Poly (dimethyl diphenyl imide) siloxane / phenolic aldehyde-based dual-network hybrid resin as well as preparation method and application of poly (dimethyl diphenyl imide) siloxane / phenolic aldehyde-based dual-network hybrid resin

By imidizing the copolymer of poly(dimethyldiphenimide)siloxane and phenolic binet hybrid resin with phenolic resin, the problem of poor interface compatibility between ceramic fillers and resin is solved, and the problem of poor interfacial compatibility between ceramic fillers and resin is achieved. High-performance ablation protection in harsh environments improves the ablation resistance of the resin.

CN118994575AActive Publication Date: 2024-11-22SICHUAN UNIV

Patent Information

Application Number
CN202310550984.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-22
Estimated Expiration
2043-05-16

AI Technical Summary

Technical Problem

Traditional phenolic resins are difficult to meet high performance requirements in harsh environments. The poor compatibility of ceramic fillers and resins with resins leads to limited improvement in ablation performance. The introduced polysiloxanes have low or high molecular weights and bite reactions and phases. Separation problem.

Method used

Using poly(dimethyldiphenimide)siloxane and phenolic binet hybrid resin, through PMP, 3,3',4,4'-biphenyltetracarboxylic acid dianhydride and (3-aminopropyl The triethoxysilane is used as a raw material and synthesized through anionic ring-opening polymerization to form a copolymer and imidized with a phenolic resin to prepare a hybrid resin with a dual network structure.

Benefits of technology

The good compatibility between copolymer and phenolic resin is achieved. The resin is graphitized and ceramicized during the ablation process, which significantly improves the ablation resistance. The generated SiO2 liquid film has high viscosity and radiation heat dissipation ability, which enhances the The mechanical erosion and oxygen isolation capability of oxyacetylene flame.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994575A_ABST
    Figure CN118994575A_ABST
Patent Text Reader

Abstract

The invention provides poly (dimethyl diphenylimide) siloxane / phenolic aldehyde-based dual-network hybrid resin as well as a preparation method and application thereof, and belongs to the technical field of advanced materials. The invention firstly provides a copolymer for preparing ablation thermal protection hybrid resin. The structure of the copolymer is shown as a formula I in the specification. A hybrid resin prepared with the copolymer is then provided. According to the hybrid resin disclosed by the invention, the copolymer shown in the formula I and the phenolic resin have good compatibility, and the copolymer is uniformly distributed in the phenolic resin; and the hybrid resin is graphitized and ceramized in the ablation process, and has excellent ablation resistance. The invention provides a thought and a method for preparing the novel ablation-resistant hybrid phenolic resin through copolymerization, and the novel ablation-resistant hybrid resin which is expected to meet the increasingly stringent flight environment in the future is prepared. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of advanced materials, and specifically relates to a poly(dimethylbenzimide)siloxane / phenolic double network hybrid resin and a preparation method and application thereof. Background Art

[0002] As countries around the world become more interested in space exploration, the environment in which spacecraft are used is becoming more and more harsh, which has accelerated the development of new materials for spacecraft with higher performance and capable of coping with extreme conditions. When a spacecraft enters the atmosphere, the shock wave between the external gas and the surface of the spacecraft will generate a very serious heat load. At this time, a thermal protection system (TPS) is needed to protect the spacecraft from the effects of the heat load. Phenolic resin (PR) is the most widely used TPS material to date, but as the service environment becomes increasingly harsh, traditional phenolic resin is no longer competent and urgently needs to be modified to meet more demanding environments.

[0003] Ceramic fillers undergo complex endothermic reactions during the ablation process to generate a protective ceramic layer that resists the erosion of heat flow. Therefore, ceramic fillers such as SiC, POSS, ZrSi2, ZrB2, etc. are often introduced into PR. Wang (Wang S, Huang H, Tian Y, et al. Effects of SiC content on mechanical, thermal and ablative properties of carbon / phenolic composites[J]. Ceramics International, 2020, 46(10): 16151-16156.) tried to introduce SiC into PR and found that during the ablation process, SiC can form a SiO2 liquid protective film, thereby reducing the linear ablation rate of the material. Ding (Ding J, Yang T, Huang Z, et al. Thermal stability and ablation resistance, and ablation mechanism of carbon-phenolic composites with different zirconium silicide particle loadings [J]. Composites Part B: Engineering, 2018, 154: 313-320.) et al. found that the introduced ZrSi2 can form a SiO2-ZrO2 ceramic protective layer covering the ablation surface of the composite material. However, the interface compatibility between the introduced ceramic filler and PR is poor, making it difficult to disperse evenly, and the ceramic filler is easy to agglomerate in the PR matrix, which is undoubtedly unfavorable for further improving the ablation performance of the material.

