST
    Figure CN118993168A_ABST
Patent Text Reader

Abstract

The invention provides a cobalt-free nickel-manganese binary precursor material and a preparation method and application thereof, and the preparation method comprises the following steps: mixing a nickel-manganese metal source solution, a precipitant solution and a first complexing agent solution, and carrying out a nucleation stage of a coprecipitation reaction; after the nucleation stage is finished, adjusting the pH value of the coprecipitation reaction, replacing the first complexing agent solution with a second complexing agent solution containing an additive, and carrying out a growth stage of the coprecipitation reaction to obtain precursor slurry; and washing and drying the precursor slurry to obtain the cobalt-free nickel manganese binary precursor material, a washing solution adopted for washing comprises a reducing agent. According to the preparation method disclosed by the invention, the additive is added in the growth stage of the coprecipitation reaction to control the crystal growth, and the reducing agent is added in the washing stage of the post-treatment to inhibit the precipitation of the manganese oxide, so that the obtained precursor has better crystallinity and lower precipitation amount of the manganese oxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries and relates to a cobalt-free nickel-manganese binary precursor material and a preparation method and application thereof. Background Art

[0002] The rapid development of electric vehicles has increased the demand for high-performance, high-safety and long-life lithium-ion batteries. Ternary cathode materials have become a research hotspot in the current power battery field due to their high energy density and good electrochemical properties. However, due to the scarcity and high price of metal cobalt resources, current research on cathode materials has gradually shifted to cobalt-free nickel-manganese binary material systems to avoid the limitations of cobalt resource shortages on the development of cathode materials. Nickel and manganese resources are relatively abundant, and nickel-manganese binary materials also have the advantages of high capacity, good capacity retention, low toxicity and low cost, making cobalt-free nickel-manganese binary materials a research hotspot for cathode materials.

[0003] However, the traditional cobalt-free nickel-manganese binary precursor often has problems such as poor crystallinity and easy precipitation of manganese oxide during the preparation process. These problems not only affect the electrochemical performance of the positive electrode material, but also reduce its cycle stability and safety. In the prior art, additives are usually added during the coprecipitation of the precursor to improve the above problems. For example, CN 116216796A adds ethylene glycol as a modifier to the reaction bottom liquid, which properly controls the crystallinity of the nickel-manganese binary precursor, inhibits the precipitation of manganese tetraoxide, and improves the material morphology. However, ethylene glycol may be mixed in the precursor particles, and for nickel-manganese binary materials with high manganese content, it may still be difficult to avoid manganese being oxidized in the post-processing link, thereby affecting the quality of the precursor product.

[0004] Therefore, it is necessary to develop a method for preparing a cobalt-free nickel-manganese binary precursor without introducing new impurities and ensuring that the precursor product has good crystallinity and no manganese oxide precipitation. Summary of the invention

[0005] The object of the present invention is to provide a cobalt-free nickel-manganese binary precursor material and a preparation method and application thereof. The preparation method controls crystal growth by adding an additive in the growth stage of the coprecipitation reaction, and adds a reducing agent in the washing stage of the post-treatment to inhibit the precipitation of manganese oxide, so that the obtained precursor has better crystallinity and lower manganese oxide precipitation, thereby improving the product quality of the precursor.

[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a method for preparing a cobalt-free nickel-manganese binary precursor material, the preparation method comprising the following steps:

[0008] (1) mixing a nickel-manganese metal source solution, a precipitant solution and a first complexing agent solution to perform a nucleation stage of a coprecipitation reaction;

[0009] (2) after the nucleation stage of step (1) is completed, the pH of the coprecipitation reaction is adjusted, and the first complexing agent solution is replaced with a second complexing agent solution containing an additive to carry out a growth stage of the coprecipitation reaction to obtain a precursor slurry;

[0010] (3) washing and drying the precursor slurry in step (2) to obtain the cobalt-free nickel-manganese binary precursor material;

[0011] The washing liquid used in the washing includes a reducing agent.

[0012] The present invention adds a small amount of additives that can affect the growth of the precursor crystal surface during the growth stage of the coprecipitation reaction, thereby regulating the crystallinity and crystal structure of the precursor and avoiding the additives from being wrapped inside the particles and introducing more impurities during the rapid nucleation stage of the precursor; and the present invention adds a reducing agent to wash the precursor slurry in the washing step of post-treatment, thereby inhibiting the precipitation of manganese oxide on the particle surface, further ensuring the high crystallinity and structural uniformity of the precursor, improving the surface morphology of the precursor, and preparing a cobalt-free nickel-manganese binary precursor with good crystallinity and no precipitation of manganese oxide.

