Crystalline hyperbranched multi-arm copolymer, self-supporting graphene film as well as preparation and application of crystalline hyperbranched multi-arm copolymer and self-supporting graphene film
Through the liquid phase peeling process of crystalline hyperbranched multi-arm copolymer and graphite powder, a self-supported graphene film with excellent electrothermal properties and shape memory functions was prepared, which solved the problems of high temperature, high cost and structural defects in the prior art. It adapts to the complex interface and heat dissipation needs of electronic components.
Patent Information
- Application Number
- CN202411003011.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-25
AI Technical Summary
The existing graphene electric-thermal film preparation methods have high temperature, expensive equipment and complex processes, which lead to high costs, many structural defects, and difficulty in adapting to complex interface shapes and shape memory functions, limiting its large-scale applications and the heat dissipation needs of electronic components.
The crystalline hyperbranched multi-arm copolymer is used to catalyze the copolymerization of ethylene and bromine-containing functional monomers through an α-diimine palladium catalyst to obtain a hyperbranched macromolecular initiator, and then atom-transfer radical polymerization is carried out with acrylate functional monomers. A crystalline hyperbranched multi-arm copolymer was formed and high-performance liquid phase stripped from graphite powder in a low boiling point organic solvent to prepare a supporting graphene film.
It realizes high-performance preparation of graphene films, has excellent electrothermal performance, mechanical strength and shape memory functions, adapts to complex interface shapes, reduces preparation costs and structural defects, and promotes large-scale applications and heat dissipation needs of electronic components.
Smart Images

Figure BDA0004962156010000021 
Figure BDA0004962156010000031 
Figure BDA0004962156010000032
Abstract
Description
Technical Field
[0001] The invention relates to a crystalline hyperbranched multi-arm copolymer, a self-supporting graphene film and preparation and application thereof. Background Art
[0002] Graphene has a unique two-dimensional nanostructure and excellent electrical, thermal and mechanical properties. Graphene films made from graphene nanosheets can convert electrical energy into thermal energy efficiently and quickly based on the Joule heating effect, showing excellent electric heating function. Compared with traditional electric heating technology, graphene electric heating films have the advantages of high electric-thermal conversion efficiency, fast response, and energy saving. They also have the advantages of abundant raw material sources, light weight, and flexibility. They have important application prospects in many fields such as de-icing, intelligent driving, health therapy, national defense, military industry, industry, and civilian use.
[0003] The existing preparation methods of graphene electric heating film mainly include the following two categories: First, a graphene film is grown on the surface of a metal substrate by CVD technology, and then it is transferred to the surface of various polymer films by etching, transfer and other processes to obtain a graphene electric heating film with a polymer film as the substrate; this method is conducive to the preparation of graphene films with larger lateral dimensions, but the preparation process involves high temperature, expensive equipment and complex graphene transfer process, and the preparation cost is high, which is not conducive to large-scale application. Second, graphene oxide is obtained by oxidation of natural graphite, and a self-supporting graphene electric heating film or a graphene electric heating film with a polymer film as the substrate is obtained by vacuum filtration, dip coating, scraping, drip coating, spin coating and other processes and high temperature or chemical reduction; the graphene oxide involved in this method can be stably dispersed in an aqueous medium, so that a graphene electric heating film can be obtained by a variety of liquid phase processing methods, which is conducive to large-scale preparation and application, but the graphene oxidation-reduction process often involves toxic chemical reagents, high temperature and complex steps, and the resulting graphene structure has many defects, which is not conducive to the electric heating performance of the film. Therefore, how to start from the abundant natural graphite resources, prepare high-performance graphene electric heating films through green, environmentally friendly, simple and feasible processes, and promote their large-scale preparation and application, is still an important key technology that needs to be researched and broken through in this field.
[0004] In addition, with the development of advanced information technologies such as 5G, various electronic components are becoming increasingly miniaturized, high-frequency and multifunctional. Their significantly increased power density makes efficient heat dissipation a common key requirement. In response to this demand, a series of high-performance thermal conductive interface material preparation and application research have been widely reported, mainly including thermal conductive gaskets, thermal conductive gels, thermal conductive adhesives, thermal conductive films, thermal conductive phase change materials, etc. Among them, graphene thermal conductive films made with graphene as the main raw material have outstanding application advantages in this field for the following reasons: First, graphene materials can be prepared from abundant natural graphite resources; second, graphene has a unique two-dimensional nanostructure and shows excellent anisotropic thermal conductivity; third, graphene films have the characteristics of light weight and flexibility, which can better adapt to the application requirements of electronic components for thinness and flexibility. Therefore, the preparation and application technology development of graphene thermal conductive films is of great significance to solving the heat dissipation needs of electronic components.
[0005] So far, many methods for preparing graphene thermal conductive films have been developed and reported, mainly including the following two categories: First, graphene films are first grown on the surface of various metal substrates by chemical vapor deposition technology, and then transferred to the surface of a specific polymer film by transfer or etching to obtain a graphene thermal conductive film with a polymer film as the substrate; since this method involves high temperature, expensive equipment and complex graphene transfer process, the preparation cost is high, which is not conducive to large-scale application. Second, graphene oxide is first obtained by oxidation of graphite, and then the graphene thermal conductive film is obtained by vacuum filtration, dip coating, scraping, drip coating, spin coating and other processes and high temperature or chemical reduction treatment; this method can obtain graphene thermal conductive films in various ways through liquid phase processing methods. Although it is conducive to large-scale application, the graphene oxidation-reduction process often involves toxic chemical reagents, high temperature and complex steps. At the same time, the obtained graphene structure has many defects, which is not conducive to the thermal conductivity of the obtained graphene film. In addition, with the increasing prevalence and in-depth application of electronic information technology, the interface shapes of electronic components have become more complex and diverse. There is an urgent need to develop graphene flexible thermal conductive films with shape memory function that can adapt to complex interface shapes. However, the research and application of this type of technology are rarely reported. Summary of the invention
[0006] The first object of the present invention is to provide a crystalline hyperbranched multi-arm copolymer with strong crystallization ability.
[0007] The second object of the present invention is to provide a method for preparing a self-supporting graphene film using the crystalline hyperbranched multi-arm copolymer, which has significant advantages such as abundant raw material sources, simple preparation process, mild conditions, and controllable and adjustable performance.