[0004] In order to avoid the occurrence of agglomeration, researchers are now shifting their attention to introducing ceramic elements such as B, Si, Zr, etc. into the PR matrix through chemical bonding. During the ablation process, organic silicon will undergo a complex ceramicization reaction to generate high-temperature ceramics such as SiO2 and SiC, which greatly improves the ablation resistance of the material. Therefore, it has attracted the attention of more and more researchers. For example, Li (Li S, Han Y, Chen F, et al. The effect of structure on thermal stability and anti-oxidation mechanism of silicone modified phenolic resin [J]. Polymer Degradation and Stability, 2016, 124: 68-76.) and others introduced silanes of different polymerization degrees into PR through Si-O-ph bonds to prepare uniformly dispersed organic silicon / phenolic hybrid resins with greatly improved thermal residual weight at 800 ° C. However, these introduced polysiloxanes have a low molecular weight (Mn is only a few hundred g·mol -1 ), they will produce a backbiting reaction during the ablation process, producing a large amount of volatile and flammable cyclic siloxanes, which are not only not conducive to the occurrence of ceramic reaction, but also destroy the integrity of the carbon layer, resulting in a decrease in ablation resistance. The higher molecular weight silicone resin has poor compatibility with PR, and the hybrid resin will undergo phase separation, which has an adverse effect on the ablation performance. Therefore, how to balance high molecular weight and good compatibility is a key to the current preparation of high-performance hybrid resins. Summary of the invention

[0005] In order to solve the problems existing in the prior art, the present invention provides a poly(dimethylbenzimide)siloxane / phenolic double network hybrid resin and a preparation method and use thereof.

[0006] The present invention provides a copolymer for preparing an ablative heat protection hybrid resin, the structure of which is shown in Formula I:

[0007]

[0008] Wherein, x is selected from an integer of 0 to 6;

[0009] y is selected from an integer of 3 to 18;

[0010] z is selected from integers of 3-24.

[0011] Further,

[0012] x is an integer selected from 1 to 2;

[0013] y is selected from an integer of 7 to 10;

[0014] z is selected from integers of 8-12.

[0015] Furthermore, the aforementioned copolymer is prepared from PMP, 3,3',4,4'-biphenyltetracarboxylic dianhydride and (3-aminopropyl)triethoxysilane as raw materials;

[0016] The PMP is synthesized by using octaphenylcyclotetrasiloxane, octamethylcyclotetrasiloxane and 1,3-bis(3-aminopropyl)tetramethyldisiloxane as raw materials through anionic ring-opening polymerization.

[0017] Further,

[0018] The molar ratio of the amino group in the PMP to the anhydride in 3,3',4,4'-biphenyltetracarboxylic dianhydride is 1:1 to 1.1;

[0019] The (3-aminopropyl)triethoxysilane is 0 to 40 mol% of the amino content in PMP;

[0020] Preferably,

[0021] The (3-aminopropyl)triethoxysilane is 20-40 mol% of the amino group content in PMP.

[0022] Further,

[0023] The molar ratio of octaphenylcyclotetrasiloxane, octamethylcyclotetrasiloxane and 1,3-bis(3-aminopropyl)tetramethyldisiloxane is 0-6:2-12:0-4;

[0024] Preferably, the molar ratio of octaphenylcyclotetrasiloxane, octamethylcyclotetrasiloxane and 1,3-bis(3-aminopropyl)tetramethyldisiloxane is 0.5-3:7-10:1-3;

[0025] More preferably, the molar ratio of octaphenylcyclotetrasiloxane, octamethylcyclotetrasiloxane and 1,3-bis(3-aminopropyl)tetramethyldisiloxane is 0.5-3:7-9.5:2;

[0026] More preferably, the molar ratio of octaphenylcyclotetrasiloxane, octamethylcyclotetrasiloxane and 1,3-bis(3-aminopropyl)tetramethyldisiloxane is 1.5:8.5:2.