[0013] Preferably, the total metal ion concentration of the nickel-manganese metal source solution in step (1) is 1.0-3.0 mol / L, for example, 1.0 mol / L, 2.0 mol / L or 3.0 mol / L, wherein the molar ratio of nickel ions to manganese ions is (1-x):x, wherein x is 0.1-0.95, for example, 0.1, 0.3, 0.5, 0.7, 0.9 or 0.95, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0014] Preferably, the concentration of the precipitant solution in step (1) is 20-40wt%, for example, 20wt%, 30wt% or 40wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0015] Preferably, the concentration of the first complexing agent solution in step (1) is 10-25wt%, for example, 10wt%, 20wt% or 25wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0016] Preferably, the mixing in step (1) comprises flowing the nickel-manganese metal source solution, the precipitant solution and the first complexing agent solution into the base solution in parallel.

[0017] Preferably, the base solution comprises water, a precipitant solution and a first complexing agent solution.

[0018] Preferably, the pH of the base solution is 11.2-12.5, for example, 11.2, 11.5, 12.0 or 12.5, and the concentration of the complexing agent is 2-12 g / L, for example, 2 g / L, 5 g / L, 10 g / L or 12 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] Preferably, the temperature of the nucleation stage in step (1) and the growth stage in step (2) are independently 40-80°C, for example, 40°C, 60°C or 80°C, the concentration of the complexing agent in the reaction system is maintained in the range of 2-12 g / L, for example, 2 g / L, 5 g / L, 10 g / L or 12 g / L, and the reaction is carried out in nitrogen and / or argon.

[0020] Preferably, the pH value in the nucleation stage of step (1) is 11.3-12.5, for example, 11.3, 11.5, 12.0 or 12.5, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0021] Preferably, in the second complexing agent solution in step (2), the content of the additive is 0.1-10wt%, for example, it can be 0.1wt%, 1wt%, 3wt%, 5wt%, 7wt%, 9wt% or 10wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0022] The content of additives added in the growth stage of the present invention will affect crystal growth. If the amount of additives added is too little, it will not play a role in regulating the growth of particle crystals. If the amount of additives added is too much, it is easy to remain in the sample, affecting the quality of the precursor and increasing material costs.

[0023] Preferably, the additive in step (2) comprises any one of polyvinyl pyrrolidone, polyethylene glycol, tetramethylammonium hydroxide, hexadecyltrimethylammonium bromide or triethanolamine, or a combination of at least two thereof.

[0024] Preferably, in the second complexing agent solution in step (2), the content of the complexing agent is 10-25wt%, for example, 10wt%, 15wt%, 20wt% or 25wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0025] Preferably, in step (2), the pH of the coprecipitation reaction is adjusted to 9.6-11.3, for example, 9.6, 10, 10.5, 11 or 11.3, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0026] Preferably, the growth stage of step (2) reacts to a precursor particle size D50 of 2-20 μm, for example, 2 μm, 5 μm, 10 μm, 15 μm or 20 μm, but is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable, preferably 4-12 μm.

[0027] Preferably, the precursor slurry in step (2) is aged before being washed in step (3).

[0028] Preferably, the aging pH is 9-11, for example, 9, 10 or 11, and the aging time is 6-12h, for example, 6h, 8h, 10h or 12h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0029] The precursor slurry of the present invention is allowed to stand, and after the supernatant is extracted, alkali solution and pure water are added to adjust the pH value of aging to 9-11 for aging.

[0030] Preferably, in the washing liquid of step (3), the content of the reducing agent is 0.1-10wt%, for example, it can be 0.1wt%, 1wt%, 3wt%, 5wt%, 7wt%, 9wt% or 10wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] The content of the reducing agent in the washing process of the present invention will affect the washing effect. If the amount of reducing agent added is too little, the precipitation of manganese oxide cannot be effectively suppressed. If the amount of reducing agent added is too much, it may remain in the sample, affecting the quality of the precursor and appropriately increasing the cost.

[0032] Preferably, the reducing agent comprises any one of glucose, citric acid, ascorbic acid or oxalic acid, or a combination of at least two thereof.

[0033] Preferably, the washing liquid in step (3) comprises an alkaline solution containing a reducing agent, and / or water containing a reducing agent.