[0008] The third object of the present invention is to provide a self-supporting graphene film.
[0009] The fourth object of the present invention is to provide the use of the self-supporting graphene film as an electric heating film, which has both excellent electric heating performance and mechanical strength.
[0010] A fifth object of the present invention is to provide the use of the self-supporting graphene film as a thermally conductive film, which has both shape memory and anisotropic thermal conductivity functions.
[0011] In order to achieve the above-mentioned invention object, the present invention adopts the following technical scheme:
[0012] In a first aspect, the present invention provides a crystalline hyperbranched multi-arm copolymer, which is prepared by the following method: using an α-diimine palladium catalyst to catalyze the "chain removal" copolymerization of ethylene and a bromine-containing functional monomer in an anhydrous solvent in a one-step process to obtain a hyperbranched macromolecular initiator; then using the hyperbranched macromolecular initiator to initiate an atom transfer radical polymerization of an acrylate functional monomer to obtain a crystalline hyperbranched multi-arm copolymer;
[0013] The structure of the bromine-containing functional monomer is shown below:
[0014]
[0015] The acrylic acid ester functional monomer is selected from one of the following compounds: hexadecyl acrylate, tetradecyl acrylate, octadecyl acrylate, and behenyl acrylate;
[0016]
[0017] Preferably, the α-diimine palladium catalyst is selected from α-diimine palladium catalyst 1 or 2 whose structure is shown below:
[0018]
[0019] Both of the above can be synthesized in the laboratory according to the following literature:
[0020] [1] Johnson LK, Killian CM, Brookhart MJAm.Chem.Soc., 1995, 117, 6414; [2] Johnson LK, Mecking S., Brookhart MJAm.Chem.Soc., 1996, 118, 267.
[0021] Preferably, the anhydrous solvent is selected from one of the following: dichloromethane, chlorobenzene, chloroform, preferably anhydrous dichloromethane.
[0022] Preferably, the bromine-containing functional monomer can be synthesized in the laboratory according to the literature (Matyjaszewski K., Gaynor SG, Kulfan A., Podwika M. Macromolecules, 1997, 30, 5192).
[0023] Preferably, in the one-step "chain removal" copolymerization system, the feed concentration of the α-diimine palladium catalyst is 0.5-50 g / L, preferably 2-20 g / L, based on the total volume of the anhydrous solvent, and the feed concentration of the bromine-containing functional monomer is 0.05-10 M, preferably 0.1-2 M, based on the total volume of the anhydrous solvent.
[0024] Preferably, the temperature of the one-step "chain removal" copolymerization is 5 to 35°C, preferably 15 to 25°C; the ethylene pressure is 0.05 to 0.5 MPa, preferably 0.1 MPa; and the copolymerization time is 0.5 to 48 h, preferably 2 to 24 h.
[0025] Preferably, the purification of the hyperbranched macromolecular initiator is carried out according to the following steps:
[0026] (a) After the polymerization reaction is completed, the reaction solution is exposed to air to terminate the reaction;
[0027] (b) removing the solvent by blowing cold air to obtain a preliminary polymerization product;
[0028] (c) adding an appropriate amount of THF to dissolve the product, then adding a small amount of concentrated HCl and hydrogen peroxide solution, and dissolving the residual palladium particles of catalyst A by stirring or ultrasound;
[0029] (d) removing the solvent by blowing with cold air, adding an appropriate amount of THF to dissolve the product again to form a saturated solution, adding a large amount of methanol to precipitate the product, and removing the upper solution to obtain a polymer product; repeating this step 2 to 4 times;
[0030] (e) The obtained product is vacuum dried at 50-80° C. to a constant weight to obtain a hyperbranched macromolecular initiator.
[0031] Preferably, the atom transfer radical polymerization is specifically as follows: under the protection of an inert gas (nitrogen, argon or other inert gases), a hyperbranched macromolecular initiator, an acrylate functional monomer, anhydrous toluene as a solvent, pentamethyldiethylenetriamine (PMDETA) or 2,2'-bipyridine (bpy) as a ligand, and cuprous bromide (CuBr) as a catalyst are added into a reaction container, and after the addition, an atom transfer radical polymerization is carried out, and after the polymerization is completed, a crystalline hyperbranched multi-arm copolymer is obtained by separation and purification; the feed concentration of the hyperbranched macromolecular initiator in the polymerization system is 0.001-0.1 mol / L (preferably 0.001-0.01 mol / L) based on the molar concentration of bromine groups contained therein, and the initial feed molar concentration ratio of the hyperbranched macromolecular initiator, the acrylate functional monomer, the ligand, and the catalyst is 1:200-800:0.5-4:0.5-2, preferably 1:400-600:4:2.
[0032] As further preferred, the polymerization temperature of the atom transfer radical polymerization is controlled at 45 to 100° C., more preferably 70 to 80° C.; the reaction time is controlled at 0.5 to 24 h, more preferably 0.5 to 5 h.
[0033] As a further preference, the separation and purification of the crystalline hyperbranched multi-arm copolymer is carried out according to the following steps:
[0034] (a) After the reaction is completed, the reaction solution is exposed to air to terminate the reaction, and a preliminary product is obtained by purging;
[0035] (b) adding an appropriate amount of THF to dissolve the product, then adding a large amount of methanol to precipitate the product, and obtaining a polymer product through separation;
[0036] (c) Repeat step (b) 3 to 5 times, and dry the obtained product at 25 to 80° C. to constant weight to obtain a final polymerization product.
[0037] The crystalline hyperbranched multi-arm copolymer prepared by the invention has a crystallinity of 30 to 80%, preferably 70 to 80%.
[0038] In a second aspect, the present invention provides a method for preparing a self-supporting graphene film, comprising the following steps:
[0039] The crystalline hyperbranched multi-arm copolymer, graphite powder and solvent described in the first aspect are mixed in proportion, and an initial graphene dispersion is obtained by ultrasonic and centrifugal separation, and then a self-supporting graphene film is obtained by suction filtration, elution and drying.
[0040] Preferably, the graphite powder is selected from one of the following: natural phosphorus flake graphite or expanded graphite, preferably natural phosphorus flake graphite; the particle size of the graphite powder is controlled in the range of 100 to 1000 mesh, preferably 100 to 500 mesh.