[0027] Furthermore, the preparation method of the PMP comprises the following steps:

[0028] Octaphenylcyclotetrasiloxane, octamethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)tetramethyldisiloxane and a catalyst are mixed, nitrogen is introduced, and the mixture is reacted to obtain the product;

[0029] Preferably, the catalyst is selected from tetramethylammonium hydroxide;

[0030] And / or, vacuuming is performed before introducing nitrogen;

[0031] And / or, the reaction is carried out at 100-120° C. for 1-5 hours, and then the temperature is raised to 150-200° C. and maintained for 0.5-5 hours;

[0032] More preferably, the mass of the catalyst is 0.5-5 wt % of the total mass of octaphenylcyclotetrasiloxane and octamethylcyclotetrasiloxane.

[0033] The present invention also provides a method for preparing the aforementioned copolymer, which comprises the following steps:

[0034] (1) In a solvent, 3,3',4,4'-biphenyltetracarboxylic dianhydride and PMP are mixed and reacted;

[0035] (2) adding (3-aminopropyl)triethoxysilane and continuing the reaction to obtain;

[0036] Preferably,

[0037] In step (1), the solvent is tetrahydrofuran;

[0038] And / or, in step (1), the reaction temperature is 30 to 50° C., and the reaction time is 1 to 5 hours;

[0039] And / or, in step (2), the reaction temperature is 30 to 50° C., and the reaction time is 1 to 5 hours;

[0040] More preferably,

[0041] In step (1), the mass ratio of the solvent to PMP is (1-5):1.

[0042] The present invention also provides the use of the aforementioned copolymer and resin as raw materials in the preparation of ablative heat protection hybrid resin;

[0043] Preferably, the resin is a phenolic resin.

[0044] The present invention also provides an ablative heat protection hybrid resin, which is prepared by mixing the aforementioned copolymer with a resin, and then curing and imidizing the mixture;

[0045] Preferably, the mass ratio of the copolymer to the resin is 1:1 to 5;

[0046] And / or, the reaction is carried out in a solvent;

[0047] And / or, the reaction temperature is 80-100°C; the reaction time is 1-10h;

[0048] And / or, the curing and imidization procedures are sequentially maintained at 100-120° C. for 0.1-1 h, 130-170° C. for 1-5 h, 180-190° C. for 1-5 h, and 200-220° C. for 1-5 h;

[0049] More preferably, the resin is a phenolic resin;

[0050] And / or, the mass ratio of the copolymer to the resin is 1:2;

[0051] And / or, the solvent is anhydrous ethanol;

[0052] And / or, the solvent is removed by vacuuming before curing and imidization;

[0053] And / or, the curing and imidization procedures are sequentially maintained at 120° C. for 0.5 h, 160° C. for 1 h, 180° C. for 1 h, and 200° C. for 2 h.

[0054] The present invention also provides the use of the aforementioned copolymer or the aforementioned ablation heat protection hybrid resin in the preparation of ablation resistant materials;

[0055] Preferably, the ablation-resistant material is an ablation-resistant material used in extreme environments.

[0056] Compared with the prior art, the present invention has the following beneficial effects:

[0057] The present invention provides a copolymer, which can obtain a hybrid resin with a double network structure after mixing and imidizing the copolymer with a phenolic resin. The copolymer and the phenolic resin in the hybrid resin have good compatibility, and the copolymer is evenly distributed in the phenolic resin; and the hybrid resin undergoes graphitization and ceramicization during the ablation process, and has excellent ablation resistance. The present invention provides a concept and method for preparing a new type of ablation-resistant hybrid phenolic resin by copolymerization, and prepares a new type of ablation-resistant hybrid resin that is expected to meet the increasingly harsh flight environment in the future.

[0058] In the present invention, PMPI undergoes graphitization and ceramicization reactions during the ablation process to generate a carbon layer and a SiO2 liquid film covering the carbon layer. Coke and SiO2 undergo a carbon thermal reduction reaction to generate SiC grains. Thereafter, the SiC grains continue to grow, increasing the viscosity and oxygen diffusion coefficient of the SiO2 liquid film, which gives the SiO2 protective layer excellent resistance to mechanical erosion by oxyacetylene flames and the ability to isolate oxygen, while the SiO2 liquid film also has a strong radiation heat dissipation capability. These together greatly enhance the ablation resistance of the PMPI / PR hybrid resin.

[0059] Obviously, according to the above contents of the present invention, in accordance with common technical knowledge and customary means in the art, without departing from the above basic technical ideas of the present invention, other various forms of modification, replacement or change may be made.