[0034] The washing in step (3) of the present invention comprises alkali washing twice or more and then water washing twice or more, wherein the alkali washing is performed using an alkali solution containing a reducing agent and the water washing is performed using water containing a reducing agent.

[0035] Preferably, the alkali content in the alkali solution containing the reducing agent is 1-10wt%, for example, 1wt%, 5wt% or 10wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] Preferably, the number of washings in step (3) is 2 or more times, for example, 2, 4, 6 or 8 times, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0037] Preferably, the drying temperature in step (3) is 80-150°C, for example, 80°C, 100°C, 130°C or 150°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0038] Preferably, the water content of the cobalt-free nickel-manganese binary precursor material in step (3) is below 0.8wt%, for example, 0.8wt%, 0.6wt%, 0.4wt% or 0.2wt%, and the chemical formula of the cobalt-free nickel-manganese binary precursor material is Ni 1-x Mn x (OH)2, wherein 0.10≤x≤0.95, for example, it can be 0.1, 0.3, 0.5, 0.7, 0.9 or 0.95, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0039] As a preferred technical solution of the preparation method of the present invention, the preparation method comprises the following steps:

[0040] (1) a nickel-manganese metal source solution having a total metal ion concentration of 1.0-3.0 mol / L, a precipitant solution having a concentration of 20-40 wt % and a first complexing agent solution having a concentration of 10-25 wt % are introduced into the bottom liquid in parallel, and a nucleation stage of a coprecipitation reaction is performed in nitrogen and / or argon at a temperature of 40-80° C., a complexing agent concentration of 2-12 g / L and a pH of 11.3-12.5;

[0041] The base solution includes water, a precipitant solution and a first complexing agent solution, the pH of the base solution is 11.2-12.5, and the concentration of the complexing agent is 2-12 g / L;

[0042] (2) After the nucleation stage of step (1), the pH of the coprecipitation reaction is adjusted to 9.6-11.3, and the first complexing agent solution is replaced with a second complexing agent solution containing an additive to carry out the growth stage of the coprecipitation reaction until the particle size D50 of the precursor particles is 2-20 μm, and then aged at a pH of 9-11 for 6-12 hours to obtain a precursor slurry;

[0043] In the second complexing agent solution, the content of the additive is 0.1-10wt%, and the content of the complexing agent is 10-25wt%;

[0044] (3) washing the precursor slurry of step (2), and then drying it at 80-150° C. to obtain the cobalt-free nickel-manganese binary precursor material having a moisture content of less than 0.8 wt %;

[0045] The washing liquid used in the washing comprises 0.1-10 wt % of a reducing agent, and the washing liquid comprises an alkali solution containing a reducing agent, and / or water containing a reducing agent.

[0046] In a second aspect, the present invention provides a cobalt-free nickel-manganese binary precursor material, wherein the cobalt-free nickel-manganese binary precursor material is prepared by the preparation method described in the first aspect.

[0047] In a third aspect, the present invention provides a cobalt-free nickel-manganese binary positive electrode material, which is obtained by mixing and sintering a lithium source and the cobalt-free nickel-manganese binary precursor material as described in the second aspect.

[0048] In a fourth aspect, the present invention provides a lithium-ion battery, wherein the lithium-ion battery comprises the cobalt-free nickel-manganese binary positive electrode material as described in the third aspect.

[0049] Compared with the prior art, the present invention has the following beneficial effects:

[0050] The present invention regulates the crystallinity and crystal structure of the precursor by adding a small amount of additives that can affect the growth of the precursor crystal surface during the growth stage of the coprecipitation reaction, and avoids the additives being wrapped inside the particles during the rapid nucleation stage of the precursor to introduce more impurities; and the present invention adds a reducing agent to wash the precursor slurry in the washing step of post-treatment, thereby inhibiting the precipitation of manganese oxide on the particle surface, further ensuring the high crystallinity and structural uniformity of the precursor, improving the surface morphology of the precursor, and preparing a cobalt-free nickel-manganese binary precursor with good crystallinity and no manganese oxide precipitation. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 This is a SEM image of the cobalt-free nickel-manganese binary precursor material obtained in Example 1 of the present invention;

[0052] Figure 2 This is a SEM image of the cobalt-free nickel-manganese binary precursor material obtained in Comparative Example 1 of the present invention;

[0053] Figure 3 This is a SEM image of the cobalt-free nickel-manganese binary precursor material obtained in Comparative Example 2 of the present invention;

[0054] Figure 4This is a SEM image of the cobalt-free nickel-manganese binary precursor material obtained in Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0055] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0056] Example 1