[0041] Preferably, the solvent is one of the following analytically pure or chemically pure solvents: chloroform, THF, acetone, dichloromethane, preferably THF or chloroform.
[0042] Preferably, the initial charge mass of graphite powder is 1-200 mg / mL, preferably 2-20 mg / mL, based on the total volume of the solvent; the charge mass ratio of the crystalline hyperbranched multi-arm copolymer to the graphite powder is 0.001-2, more preferably 0.01-2, and further preferably 0.1-2.
[0043] Preferably, the ultrasound can be carried out in a container of glass, plastic, metal or other suitable materials; the ultrasound method can be an ultrasound pool or a pulse method, preferably an ultrasound pool method; the ultrasound temperature is controlled at 15 to 45°C, preferably 25 to 35°C; the ultrasound power is controlled at 20 to 100W, preferably 40 to 80W; the ultrasound duration is controlled at 12 to 120h, preferably 24 to 48h.
[0044] Preferably, the centrifugal separation is carried out at a rotation speed of 500 to 8000 rpm, preferably 2000 to 5000 rpm; the centrifugal time is controlled at 5 to 120 min, preferably 25 to 60 min.
[0045] Preferably, the filtration is performed using a filter membrane with an average pore size of 50 to 300 nm and a material of polytetrafluoroethylene, polyvinylidene fluoride, nylon or polypropylene, preferably a filter membrane with a pore size of 100 to 200 nm and a material of polytetrafluoroethylene or nylon.
[0046] Preferably, in the self-supporting graphene film, the content of the crystalline hyperbranched multi-arm copolymer is controlled at 5 to 50% by mass, preferably 20 to 40% by mass.
[0047] Preferably, the thickness of the self-supporting graphene film is controlled to be 25 to 500 μm.
[0048] In a third aspect, the present invention provides a self-supporting graphene film prepared according to the preparation method described in the second aspect.
[0049] In a fourth aspect, the present invention provides the use of the self-supporting graphene film described in the third aspect as an electric heating film.
[0050] In a fifth aspect, the present invention provides the use of the self-supporting graphene film described in the third aspect as a thermally conductive film.
[0051] Compared with the prior art, the present invention has the following outstanding advantages and beneficial effects:
[0052] First, the present invention independently designs and synthesizes a crystalline hyperbranched multi-arm copolymer, which is composed of a polyethylene core in the form of a hyperbranched chain and a linear polymer side chain. It not only has a hyperbranched chain morphology, but also has a strong crystallization ability.
[0053] Secondly, the present invention uses the independently designed and synthesized hyperbranched multi-arm copolymer to effectively promote the efficient liquid phase exfoliation of graphite in common low-boiling point organic solvents through the principle of non-covalent CH-π interaction, and obtains a graphene dispersion. On this basis, a graphene film can be obtained through simple vacuum filtration, avoiding the steps of graphene transfer, oxidation-reduction, etc., and does not involve the use of toxic chemical reagents, high temperatures and special equipment. It has the advantages of simple process and low preparation cost, and is conducive to large-scale application.
[0054] Third, the synthesis of the hyperbranched multi-arm copolymer of the present invention mainly uses ethylene as raw material, and a small amount of functional monomers such as hexadecyl acrylate is also a conventional chemical reagent; the subsequent steps use natural graphite powder or expanded graphite and conventional organic solvents as main raw materials. Therefore, the present invention has the significant advantage of abundant and easily available raw materials, which is also conducive to subsequent applications.
[0055] Fourth, the present invention gives full play to the multifunctional properties of crystalline hyperbranched multi-arm copolymers, namely, promoting liquid phase exfoliation of graphene, realizing non-covalent modification of graphene surface, and promoting stable assembly of graphene sheets to obtain a self-supporting graphene high-performance multifunctional film with sufficient mechanical strength. This feature makes the preparation process completely controllable, which is conducive to the flexible regulation of film performance.
[0056] Fifth, the graphene described in the present invention is obtained through a liquid phase exfoliation process, and has fewer structural defects and better performance than redox graphene. At the same time, with the help of the unique structural design of the crystalline hyperbranched multi-arm copolymer, the mechanical strength of the graphene film can be effectively improved through its crystallization assembly. The graphene film has both excellent electrothermal performance and mechanical strength, and can be used as a graphene electrothermal film, which is conducive to its further practical application.
[0057] Sixth, the present invention utilizes the hyperbranched multi-arm copolymer to not only effectively promote the liquid phase exfoliation of natural graphite to obtain low-defect graphene, but also the copolymer can be stably adsorbed on the surface of the obtained graphene based on the principle of non-covalent CH-π action, and the obtained graphene can be stably assembled to obtain a flexible, high-strength, self-supporting graphene film through the crystallization of the polymer side chains in the copolymer structure; at the same time, the obtained graphene film can be endowed with shape memory function by means of the copolymer crystallization; in addition, the graphene nanosheets can be oriented and arranged by means of vacuum filtration, thereby giving the obtained film anisotropic thermal conductivity. Therefore, through the method described in the present invention, the obtained graphene film has excellent flexibility, strength, anisotropic thermal conductivity, shape memory and other functions, and can be used as a thermally conductive film to better meet the interface heat dissipation requirements of various electronic components. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 : Schematic diagram of the preparation steps of the self-supporting graphene electric heating film described in the present invention.
[0059] Figure 2 :(a) DSC cooling curves of HBPE@PHDA (Example 1) and HBPE@Br (Comparative Example 1); (b) DSC secondary heating curves of HBPE@PHDA (Example 1) and HBPE@Br (Comparative Example 1); (c) Polarized microscope photos of HBPE@PHDA (Example 1) at 25 and 40°C, respectively.
[0060] Figure 3 : (a) Appearance photograph of the sample of Comparative Example 1; (b) Appearance photograph of the sample of Example 1; (c) Surface SEM photograph of the sample of Example 1; (d) Cross-sectional SEM photograph of the sample of Example 1; (e) Local cross-sectional SEM photograph of the sample of Example 1; (f) Stress-strain curve of the sample of Example 1.
[0061] Figure 4 :(a) The electric heating / cooling curve of the sample in Example 1 under different voltages; (b) The infrared thermal image corresponding to each heating time of the sample in Example 1 under a driving voltage of 10V.