[0060] The above contents of the present invention are further described in detail below through specific implementation methods in the form of embodiments. However, this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above contents of the present invention belong to the scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] Figure 1 The synthetic route of the poly(dimethylbenzimide)siloxane / phenolic double network hybrid resin of the present invention is shown in FIG. a. The synthetic route of PMP; b. The synthetic route of PMPA; and c. The synthetic route of PMPI / PR hybrid resin.

[0062] Figure 2 The structural characterization results of PMP, PMPA and hybrid resin of the present invention are as follows: a is the FTIR spectrum of PMP; b is the 1 H-NMR spectrum; c is the FTIR spectrum of PMPA; d is the FTIR spectrum of hybrid resin and phenolic resin (PR).

[0063] Figure 3 The scanning electron microscope (SEM) images of PMPI / PR hybrid resins with different phenyl contents: a is S0; b is S5; c is S 15 ; d is S 20 .

[0064] Figure 4 This is a scanning electron microscope image of pure phenolic resin (PR).

[0065] Figure 5 Hybrid resin S 15 AFM and TEM test results: a is S 15 AFM image of S 15 HAADF plot of .

[0066] Figure 6 TGA results of PMPI / PR hybrid resins with different phenyl contents: a is 800℃, nitrogen; b is 800℃, air; c is the degradation activation energy.

[0067] Figure 7 Optical images after ablation of different resins.

[0068] Figure 8The ablation resistance study results of the PMPI / PR hybrid resin of the present invention: a is the linear ablation rate result of the PMPI / PR hybrid resin; b is the mass ablation rate result of the PMPI / PR hybrid resin; c is a schematic diagram of the ablation layer; d is the thickness distribution result of the residual resin; e is the linear ablation rate distribution result; x in d and e represents the different positions of the sample points on a straight line in the cross section with one end of the sample cross section as the starting point.

[0069] Fig. 9 The XRD patterns and SEM images of the carbon layer of each resin after ablation: a is the XRD pattern of the carbon layer; b is the SEM pattern of the carbon layer after PR ablation; c is the SEM pattern of the carbon layer after S0 ablation; d is the SEM pattern of the carbon layer after S5 ablation; e is the SEM pattern of the carbon layer after S 15 SEM spectrum of the carbon layer after ablation; f is S 30 SEM image of the carbon layer after ablation; d' is the image after the image in the red box in d is enlarged; e' is the image after the image in the red box in e is enlarged; f' is the image after the image in the red box in f is enlarged. DETAILED DESCRIPTION

[0070] The raw materials and equipment used in the specific embodiments of the present invention are all known products, which are obtained by purchasing commercially available products. The full names and corresponding abbreviations of some reagents of the present invention are as follows:

[0071] Octaphenylcyclotetrasiloxane (P4), octamethylcyclotetrasiloxane (D4), (3-aminopropyl)triethoxysilane (APTES), 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA).

[0072] Example 1. Preparation of poly(dimethylbenzamide)siloxane / phenolic double network hybrid resin of the present invention

[0073] 1. Synthesis of PMP with different phenyl content

[0074] PMP is synthesized by anionic ring-opening polymerization of D4, P4, and 1,3-bis(3-aminopropyl)tetramethyldisiloxane under the catalysis of tetramethylammonium hydroxide. Specifically, D4, P4, end-capping agent 1,3-bis(3-aminopropyl)tetramethyldisiloxane and tetramethylammonium hydroxide (TMAOH) are added to a three-necked flask, and first the system is evacuated at 60°C to remove the water in the system. Subsequently, nitrogen is introduced to restore the system to normal pressure, and the system is reacted at 120°C for 2.5 hours. Then, the temperature of the system is raised to 150°C and maintained for 0.5 hours, and the catalyst tetramethylammonium hydroxide decomposes into trimethylamine and methanol. Finally, the system is evacuated to remove unreacted monomers, trimethylamine and methanol to obtain a colorless, transparent, viscous liquid, which is PMP. The synthesis route of PMP is as follows Figure 1The raw material formula for synthesizing PMP with different phenyl content is shown in Table 1, and the amount of catalyst tetramethylammonium hydroxide is 0.5wt% of the total mass of P4 and D4. In Table 1, PMP0 means that the molar content of phenyl in the synthesized PMP is 0%, PMP5 means that the molar content of phenyl in the synthesized PMP is 5%, and PMP 15 The molar content of phenyl in the synthesized PMP is 15%. 30 This indicates that the molar content of phenyl in the synthesized PMP is 30%.