[0057] This embodiment provides a method for preparing a cobalt-free nickel-manganese binary precursor material, the preparation method comprising the following steps:

[0058] (1) According to the molecular formula Ni 0.25 Mn 0.75 (OH)2, manganese sulfate, nickel sulfate and water are prepared into a nickel-manganese metal source solution with a total metal ion concentration of 2 mol / L, the nickel-manganese metal source solution with a total metal ion concentration of 2 mol / L, a sodium hydroxide solution with a concentration of 32 wt% and a first ammonia solution with a concentration of 16 wt% are added into a 50 L reactor containing a bottom liquid at flow rates of 1.86 kg / h, 0.78 kg / h and 0.24 kg / h, respectively, to carry out a nucleation stage of a co-precipitation reaction, and the pH of the nucleation stage is controlled at 12.0 and maintained for 6 hours;

[0059] The entire coprecipitation reaction stage was carried out in nitrogen at a temperature of 55° C., a stirring speed of 600 rpm, and an ammonia concentration of 5.5 g / L; the base liquid included water, sodium hydroxide solution, and ammonia solution, and the pH of the base liquid was 12.2 and the ammonia concentration was 5.5 g / L;

[0060] (2) After the nucleation stage in step (1) is completed, the pH of the coprecipitation reaction is adjusted to 10.0, and the first ammonia solution is replaced with a second complexing agent solution containing an additive to carry out the growth stage of the coprecipitation reaction until the precursor particle size D50 is 10 μm, the feeding is stopped, and then the mixture is allowed to stand, and after the supernatant is extracted, sodium hydroxide alkali solution and pure water are added to adjust the pH to 10 and aged for 8 hours to obtain a precursor slurry;

[0061] In the second complexing agent solution, the content of the additive is 4wt%, the content of the complexing agent is 16wt%, the additive is triethanolamine, and the complexing agent is ammonia water;

[0062] (3) The precursor slurry of step (2) is transferred to a scrubber, and is alkali washed three times and water washed three times using a dilute sodium hydroxide solution containing D-isoascorbic acid (reducing agent D-isoascorbic acid: sodium hydroxide: water = 1:4:95) and water (reducing agent D-isoascorbic acid: water = 2:98), and then dried at 120° C. after solid-liquid separation to obtain the cobalt-free nickel-manganese binary precursor material with a moisture content of 0.5wt%. The molecular formula of the cobalt-free nickel-manganese binary precursor material is Ni 0.25 Mn 0.75 (OH)2;

[0063] The content of D-isoascorbic acid in the dilute sodium hydroxide solution containing D-isoascorbic acid is 1 wt %, and the content of D-isoascorbic acid in the water containing D-isoascorbic acid is 2 wt %;

[0064] The SEM image of the cobalt-free nickel-manganese binary precursor material obtained in this example is as follows: Figure 1 Shown

[0065] Example 2

[0066] This embodiment provides a method for preparing a cobalt-free nickel-manganese binary precursor material, the preparation method comprising the following steps:

[0067] (1) According to the molecular formula Ni 0.5 Mn 0.5 (OH)2, manganese sulfate, nickel sulfate and water are prepared into a nickel-manganese metal source solution with a total metal ion concentration of 3.0 mol / L, and the nickel-manganese metal source solution with a total metal ion concentration of 3.0 mol / L, a sodium hydroxide solution with a concentration of 40 wt% and a first ammonia solution with a concentration of 25 wt% are added into a 50 L reactor containing a bottom liquid to carry out a nucleation stage of a coprecipitation reaction, and the pH of the nucleation stage is controlled at 11.3 and maintained for 6 hours;

[0068] The entire coprecipitation reaction stage is carried out in nitrogen, at a temperature of 80° C. and an ammonia concentration of 12 g / L; the base liquid includes water, sodium hydroxide solution and ammonia, the pH of the base liquid is 11.2, and the complexing agent concentration is 12 g / L;

[0069] (2) After the nucleation stage in step (1) is completed, the pH of the coprecipitation reaction is adjusted to 9.6, and the first ammonia solution is replaced with a second complexing agent solution containing an additive to carry out the growth stage of the coprecipitation reaction until the precursor particle size D50 is 12 μm, the feeding is stopped, and then the mixture is allowed to stand, and after the supernatant is extracted, sodium hydroxide alkali solution and pure water are added to adjust the pH to 9 for aging for 12 hours to obtain a precursor slurry;