[0062] Figure 5 : Electrothermal heating / cooling curves of the samples of Example 2 and Comparative Example 2 at a driving voltage of 9V.
[0063] Figure 6 : Electric heating / cooling curves of the samples of Example 3 and Comparative Example 2 at a driving voltage of 9V.
[0064] Figure 7 :(a) Comparison of the steady-state temperatures of the samples of Example 4 and Comparative Example 2 at 9V; (b) Comparison of the electrothermal heating rates of the samples of Example 4 and Comparative Example 2 at 9V.
[0065] Figure 8 :(a) Comparison of the steady-state temperature of the samples of Example 5 and Comparative Example 2 at 10V; (b) Comparison of the electrothermal heating rate of the samples of Example 5 and Comparative Example 2 at 10V; (c) Comparison of the tensile strength of the samples of Example 5 and Comparative Example 2.
[0066] Fig. 9 : (a) Appearance of the graphene film obtained in Example 6; (b) Stress-strain curve of the graphene film obtained in Example 6; (c) Appearance of the graphene film obtained in Comparative Example 3; (d) Thermal conductivity result of the graphene film obtained in Example 6; (e) Evaluation of the shape memory performance of the graphene film obtained in Example 6.
[0067] Fig.10 : (a) Thermal conductivity results of the graphene film obtained in Example 7; (b) Method for evaluating the heat transfer performance in the vertical direction of the graphene film obtained in Example 7; (c) Trend of surface temperature of the graphene film obtained in Example 7 with test time (vertical heat transfer); (d) Method for evaluating the in-plane heat transfer performance of the graphene film obtained in Example 7; (eg) Infrared thermal images of the graphene film obtained in Example 7 at different test times (in-plane heat transfer).
[0068] Fig.11 : Evaluation of the application performance of the graphene film obtained in Example 8 in mobile phone heat dissipation.
[0069] Fig.12 : (a) Thermal conductivity of the graphene film obtained in Example 9; (b) Thermal conductivity of the graphene film obtained in Comparative Example 4.
[0070] Fig.13 : (a) Thermal conductivity of the graphene film obtained in Example 10; (b) Thermal conductivity of the graphene film obtained in Comparative Example 4. DETAILED DESCRIPTION
[0071] The present invention is further described below in conjunction with specific embodiments, but the embodiments of the present invention are not limited thereto.
[0072] Example 1, Comparative Example 1
[0073] 1. Sample preparation
[0074] (1) The sample of Example 1 was prepared according to the following steps:
[0075] Step 1: Under ethylene protection, anhydrous solvent (dichloromethane, 20.0 mL) and functional monomer (its structural formula is shown in the attached Figure 1, 1.6g / 6.0mmol, feed concentration is 0.30M) is added into a 100mL Schlenk bottle, stirred for 10min to form a uniform solution and kept at a constant temperature of 25°C; then 0.20g of catalyst (α-diimine palladium catalyst 1, feed concentration is 10.0g / L) is added, and the polymerization is continuously stirred for 24h at an ethylene pressure of 0.1MPa and 25°C; after the reaction, the solvent is purged by air to remove the solvent, and the obtained product is dissolved in a small amount of THF. After adding a few drops of HCl and H2O2 solution, the residual palladium particles are removed by stirring, and the solvent is purged again. The obtained product is dissolved in a small amount of THF and precipitated by methanol. The process is repeated 2 to 3 times. The obtained product is vacuum dried at 60°C for 24h to obtain a hyperbranched macromolecular initiator (HBPE@Br, 2.3g).
[0076] Furthermore, under nitrogen protection, 0.10 g HBPE@Br (containing 0.069 mmol Br), 12.3 g functional monomer (hexadecyl acrylate, HDA, 41.4 mmol) and 12.3 mL anhydrous grade toluene were added into a 250 mL Schlenk bottle in sequence and stirred at room temperature to form a uniform solution; then 47.8 mg ligand PMDETA (0.276 mmol) was added, stirred for 0.5 h and then freeze-thawed for 3 times to remove residual oxygen; then the temperature was raised to 75 °C, 19.8 mg catalyst CuBr (0.138 mmol) was added and the polymerization was continued with stirring for 1 h; after the polymerization was completed, the solvent was removed by air blowing, the obtained product was dissolved in a small amount of THF, methanol was added for precipitation, and the process was repeated 2 to 3 times, and the product was vacuum dried at 60 °C for 24 h to obtain a crystalline hyperbranched multi-arm copolymer (HBPE@PHDA, about 0.5 g). ([-Br]:[HDA]:[PMDETA]:[CuBr]=1:600:4:2)
[0077] Step 2: In a 100 mL cylindrical glass bottle, graphite powder (natural flake graphite, 640 mg), HBPE@PHDA (80 mg) and solvent (chloroform, 80 mL) were added in sequence (the initial concentration of graphite powder was 8 mg / mL, and the polymer / graphite mass ratio was 0.125). After sealing, it was placed in an ultrasonic tank (KQ-250V, output power 250 W) and continuously ultrasonicated for 48 hours at room temperature. The obtained product was centrifuged at 4000 rpm for 45 minutes to remove unpeeled graphite particles. About 70 mL of the upper clear liquid was carefully collected to obtain the graphene initial dispersion. The above process was repeated to obtain a large volume of graphene initial dispersion. An appropriate amount was taken from it and vacuum filtered using a 0.20 μm nylon membrane, and washed with chloroform solvent. The number of washings was controlled to regulate the residual proportion of the polymer in the graphene film. After drying at room temperature, a self-supporting graphene film sample I (thickness of about 75.0 μm) with a graphene ratio of 75 wt% was obtained, which was recorded as GH75.
[0078] (2) Comparative Example 1
[0079] HBPE@Br was obtained according to step 1 of Example 1, and a graphene film sample was obtained according to step 2 of Example 1 by replacing HBPE@PHDA with HBPE@Br.