[0075] Table 1. Raw material formula for synthesizing PMP with different phenyl content

[0076]

[0077] 2. Synthesis of PMPA with different phenyl contents

[0078] Under nitrogen atmosphere, a THF solution containing 50 wt% PMP was added dropwise to a three-necked flask containing BPDA (the molar ratio of amino groups in PMP to anhydride in BPDA was 1:1.05) and tetrahydrofuran (THF, the mass ratio of THF to PMP was 1:1), and the reaction was carried out at 35°C for 2.5 hours to ensure that the molecular chain was capped with excess anhydride. Subsequently, the capping agent APTES was added (the amount of APTES added was 20 mol% of the amino group content in PMP), and the reaction was continued for 1 hour to obtain a transparent viscous PMPA. The synthetic route of PMPA is as follows Figure 1 PMPA with different phenyl content was prepared by using PMP with different phenyl content, and was named PMPA0, PMPA5, PMPA 15 、PMPA 30 .

[0079] 3. Synthesis of PMPI / PR hybrid resins with different phenyl contents

[0080] PMPA was added to an anhydrous ethanol solution containing 50wt% PR (the mass ratio of PR to anhydrous ethanol was 1:1), the mass ratio of PMPA to PR was 1:2, and the reaction was carried out at 80°C for 1h, and then vacuum was evacuated at 90°C to remove the solvent to obtain a light yellow powder. The hybrid resin was cured and imidized by hot pressing to finally obtain PMPI / PR hybrid resin. The curing and imidization procedures were sequentially maintained at 120°C for 0.5h, 160°C for 1h, 180°C for 2h, and 200°C for 2h. The synthesis route of PMPI / PR hybrid resin is as follows Figure 1 PMPA with different phenyl contents were used to prepare PMPI / PR hybrid resins with different phenyl contents, which were named S0, S5, S 15 , S 30 .

[0081] The beneficial effects of the present invention are demonstrated below through specific test examples.

[0082] Experimental Example 1: Structural Characterization of PMP and PMPI / PR Hybrid Resins with Different Phenyl Contents

[0083] 1. Experimental methods

[0084] Fourier transform infrared spectrometer (FTIR) was used to analyze the PMP0, PMP5, PMP 15 、PMP 30 、PMPA0、PMPA5、PMPA 15 、PMPA 30 , S0, S5, S 15 , S 30 and pure phenolic resin (PR) were tested; H NMR ( 1 H-NMR) of PMP0, PMP5, PMP 15 and PMP 30 Conduct testing.

[0085] FTIR detection conditions: room temperature, carried out on a Nicolet is50 spectrometer.

[0086] 1 H-NMR detection conditions: The samples were dissolved in CDCl3 and measured on a Bruker AV III HD 400 MHz spectrometer.

[0087] 2. Experimental results

[0088] Figure 2 (a) and (b) show the FTIR and 1 H-NMR results. Figure 2 (a) 3380~3310cm -1 The absorption peak corresponds to the NH stretching vibration of the terminal amino group in the PMP molecular chain. -1 The peaks near 1132-1009cm represent the CH stretching vibrations on the benzene ring, which increase with the increase of phenyl content. -1 The broad peak nearby corresponds to the Si-O-Si skeleton in the molecular chain. Figure 2 In (b), the chemical shift at 0.1ppm belongs to the characteristic absorption peak of the side methyl group in PMP, and the multiple peaks between 7.0 and 8.0ppm correspond to the characteristic absorption peaks of H on the benzene ring. The characteristic absorption peak of the amino group is located at 1.4ppm, which coincides with -C-CH2-C- in 1,3-bis(3-aminopropyl)tetramethyldisiloxane.1 The integrated areas of the characteristic absorption peaks of different functional groups in the H-NMR spectrum were used to calculate the contents of phenyl and amino groups in PMPs with different phenyl contents, and the results are shown in Table 2. In addition, the molecular weight data of PMPs with different phenyl contents are also listed in Table 2.