[0070] In the second complexing agent solution, the content of the additive is 10wt%, the content of the complexing agent is 10wt%, the additive is hexadecyltrimethylammonium bromide, and the complexing agent is ammonia water;

[0071] (3) The precursor slurry of step (2) is transferred to a scrubber, and is alkaline washed twice and washed three times with water using a dilute sodium hydroxide solution containing citric acid (reducing agent citric acid: sodium hydroxide: water = 10:4:86) and water (reducing agent citric acid: water = 0.1:99.9), and then dried at 150° C. after solid-liquid separation to obtain the cobalt-free nickel-manganese binary precursor material with a moisture content of 0.8wt%. The molecular formula of the cobalt-free nickel-manganese binary precursor material is Ni 0.5 Mn 0.5 (OH)2;

[0072] The content of citric acid in the dilute sodium hydroxide solution containing citric acid is 10 wt %, and the content of citric acid in the water containing citric acid is 0.1 wt %.

[0073] Example 3

[0074] This embodiment provides a method for preparing a cobalt-free nickel-manganese binary precursor material, the preparation method comprising the following steps:

[0075] (1) According to the molecular formula Ni 0.25 Mn 0.75 (OH)2, manganese sulfate, nickel sulfate and water are prepared into a nickel-manganese metal source solution with a total metal ion concentration of 1.0 mol / L, and the nickel-manganese metal source solution with a total metal ion concentration of 1.0 mol / L, a sodium hydroxide solution with a concentration of 20 wt% and a first ammonia solution with a concentration of 10 wt% are added into a 50 L reactor containing a bottom liquid to carry out a nucleation stage of a coprecipitation reaction, and the pH of the nucleation stage is controlled at 12.5 and maintained for 6 hours;

[0076] The entire coprecipitation reaction stage is carried out in nitrogen, at a temperature of 40° C. and an ammonia concentration of 2 g / L; the base liquid includes water, a precipitant solution and a first complexing agent solution, the pH of the base liquid is 12.5, and the complexing agent concentration is 2 g / L;

[0077] (2) After the nucleation stage in step (1) is completed, the pH of the coprecipitation reaction is adjusted to 11.3, and the first ammonia solution is replaced with a second complexing agent solution containing an additive to carry out the growth stage of the coprecipitation reaction until the precursor particle size D50 is 4 μm, the feeding is stopped, and then the mixture is allowed to stand, and after the supernatant is extracted, sodium hydroxide alkali solution and pure water are added to adjust the pH to 11 and aged for 6 hours to obtain a precursor slurry;

[0078] In the second complexing agent solution, the content of the additive is 0.1wt%, the content of the complexing agent is 25wt%, the additive is triethanolamine, and the complexing agent is ammonia water;

[0079] (3) The precursor slurry of step (2) is transferred to a scrubber, and is alkali-washed 3 times and washed with water 2 times using a dilute sodium hydroxide solution containing D-isoascorbic acid (reducing agent D-isoascorbic acid: sodium hydroxide: water = 0.1:4:95.9) and water (reducing agent D-isoascorbic acid: water = 10:90), and then dried at 100° C. after solid-liquid separation to obtain the cobalt-free nickel-manganese binary precursor material with a moisture content of 0.8wt%. The molecular formula of the cobalt-free nickel-manganese binary precursor material is Ni 0.25 Mn 0.75 (OH)2;

[0080] The content of D-isoascorbic acid in the dilute sodium hydroxide solution containing D-isoascorbic acid is 0.1 wt %. The content of D-isoascorbic acid in the water containing D-isoascorbic acid is 10 wt %.

[0081] Example 4

[0082] This embodiment provides a method for preparing a cobalt-free nickel-manganese binary precursor material. The preparation method is the same as that of Embodiment 1 except that in step (2), the content of the additive in the second complexing agent solution is 0.05 wt %.

[0083] Example 5

[0084] This embodiment provides a method for preparing a cobalt-free nickel-manganese binary precursor material. The preparation method is the same as that of Embodiment 1 except that in step (2), the content of the additive in the second complexing agent solution is 12 wt %.

[0085] Example 6

[0086] This embodiment provides a method for preparing a cobalt-free nickel-manganese binary precursor material, which is the same as that of Embodiment 1 except that the content of D-isoascorbic acid in the dilute sodium hydroxide solution containing D-isoascorbic acid is 0.05 wt %.