[0080] 2. Characterization and testing
[0081] Differential scanning calorimetry (DSC) analysis was performed using a DSC214 differential scanning calorimeter (Netzsch, Germany) in a nitrogen atmosphere. The sample size was 5–10 mg. The sample was first heated from room temperature to 100 °C at a rate of 10 °C min-1 and kept constant for 3 min to eliminate the thermal history. The sample was then cooled to -20 °C at the same rate and the cooling curve was recorded. The sample was then heated from room temperature to 100 °C at the same rate and the heating curve was recorded. Polarizing microscope (POM) images were recorded using a BX53M-P hot stage polarizing microscope (Olympus, Japan). The sample was placed on the hot stage surface via a glass slide. The sample was first heated from room temperature to 60 °C at a constant rate and then cooled to room temperature at the same rate. The camera took pictures at an interval of 1 s. Scanning electron microscope (SEM) images were taken using a Nano Nova The graphene film was obtained by a 450 field emission scanning electron microscope (FEI, USA), and the test sample was obtained by brittle fracture after liquid nitrogen freezing; the stress-strain curve of the graphene film was obtained by testing with an A-7000-SU1 electronic universal material testing machine (Guangzhou High-speed Railway Testing Instrument Co., Ltd.), with a stretching rate of 1mm / min, a clamp spacing of 10mm, a test temperature of room temperature, and sample specifications: length 30mm, width 10mm, thickness 50μm; the electrothermal properties of the graphene film were evaluated by using an infrared thermometer to test the change of the film surface temperature with heating time under a DC voltage.
[0082] 3. Comparison and analysis of test results
[0083] like Figure 2 (a) and (b) show that there is an obvious endothermic / exothermic phenomenon on the DSC curve of HBPE@PHDA (Example 1), indicating that the hyperbranched multi-arm copolymer has a strong crystallization ability. Figure 2 The melting heat data (126.8 J / g) of the sample HBPE@PHDA (Example 1) measured in (b) combined with the melting heat data (166.5 J / g) of the compound HAD show that the crystallinity of the sample HBPE@PHDA is 76.2%. However, there is no endothermic / exothermic phenomenon on the DSC curve of HBPE@Br (Comparative Example 1), indicating that the hyperbranched macromolecular initiator does not have the ability to crystallize. This is because the polyhexadecyl acrylate PHDA with crystallization ability is introduced into the HBPE structure. Figure 2 (c) further gives polarizing microscope photos of the above HBPE@PHDA sample at 25 and 40°C, which shows that the sample has an obvious spherulite structure at room temperature, while the crystalline structure disappears due to melting at higher temperatures, which once again confirms that the sample has a strong crystallization ability.
[0084] Figure 3 (a) and (b) respectively show the appearance of the graphene films prepared in Comparative Example 1 and Example 1. As shown in the figure, the mechanical strength of the graphene film obtained in Comparative Example 1 is very poor and it cannot exist independently. It can only exist under the support of the filter membrane, while the graphene film obtained in Example 1 can be peeled off from the surface of the filter membrane and exists as a self-supporting film, showing significantly improved mechanical strength and excellent flexibility. This is because in the film structure obtained in Example 1, the crystalline hyperbranched multi-arm copolymer HBPE@PHDA adsorbed on the graphene surface effectively promotes the close stacking and assembly of the graphene sheets in the system through mutual crystallization and entanglement, thereby forming a macroscopic film of a certain strength. This can be seen from Figure 3 The SEM results of the sample shown in (c)-(e) were confirmed. Figure 3 (f) shows the stress-strain curve of the graphene film prepared in Example 1, which shows that the tensile strength of the film is 3.0 MPa and the elongation at break is approximately 2%, which once again confirms that the graphene film obtained in Example 1 has significantly improved mechanical strength.
[0085] Figure 4 (a) shows the electrothermal heating / cooling curves of the film obtained in Example 1 under different driving voltages. The figure shows that the film can reach a steady-state temperature in a relatively short time (about 30s), and its steady-state temperatures can reach 31.6, 43.5 and 58.5°C for driving voltages of 6, 9 and 10V, respectively, indicating that the graphene film has an excellent electrothermal response rate and an adjustable steady-state temperature, indicating that it has excellent electrothermal performance. Figure 4 (b) shows the infrared thermal images of the film at different heating times at 10V, showing that different parts of the film have uniform heating performance. The above results comprehensively show that: compared with Comparative Example 1, in Example 1, by introducing PHDA side chains with crystallization ability into the HBPE structure, the mechanical strength of the graphene film prepared is significantly improved, and at the same time, excellent electrothermal performance is shown.
[0086] Example 2, Comparative Example 2
[0087] 1. Sample preparation
[0088] (1) The sample of Example 2 was prepared according to the following steps:
[0089] Step 1: proceed with reference to Step 1 in Example 1. The difference is that the functional monomer hexadecyl acrylate is replaced by octadecyl acrylate.
[0090] Step 2: proceed as per step 2 in Example 1.
[0091] (2) The sample of Comparative Example 2 was prepared according to the following steps:
[0092] The above-mentioned Example 1 was referred to, and the obtained graphene film sample was used as Comparative Example 2.
[0093] 2. Characterization and testing
[0094] Refer to the method described in the above-mentioned Example 1 and Comparative Example 1.
[0095] 3. Comparison and analysis of test results
[0096] Figure 5 The electrothermal heating / cooling curves of the samples of Example 2 and Comparative Example 2 were compared, and the test was performed at a voltage of 9V. As shown in the figure, the electrothermal performance of the two samples is basically similar: the steady-state temperature is basically around 45°C, and the steady-state temperature can be reached in about 20 seconds. This shows that in the process of synthesizing the hyperbranched multi-arm copolymer, octadecyl acrylate is used instead of hexadecyl acrylate, and a graphene film with excellent electrothermal performance can also be prepared by the method of the present invention.
[0097] Example 3, Comparative Example 2
[0098] 1. Sample preparation
[0099] (1) The sample of Example 3 was prepared according to the following steps:
[0100] Step 1: proceed as in Step 1 of Example 1, except that the monomer feed ratio ([-Br]:[HDA]:[PMDETA]:[CuBr]) was adjusted from 1:600:4:2 to 1:400:4:2.
[0101] Step 2: proceed as per step 2 in Example 1.
[0102] (2) The sample of Comparative Example 2 was prepared according to the following steps:
[0103] The above-mentioned Example 1 was referred to, and the obtained graphene film sample was used as Comparative Example 2.
[0104] 2. Characterization and testing
[0105] Refer to the method described in the above-mentioned Example 1 and Comparative Example 1.