[0089] Table 2. Phenyl and amino content in PMP and molecular weight of PMP

[0090]

[0091] Figure 2 (c) at 1644 cm -1 The amide I band appears at 1574 cm -1 The NH angle vibration in the amic acid is the "ring breathing" mode in aromatic amines and belongs to the amide II band. These evidences show that the amic acid was successfully introduced into PMPA. The FTIR spectrum of the hybrid resin after curing and imidization is shown in Figure 2. Figure 2 (d) The hybrid resin has a peak at 1775 cm -1 and 1716cm -1 Nearby, the absorption peaks of the asymmetric stretching of C=O and the symmetric stretching of C=O in the imide group appeared. -1 The peak at 970 cm represents the CN stretching vibration in the imide group. -1 The nearby peaks belong to the Si-O-ph structure, which indicates that the ethoxy groups at the ends of the PMPI molecular chains reacted successfully with the hydroxyl groups in PR, promoting the construction of a three-dimensional cross-linked network structure.

[0092] Experimental Example 2: Microstructure of PMPI / PR hybrid resins with different phenyl contents

[0093] 1. Experimental methods

[0094] SEM was used to examine the S0, S5, and S 15 , S 30 The S was tested by AFM and TEM. 15 Conduct testing.

[0095] SEM detection conditions: After the sample was fractured in liquid nitrogen, it was observed using a Japanese Hitachi Co. S-4800 electron microscope at an accelerating voltage of 15 kV.

[0096] AFM detection conditions: The sample cross section was observed using the tapping mode on a Bruker Dimension ICON.

[0097] TEM detection conditions: After the resin sections were stained with phosphotungstic acid, they were observed on Talos F200S G2.

[0098] 2. Experimental results

[0099] Figure 3 This is the SEM test picture of the cross section of the hybrid resin with different phenyl content. Figure 4 is a SEM image of the cross section of pure PR. EDS analysis shows that silicone resins with different phenyl contents are uniformly distributed in the PR matrix without obvious phase separation. This shows that the introduction of ethoxy, imide ring and phenyl in the silicone segment can significantly improve its compatibility with PR, thereby avoiding the formation of sea island phase structure. In order to further accurately characterize the phase structure of the hybrid resin, S 15 AFM and TEM tests were performed.

[0100] Figure 5 (a) AFM tapping mode was used to measure the 15 The results of the cross-sectional test show that the hybrid resin exhibits a bright and dark distribution of a bicontinuous structure in the phase diagram, depending on the different forces between the probe and the PMPI soft chain and the PR hard chain. Figure 5 (b) is S 15 HAADF image, the black part is PMPI. It can be seen that PMPI is distributed in the matrix in a nanometer-scale co-continuous manner, similar to AFM. These results show that S 15 It presents a microstructure of a nanoscale bicontinuous network.

[0101] Test Example 3: Thermal Performance Study

[0102] 1. Experimental methods

[0103] S0, S5, S 15 , S 30 Thermogravimetric analysis (TGA) was performed on pure phenolic resin (PR).

[0104] TGA detection conditions: The test was carried out on NETZSCH STA 449F3 at a heating rate of 10°C / min.

[0105] 2. Experimental results

[0106] In order to evaluate the effect of the introduction of PMPI on the thermal stability of the hybrid resin, the thermal degradation behavior of the hybrid resin of the present invention in nitrogen and air atmospheres was studied using TGA. Figure 6 The characteristic data and heat resistance index of resin thermal degradation are listed in Table 3. Under nitrogen, S0~S 30The thermal residual weight at 800℃ is not much different, all 47%, which is lower than that of pure PR. This may be because the introduction of PMPI destroys the three-dimensional network structure of PR and reduces the crosslinking degree. 15 The thermal residual weight of the PMPI chain segments increased, which may be due to the ceramicization reaction of the PMPI chain segments, generating SiO2 and causing the weight gain. 15 The thermal residual weight of PMPI is around 10%, which is significantly higher than the 1.9% of pure PR. This is because PMPI forms a dense SiO2 protective layer in a high-temperature oxygen-containing atmosphere, which delays the thermal decomposition and oxidation of the PR matrix to a certain extent.