[0087] Example 7

[0088] This embodiment provides a method for preparing a cobalt-free nickel-manganese binary precursor material, which is the same as that of Embodiment 1 except that the content of D-isoascorbic acid in the dilute sodium hydroxide solution containing D-isoascorbic acid is 12 wt %.

[0089] Comparative Example 1

[0090] This comparative example provides a method for preparing a cobalt-free nickel-manganese binary precursor material, which is the same as Example 1 except that the first ammonia solution is not replaced by a second complexing agent solution containing an additive, and the washing solution used in step (3) does not contain a reducing agent, and a sodium hydroxide solution with a mass fraction of 4% is used for alkaline washing 3 times and pure water is used for water washing 3 times;

[0091] The SEM image of the cobalt-free nickel-manganese binary precursor material obtained in this comparative example is as follows Figure 2 shown.

[0092] Comparative Example 2

[0093] This comparative example provides a method for preparing a cobalt-free nickel-manganese binary precursor material. The preparation method is the same as Example 1 except that the washing liquid used in step (3) does not contain a reducing agent, and a sodium hydroxide solution with a mass fraction of 4% is used for alkaline washing 3 times and pure water is used for washing 3 times;

[0094] The SEM image of the cobalt-free nickel-manganese binary precursor material obtained in this comparative example is as follows Figure 3 shown.

[0095] Comparative Example 3

[0096] This comparative example provides a method for preparing a cobalt-free nickel-manganese binary precursor material, which is the same as Example 1 except that the first ammonia solution is not replaced by a second complexing agent solution containing an additive;

[0097] The SEM image of the cobalt-free nickel-manganese binary precursor material obtained in this comparative example is as follows Figure 4 shown.

[0098] Comparative Example 4

[0099] This comparative example provides a method for preparing a cobalt-free nickel-manganese binary precursor material. The preparation method is the same as Example 1 except that the first ammonia solution in step (1) is replaced by a second complexing agent solution containing an additive, so that the second complexing agent solution containing an additive is used throughout the coprecipitation reaction.

[0100] The cobalt-free nickel-manganese binary precursor material obtained in the above examples and comparative examples was evenly mixed with lithium hydroxide according to a lithium ratio of Li / TM=1.55, and then sintered at 850°C for 18 hours to obtain a lithium-rich manganese-based positive electrode material, and assembled into button cells for electrochemical performance testing. The specific experimental steps are as follows: First, the active material (lithium-rich manganese-based positive electrode material obtained by sintering), conductive agent acetylene black, and binder polyvinylidene fluoride were dissolved in N-methylpyrrolidone in a mass ratio of 8:1:1, and the slurry was mixed using a homogenizer in a multi-stage mode at room temperature; then, the ground slurry was evenly applied to the aluminum foil with a coater, and dried at 80°C in a vacuum drying oven for 12 hours; finally, the aluminum foil was punched into 1.13 cm 2 Circular electrode sheet.

[0101] The obtained electrode sheet was used as the positive electrode, the lithium metal sheet was used as the counter electrode, and the porous polypropylene membrane (Celgard2400, USA) was used as the separator to separate the positive electrode and the counter electrode. The CR-2032 battery was assembled in a glove box filled with Ar gas. The battery was tested using a battery test system (Blue Electric CT2001A, Wuhan, China), first activated three times at 0.1C rate / 2.0~4.6V, and then the activated button cell was tested for electrochemical performance under the conditions of 2.0V-4.6V@0.1C / 0.1C.

[0102] The test results are shown in Table 1:

[0103] Table 1

[0104] <![CDATA[Initial discharge specific capacity / mAh·g -1 > 0.1C cycle 100 weeks capacity retention rate / % Example 1 255.78 93.22 Example 2 253.46 92.53 Example 3 252.98 92.18 Example 4 245.26 91.70 Example 5 247.33 91.39 Example 6 244.68 90.44 Example 7 249.49 91.06 Comparative Example 1 226.63 84.39 Comparative Example 2 240.97 87.95 Comparative Example 3 237.52 85.73 Comparative Example 4 242.85 88.21

[0105] From Table 1 we can see that:

[0106] (1) It can be seen from Example 1 and Comparative Examples 1-3 that the present invention adds additives in the precursor growth stage and adds a reducing agent in the washing stage, which can ensure crystallinity and avoid the precipitation of small manganese oxide particles. Figure 1-Figure 2 By comparison, it can be seen that by adding additives in the growth stage of the coprecipitation reaction and adding reducing agents in the alkaline washing and water washing processes of the post-treatment stage, no small manganese oxide particles are precipitated on the surface of the obtained precursor particles, and the boundaries of the primary grains are clear, well-developed, and have good crystallinity. However, in Comparative Example 1, in which no additives and reducing agents are added, more tiny particles are precipitated on the surface of the precursor, and the boundaries of the primary grains are fuzzy, the morphology is porous, and the crystallinity is poor. Therefore, the first-cycle discharge specific capacity and cycle performance of the battery obtained in Comparative Example 1 are reduced.