[0106] 3. Comparison and analysis of test results
[0107] Figure 6 The electrothermal conversion performance of the samples of Example 3 and Comparative Example 2 was compared (driving voltage was 9V). As shown in the figure, the sample of Example 3 can reach a steady-state temperature of 42°C in about 30s, and can quickly recover to room temperature within 20s after the voltage is cut off, indicating that it has excellent electrothermal conversion performance. By comparing with Comparative Example 2, it can be found that the electrothermal conversion performance of the sample of Example 3 is basically close to that of Comparative Example 2. This shows that in the process of synthesizing hyperbranched multi-arm copolymers, the monomer feed ratio can be adjusted, and a graphene film with excellent electrothermal performance can be obtained by the method described in the present invention within a reasonable ratio range.
[0108] Example 4, Comparative Example 2
[0109] 1. Sample preparation
[0110] (1) The sample of Example 4 was prepared according to the following steps:
[0111] Step 1: proceed as per step 1 in Example 1.
[0112] Step 2: refer to step 2 in Example 1. The difference is that the solvent H used in ultrasound is replaced by THF instead of chloroform; the initial concentration of graphite powder is changed from 8 mg / mL to 15 mg / mL, and the polymer / graphite mass ratio is changed from 0.125 to 0.20.
[0113] (2) The sample of Comparative Example 2 was prepared according to the following steps:
[0114] The above-mentioned Example 1 was referred to, and the obtained graphene film sample was used as Comparative Example 2.
[0115] 2. Characterization and testing
[0116] Refer to the method described in the above-mentioned Example 1 and Comparative Example 1.
[0117] 3. Comparison and analysis of test results
[0118] Figure 7 The electrothermal conversion performance of the samples of Example 4 and Comparative Example 2 (driving voltage is 9V) is compared. The results in the figure show that the steady-state temperatures of the samples of Example 4 and Comparative Example 2 can reach approximately 50 and 45°C, respectively, and the heating rates are close to about 5.0°C / s, indicating that both samples have fast electrothermal conversion capabilities despite the lower driving voltage (only 9V), which can meet the application requirements of health therapy, etc. This shows that in the graphene film preparation process described in the present invention, by adjusting the type of graphene liquid phase exfoliation solvent and the ultrasonic initial feed ratio, within the ratio range provided by the present invention, a graphene electrothermal film with better performance can be obtained.
[0119] Example 5, Comparative Example 2
[0120] 1. Sample preparation
[0121] (1) The sample of Example 5 was prepared according to the following steps:
[0122] Step 1: proceed as per step 1 in Example 1.
[0123] Step 2: proceed as in Step 2 of Example 1. The difference is that the 0.20 μm nylon membrane used for filtration is replaced by a PTFE membrane with a pore size of 0.10 μm; the mass percentage of polymer in the obtained graphene film is replaced from 75% to 60%. (2) The sample of Comparative Example 2 is prepared as follows:
[0124] The above-mentioned Example 1 was referred to, and the obtained graphene film sample was used as Comparative Example 2.
[0125] 2. Characterization and testing
[0126] Refer to the method described in the above-mentioned Example 1 and Comparative Example 1.
[0127] 3. Comparison and analysis of test results
[0128] Figure 8 The electrothermal conversion performance (driving voltage is 10V) and mechanical strength of the samples of Example 5 and Comparative Example 2 are compared. The results in the figure show that the steady-state temperature of the samples of Example 5 and Comparative Example 2 can reach approximately 60°C, and the heating rate is close to about 5.0°C / s, indicating that both samples have rapid electrothermal conversion capabilities despite being at a relatively low driving voltage (only 10V), and can meet application requirements such as rapid ambient temperature and energy-saving regulation. This shows that according to the specifications and types of the filter membrane provided by the present invention, a graphene film with relatively good mechanical strength and electrothermal conversion performance can be successfully prepared according to the method.
[0129] Example 6, Comparative Example 3
[0130] 1. Sample preparation
[0131] (1) The preparation of the graphene film sample of Example 6 is the same as that of Example 1.
[0132] (2) The preparation of the graphene film sample of Comparative Example 3 is the same as that of Comparative Example 1.
[0133] 2. Characterization and testing
[0134] The stress-strain curve of the graphene film was obtained by testing with an A-7000-SU1 electronic universal material testing machine (Guangzhou High-speed Railway Testing Instrument Co., Ltd.), with a tensile rate of 1 mm / min, a clamp spacing of 10 mm, a test temperature of room temperature, and sample specifications: length 30 mm, width 10 mm, thickness 50 μm; the thermal conductivity (λ) of the graphene film was tested according to formula (1):
[0135] λ=α×ρ×C P (1)
[0136] Wherein, α is the thermal diffusion coefficient, which is measured by LFA-467 laser thermal conductivity meter (Netzsch, Germany). The test sample is a disc sample with a diameter of 12.5 mm (vertical direction test) or 25 mm (horizontal direction test) and a thickness of about 75-80 μm; ρ is the sample density, which is measured by ME 204 densitometer (Mettler Toledo, Switzerland). The sample is a 1 cm × 1 cm square sheet; C P The specific heat of the sample was measured by DSC214 differential scanning calorimeter. 5-10 mg of sample powder was taken under N2 protection at a heating rate of 10 °C min -1 The test was conducted by heating from 0°C to 60°C.
[0137] The shape memory property of the graphene film was tested by the following steps: the sample was first heat treated in an oven at 75°C for 10 min, then bent into a "U" shape, and further kept in this shape for 15 min under the action of an external force at room temperature. The external force was then removed, and the sample was placed on a heating table. The shape of the sample was recorded using an infrared thermal camera. At this time, the bending angle of the sample was the initial angle (θ1). The heating table was turned on and heated from 30°C to 50°C at a constant heating rate to restore the shape of the sample. The sample shape was continuously photographed, the recovery angle (θ2) was recorded, and the shape recovery rate (R) of the film was calculated according to formula (2). r ):
[0138]
[0139] 3. Comparison and analysis of test results
[0140] like Fig. 9 (a) shows that the graphene film prepared by Example 6 can be directly removed from the surface of the filter membrane and exists as a self-supporting film, showing excellent bendability. Fig. 9 As shown in (b), the tensile strength of the film can reach 3.0MPa; Fig. 9 (c) shows that the graphene thermal conductive film prepared by Comparative Example 3 can only be attached to the surface of the filter membrane, showing low mechanical strength, so that it is difficult to exist independently. Fig. 9(d) shows that the in-plane thermal conductivity of the graphene film obtained in Example 6 can reach 37.0 W m -1 K -1 , showing excellent in-plane thermal conductivity, while its vertical thermal conductivity is only 1.0 W m -1 K -1 , showing that the film has outstanding anisotropic thermal conductivity, with an anisotropic thermal conductivity ratio of 37. In addition, Fig. 9 (e) shows the shape memory recovery process of the sample in Example 6. The sample can be bent into any shape at 75°C, and can maintain a stable shape after cooling. It can be quickly restored to shape within 40 seconds after further treatment at 80°C, and the shape recovery rate is close to 100%, indicating that it has an outstanding shape memory function. In summary, the above results collectively show that a multifunctional graphene film with excellent flexibility, strength, shape memory and anisotropic thermal conductivity can be successfully prepared by referring to the process steps described in Example 6.
[0141] Example 7, Comparative Example 3
[0142] 1. Sample preparation
[0143] (1) The sample of Example 7 was prepared according to the following steps:
[0144] Step 1: proceed as per Step 1 in Example 6.
[0145] Step 2: refer to step 2 in Example 6. The difference is that the mass percentage of the polymer in the obtained composite film is adjusted from the original 75% to 60% by controlling different washing times in the suction filtration step.
[0146] (2) The sample of Comparative Example 3 was prepared according to the following steps:
[0147] Refer to the above-mentioned Comparative Example 3.
[0148] 2. Characterization and testing
[0149] Refer to the method described in the aforementioned Example 6 and Comparative Example 3.
[0150] 3. Comparison and analysis of test results
[0151] Fig.10 (a) compares the in-plane and perpendicular thermal conductivity data of the sample obtained in Example 7, which are 29.4 and 0.8 W m -1 K -1 , the anisotropy ratio reaches 36.75, indicating that the sample has excellent in-plane thermal conductivity and outstanding anisotropic thermal conductivity characteristics. Fig.10 (b) gives the method for evaluating the vertical heat transfer performance of the sample obtained in Example 7, and the relevant data results are summarized in Fig.10(c); As the test time increases, the sample surface temperature gradually increases. When the test time is 55s, the film surface temperature can reach nearly 55°C, indicating that it has certain vertical heat transfer performance. Fig.10 (d) gives the evaluation method of the heat transfer performance of the graphene composite film obtained in Example 7 in the in-plane direction, and the infrared thermal images of the sample surface at each test time are shown in FIG. Fig.10 (e)-(g); The figure shows that the surface temperature of the obtained graphene thermal conductive film can reach 53.5°C in only about 4s of testing time, indicating that it has excellent in-plane thermal conductivity and significant anisotropic thermal conductivity. In addition, compared with the sample in Comparative Example 3, the graphene film obtained in Example 7 has better mechanical strength and can exist independently in the form of a self-supporting film; it also exhibits excellent shape memory function. The above results show that a graphene film with both shape memory and anisotropic thermal conductivity can be obtained by the method described in Example 7.
[0152] Example 8, Comparative Example 4
[0153] 1. Sample preparation
[0154] (1) The sample of Example 8 was prepared according to the following steps:
[0155] Step 1: proceed as in Step 1 of Example 6, except that the monomer feed ratio ([-Br]:[HDA]:[PMDETA]:[CuBr]) was adjusted from 1:600:4:2 to 1:400:4:2.
[0156] Step 2: proceed as per Step 2 in Example 6.
[0157] (2) The sample of Comparative Example 4 was prepared according to the following steps:
[0158] Refer to the above-mentioned Example 6.
[0159] 2. Characterization and testing
[0160] Refer to the method described in the aforementioned Example 6 and Comparative Example 3.
[0161] 3. Comparison and analysis of test results
[0162] Fig.11The heat dissipation application performance of the graphene film obtained in Example 8 on the mobile phone was investigated. As shown in the figure, without using the graphene film, as the charging time of the mobile phone increases, the surface temperature of the back of the mobile phone increases significantly. The corresponding charging time is 30 minutes, and the temperature reaches 43.1°C, which is 14.9°C higher than the initial temperature; and after using the graphene film described in Example 8, the corresponding surface temperature of the mobile phone is 32.8°C, which is only 3.5°C higher than the initial temperature, indicating that the graphene film has excellent in-plane heat dissipation function. In addition, similar to the aforementioned Examples 6 and 7, the graphene thermal conductive film obtained in Example 8 here can also exist as a self-supporting film form, and has significantly improved mechanical strength compared with Comparative Example 3, and maintains good flexibility; at the same time, it shows excellent shape memory function, and its shape recovery rate can be restored to 100% within 30s when treated above 80°C.
[0163] Example 9, Comparative Example 4
[0164] 1. Sample preparation
[0165] (1) The sample of Example 9 was prepared by referring to the above Example 6, except that the solvent H used for liquid phase stripping in step 2 was replaced by THF instead of chloroform.
[0166] (2) The sample of Comparative Example 4 was prepared by referring to the above-mentioned Example 6.
[0167] 2. Characterization and testing
[0168] Refer to the method described in the aforementioned Example 6 and Comparative Example 3.
[0169] 3. Comparison and analysis of test results
[0170] Fig.12 The thermal conductivity of the graphene film obtained in Example 9 and Comparative Example 4 was compared. Fig.12 (a) corresponds to the result of the film obtained in Example 9. This sample was prepared by liquid phase exfoliation in THF and its in-plane thermal conductivity was as high as 29.0 W m -1 K -1 , and the vertical thermal conductivity is 0.85 W m -1 K -1 , the anisotropy ratio is 34.11, indicating that the sample also has excellent anisotropic thermal conductivity. Fig.12 (b) corresponds to the graphene film obtained in Comparative Example 4, which is prepared by liquid phase exfoliation in chloroform. The in-plane and out-of-plane thermal conductivities of this sample are 37 and 1.0 W m -1 K -1, the anisotropy ratio is 37, which is generally close to the result of Example 9. In addition, the samples of Example 9 and Comparative Example 4 both exhibit shape memory function, excellent flexibility and mechanical strength. The above results show that in the process of preparing the graphene film, the solvent for liquid phase exfoliation can be selected from a variety of different types of solvents, among which THF is also one of the effective solvents.