[0107] (2) By Figure 1 and Figure 3It can be found that in Comparative Example 2, the additive is added in the growth stage of the coprecipitation reaction but the reducing agent is not added in the post-treatment stage. The obtained precursor particles have small manganese oxide particles precipitated on the surface, but the primary grains are well developed, free of holes, and have good crystallinity, indicating that the addition of the additive plays an important role in improving its crystallinity, but the effect of inhibiting the precipitation of manganese oxide is not obvious. The first cycle discharge specific capacity and cycle performance of the battery obtained in Comparative Example 2 are lower than those in Example 1; Figure 1 and Figure 4 It can be found that in Comparative Example 3, no additive is added in the growth stage of the coprecipitation reaction, but a reducing agent is added in the post-treatment stage. No obvious small manganese oxide particles are precipitated on the surface of the obtained precursor particles, but the primary grains are poorly developed, there are holes, and the crystallinity is poor, which verifies that the reducing agent has a significant effect on inhibiting the precipitation of manganese oxide. The first cycle discharge specific capacity and cycle performance of the battery obtained in Comparative Example 3 are lower than those in Example 1; at the same time, compared Figure 2 and Figure 4 It can be found that the crystallinity of the primary grains of Comparative Example 3 is still better than that of Comparative Example 1, which can also explain that the addition of a reducing agent in the post-treatment stage also has a certain effect on improving the crystallinity of the nickel-manganese precursor while inhibiting the precipitation of manganese oxide. Therefore, the first-cycle discharge specific capacity and cycle performance of the battery of Comparative Example 3 are improved compared with those of Comparative Example 1.

[0108] (3) It can be seen from Example 1 and Comparative Example 4 that the present invention also uses a complexing agent solution containing additives in the nucleation stage, which will wrap the additives inside the particles, introduce more impurities inside the particles, and make it difficult to wash and remove them, thereby affecting the performance of the precursor; it can be seen from Example 1 and Examples 4-5 that the content of the additive will affect the effect of the additive; it can be seen from Example 1 and Examples 6-7 that the amount of the reducing agent added in the washing process of the present invention will affect its effect of inhibiting the precipitation of manganese oxides, thereby affecting the performance of the obtained precursor.

[0109] In summary, the present invention provides a cobalt-free nickel-manganese binary precursor material and a preparation method and application thereof. The preparation method controls crystal growth by adding additives in the growth stage of the coprecipitation reaction, and adds a reducing agent in the washing stage of post-treatment to inhibit the precipitation of manganese oxide, so that the obtained precursor has better crystallinity and lower manganese oxide precipitation, thereby improving the product quality of the precursor.

[0110] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a cobalt-free nickel-manganese binary precursor material, characterized in that: The preparation method comprises the following steps: (1) mixing a nickel-manganese metal source solution, a precipitant solution and a first complexing agent solution to perform a nucleation stage of a coprecipitation reaction; (2) after the nucleation stage of step (1) is completed, the pH of the coprecipitation reaction is adjusted, and the first complexing agent solution is replaced with a second complexing agent solution containing an additive to carry out a growth stage of the coprecipitation reaction to obtain a precursor slurry; (3) washing and drying the precursor slurry in step (2) to obtain the cobalt-free nickel-manganese binary precursor material; The washing liquid used in the washing includes a reducing agent.

2. The preparation method according to claim 1, characterized in that: The total metal ion concentration of the nickel-manganese metal source solution in step (1) is 1.0-3.0 mol / L, wherein the molar ratio of nickel ions to manganese ions is (1-x):x, wherein x is 0.1-0.95; Preferably, the concentration of the precipitant solution in step (1) is 20-40 wt %; Preferably, the concentration of the first complexing agent solution in step (1) is 10-25 wt %.

3. The preparation method according to claim 1 or 2, characterized in that: The mixing in step (1) includes flowing a nickel-manganese metal source solution, a precipitant solution and a first complexing agent solution into the base solution in parallel; Preferably, the base solution comprises water, a precipitant solution and a first complexing agent solution; Preferably, the pH of the base solution is 11.2-12.5, and the concentration of the complexing agent is 2-12 g / L; Preferably, the temperature of the nucleation stage in step (1) and the growth stage in step (2) are independently 40-80° C., the concentration of the complexing agent in the reaction system is maintained in the range of 2-12 g / L, and the reaction is carried out in nitrogen and / or argon; Preferably, the pH of the nucleation stage in step (1) is 11.3-12.

5.

4. The preparation method according to any one of claims 1 to 3, characterized in that Step (2) In the second complexing agent solution, the content of the additive is 0.1-10wt%; Preferably, the additive in step (2) comprises any one of polyvinyl pyrrolidone, polyethylene glycol, tetramethylammonium hydroxide, hexadecyltrimethylammonium bromide or triethanolamine, or a combination of at least two thereof; Preferably, in the second complexing agent solution in step (2), the content of the complexing agent is 10-25 wt %.

5. The preparation method according to any one of claims 1 to 4, characterized in that: Step (2) adjusting the pH of the coprecipitation reaction to 9.6-11.3; Preferably, the growth stage of step (2) is reacted until the precursor particle size D50 is 2-20 μm, preferably 4-12 μm; Preferably, the precursor slurry in step (2) is aged before being washed in step (3); Preferably, the aging pH is 9-11, and the aging time is 6-12 hours.

6. The preparation method according to any one of claims 1 to 5, characterized in that: In the washing liquid of step (3), the content of reducing agent is 0.1-10wt%; Preferably, the reducing agent comprises any one of glucose, citric acid, ascorbic acid or oxalic acid, or a combination of at least two thereof; Preferably, the washing liquid in step (3) comprises an alkaline solution containing a reducing agent, and / or water containing a reducing agent; Preferably, the drying temperature in step (3) is 80-150°C; Preferably, the water content of the cobalt-free nickel-manganese binary precursor material in step (3) is below 0.8 wt %.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: (1) a nickel-manganese metal source solution having a total metal ion concentration of 1.0-3.0 mol / L, a precipitant solution having a concentration of 20-40 wt % and a first complexing agent solution having a concentration of 10-25 wt % are introduced into the bottom liquid in parallel, and a nucleation stage of a coprecipitation reaction is performed in nitrogen and / or argon at a temperature of 40-80° C., a complexing agent concentration of 2-12 g / L and a pH of 11.3-12.5; The base solution includes water, a precipitant solution and a first complexing agent solution, the pH of the base solution is 11.2-12.5, and the concentration of the complexing agent is 2-12 g / L; (2) After the nucleation stage of step (1), the pH of the coprecipitation reaction is adjusted to 9.6-11.3, and the first complexing agent solution is replaced with a second complexing agent solution containing an additive to carry out the growth stage of the coprecipitation reaction until the particle size D50 of the precursor particles is 2-20 μm, and then aged at a pH of 9-11 for 6-12 hours to obtain a precursor slurry; In the second complexing agent solution, the content of the additive is 0.1-10wt%, and the content of the complexing agent is 10-25wt%; (3) washing the precursor slurry of step (2), and then drying it at 80-150° C. to obtain the cobalt-free nickel-manganese binary precursor material having a moisture content of less than 0.8 wt %; The washing liquid used in the washing comprises 0.1-10 wt % of a reducing agent, and the washing liquid comprises an alkali solution containing a reducing agent, and / or water containing a reducing agent.

8. A cobalt-free nickel-manganese binary precursor material, characterized in that: The cobalt-free nickel-manganese binary precursor material is prepared by the preparation method according to any one of claims 1 to 7.

9. A cobalt-free nickel-manganese binary positive electrode material, characterized in that: The cobalt-free nickel-manganese binary positive electrode material is obtained by mixing and sintering a lithium source and the cobalt-free nickel-manganese binary precursor material as claimed in claim 8.

10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the cobalt-free nickel-manganese binary positive electrode material as claimed in claim 9.

Citation Information

Patent Citations

  • Nickel-manganese binary precursor and preparation method thereof, nickel-manganese positive electrode material and battery

    CN115477332A

  • Modified lithium-rich manganese-based precursor as well as preparation method and application thereof

    CN117247055A

  • KR20230070738A

Cited By

  • Monocrystal nickel-rich cobalt-free positive electrode precursor material as well as preparation method and application thereof

    CN121627081A

  • Cobalt-free nickel-manganese binary precursor material, and preparation method therefor and use thereof

    WO2026020713A1