[0171] Example 10, Comparative Example 4
[0172] 1. Sample preparation
[0173] (1) The sample of Example 10 was prepared according to the following steps:
[0174] Step 1: Refer to the sample preparation step (1) in Example 6.
[0175] Step 2: refer to the sample preparation step (2) in Example 6. The difference is that the 0.20 μm nylon membrane used for filtration is replaced by a PTFE membrane with a pore size of 0.10 μm.
[0176] (2) The sample of Comparative Example 4 was prepared according to the following steps:
[0177] Refer to the above-mentioned Example 6 and the obtained graphene film sample is used as Comparative Example 4.
[0178] 2. Characterization and testing
[0179] Refer to the method described in the aforementioned Example 6 and Comparative Example 3.
[0180] 3. Comparison and analysis of test results
[0181] Fig.13 The thermal conductivity of the graphene thermal conductive film obtained in Example 10 and Comparative Example 4 was compared. The preparation steps and processes of the two samples were the same, except that the specifications of the filter membranes used in the preparation of the graphene membranes were different. Example 10 used a 0.1 μm PTFE membrane, while Comparative Example 4 used a 0.2 μm nylon membrane. Fig.13 (a) shows the in-plane and perpendicular thermal conductivities of the graphene thermally conductive film obtained in Example 10, which are 32.4 and 1.05 W m -1 K -1 , the anisotropy ratio is 30.9, indicating that it has excellent anisotropic thermal conductivity; this result is generally close to the sample obtained in Comparative Example 4. In addition, the membranes obtained in Example 10 and Comparative Example 4 can both exist as self-supporting membranes and have stable shape memory functions. The above results show that the two types of membranes can be used to prepare graphene thermal conductive membranes with both anisotropic thermal conductivity and shape memory functions according to the method described in the present invention.
Claims
1. A crystalline hyperbranched multi-arm copolymer, characterized in that: The crystalline hyperbranched multi-arm copolymer is prepared by the following method: using an α-diimine palladium catalyst to catalyze the copolymerization of ethylene and a bromine-containing functional monomer in an anhydrous solvent in a one-step "chain removal" process to obtain a hyperbranched macromolecular initiator; then using the hyperbranched macromolecular initiator to initiate an atom transfer free radical polymerization of an acrylate functional monomer to obtain a crystalline hyperbranched multi-arm copolymer; The structure of the bromine-containing functional monomer is shown below: The acrylic acid ester functional monomer is selected from one of the following compounds: hexadecyl acrylate, tetradecyl acrylate, octadecyl acrylate, and behenyl acrylate.
2. The crystalline hyperbranched multi-arm copolymer according to claim 1, characterized in that: The α-diimine palladium catalyst is selected from the α-diimine palladium catalyst 1 or 2 whose structure is shown below: The anhydrous solvent is selected from one of the following: dichloromethane, chlorobenzene, and chloroform.
3. The crystalline hyperbranched multi-arm copolymer according to claim 1 or 2, characterized in that: In the one-step "chain removal" copolymerization system, the feed concentration of the α-diimine palladium catalyst is 0.5-50 g / L, preferably 2-20 g / L, based on the total volume of the anhydrous solvent, and the feed concentration of the bromine-containing functional monomer is 0.05-10 M, preferably 0.1-2 M, based on the total volume of the anhydrous solvent.
4. The crystalline hyperbranched multi-arm copolymer according to claim 1, characterized in that: The temperature of the one-step "chain removal" copolymerization is 5 to 35° C., preferably 15 to 25° C.; the ethylene pressure is 0.05 to 0.5 MPa, preferably 0.1 MPa; and the copolymerization time is 0.5 to 48 h, preferably 2 to 24 h.
5. The crystalline hyperbranched multi-arm copolymer according to claim 1, characterized in that: The atom transfer radical polymerization is specifically as follows: under the protection of inert gas, a hyperbranched macromolecular initiator, an acrylate functional monomer, anhydrous toluene as a solvent, pentamethyldiethylenetriamine or 2,2'-bipyridine as a ligand, and cuprous bromide as a catalyst are added into a reaction container, and after the addition, atom transfer radical polymerization is carried out. The polymerization temperature of the atom transfer radical polymerization is controlled at 45 to 100° C., and the reaction time is controlled at 0.5 to 24 hours. After the polymerization is completed, a crystalline hyperbranched multi-arm copolymer is obtained through separation and purification. The feed concentration of the hyperbranched macromolecular initiator in the polymerization system is 0.001 to 0.1 mol / L based on the molar concentration of the bromine groups contained therein, and the initial feed molar concentration ratio of the hyperbranched macromolecular initiator, the acrylate functional monomer, the ligand, and the catalyst is 1:200 to 800:0.5 to 4:0.5 to 2.
6. The crystalline hyperbranched multi-arm copolymer according to claim 1, characterized in that: The crystallinity of the crystalline hyperbranched multi-arm copolymer is 30-80%, preferably 70-80%.
7. A method for preparing a self-supporting graphene film, characterized in that: The preparation method comprises the following steps: The crystalline hyperbranched multi-arm copolymer according to any one of claims 1 to 6, graphite powder and solvent are mixed in proportion, and an initial graphene dispersion is obtained by ultrasonic and centrifugal separation, and then a self-supporting graphene film is obtained by filtering, eluting and drying in sequence.
8. The preparation method according to claim 7, characterized in that: In the self-supporting graphene film, the content of the crystalline hyperbranched multi-arm copolymer is controlled to be 5 to 50% by mass, preferably 20 to 40% by mass.
9. A self-supporting graphene film obtained according to the preparation method of claim 7 or 8.
10. Use of the self-supporting graphene film as claimed in claim 9 as an electric heating film.
Citation Information
Patent Citations
Star poly-(methyl)acrylate long-chain ester polymer and preparation method thereof
CN101691417A
Hyperbranched elastic material capable of self-healing and preparation method thereof
CN103333346A
Soluble brown star type fluorescent polymer and preparation method thereof
CN107814947A
Method for preparing graphene powder and dispersion thereof from fluorine-containing hyperbranched polyethylene copolymers
CN108373148A
Pyrenylated terpolymer, and intermediate, preparation method and application thereof
CN111647113A