[0107] The Friedman method was used to calculate the degradation activation energy E for all samples at a heating rate of 10 °C / min. a (Friedman method is based on the method described in the literature, Paik P, Kar KK. Thermal degradation kinetics and estimation of lifetime of polyethylene particles: Effects of particlesize. Materials Chemistry and Physics. 2009; 113(2-3): 953-61.), the results are as follows Figure 6 (c). S0 (16.71 kJ / mol), S5 (17.29 kJ / mol), S 15 (16.08 kJ / mol) is higher than pure PR (11.76 kJ / mol). 30 The Ea of S0~S 15 The higher degradation activation energy is mainly attributed to the introduction of Si-O-Si bonds (446 kJ / mol) with high bond energy into the matrix by the addition of PMPI molecular chains, which is much higher than CC (358 kJ / mol) and CO (384 kJ / mol). At the same time, the introduced phenyl groups can inhibit the decomposition of Si-O-Si bonds, thereby increasing the degradation activation energy of the hybrid resin. However, when the phenyl content is too high (S 30 ), whose large steric hindrance is not conducive to the mutual chemical bonding and entanglement of PMPI and PR molecular chains, greatly destroying the three-dimensional network structure, resulting in a lower degradation activation energy. These results show that the introduction of PMPI with an appropriate phenyl content should be able to inhibit the thermal degradation of hybrid resins.

[0108] Table 3. Degradation characteristic thermal data

[0109]

[0110] T 5% and T 30% The decomposition temperatures corresponding to 5% and 30% weight loss respectively; * T Heat-resistance index =0.49×[T 5% +0.6×(T 30% –T 5% )].

[0111] Test Example 4: Ablation resistance of PMPI / PR hybrid resin

[0112] 1. Experimental methods

[0113] S0, S5, S 15 , S 30 The ablation resistance of pure phenolic resin (PR) was tested.

[0114] Ablation resistance test method: According to GJB 323A-1996, use Xi'an Zhirui Company's ZR-323A oxyacetylene ablation machine at 4MW / m 2 Ablation was performed under heat flow for 30 s.

[0115] 2. Experimental results

[0116] The heat flux is 4MW / m 2 The ablation resistance of the hybrid resin of the present invention was tested by oxyacetylene flame. The optical image of the hybrid resin after ablation is shown in FIG. Figure 7 shown. Figure 8 (a) and 8(b) show the linear ablation rate (LAR) and mass ablation rate (MAR) of the resin. As the phenyl content gradually increases, the linear ablation rate of the hybrid resin gradually decreases, and the ablation resistance improves. 15 The linear ablation rate of S was the lowest (0.055 mm / s), which was 74.4% lower than that of pure PR (0.21 mm / s). However, with the further increase of phenyl content, the linear ablation rate of hybrid resin increased and the ablation resistance decreased. 15The therapeutic ablation rate (0.055 g / s) decreased by about 15.1% compared with pure PR (0.067 g / s). Compared with PR composites introduced with tetrasilane octaphenyl POSS (T-POSS) (Niu Z, Li G, Ma X, et al. Synergetic effect of O-POSS and T-POSSto enhance ablative resistant of phenolic-based silica fiber composites via strong interphase strength and ceramic formation[J]. Composites Part A: Applied Science and Manufacturing, 2022, 155: 106855.) and carbon nanotubes (CNT) (Wang ZJ, Kwon DJ, Gu GY, et al. Ablative and mechanical evaluation of CNT / phenolic composites by thermal and microstructural analyses[J]. Composites Part B: Engineering, 2014, 60: 597-602.) (LAR is 0.100 mm / s and 0.130 mm / s, respectively), S 15 The LAR has been significantly reduced and the ablation resistance has been significantly improved.

[0117] The 3D profilometer was used to measure the sample PR, S0, S 15 The residual thickness after ablation was calculated, and the LAR of the corresponding point was obtained by dividing the thickness difference at each position before and after ablation by the ablation time. Figure 8 In (d), PR and S after ablation 15 Compared with S0, the thickness of the ablation edge area increased significantly, while S0 did not show any obvious thickness increase in the ablation edge area. f Compared with PR, there is no significant reduction in thickness. Figure 8 As shown in (e), the introduction of an appropriate amount of phenyl groups makes S 15 Compared with S0 and PR, the LAR at each point is kept at a lower level, and its maximum LAR is only 0.055 mm / s, which is about one-fourth of pure PR (0.21 mm / s). In general, the hybrid resin of the present invention can well resist the erosion of high heat flux flames and is expected to be competent for more severe service environments in the future.

[0118] The carbon layer of each resin after ablation was characterized by XRD to confirm its composition. Fig. 9 (a). The diffraction peak observed near 23.6° corresponds to amorphous SiO2. The peaks appearing near 35.3°, 59.9°, and 71.7° belong to the (1 1 1), (2 2 0), and (3 1 1) diffraction planes of SiC, respectively, which match the cubic structure of β-SiC. In addition, a small shoulder peak appears on the left side of the (1 1 1) peak, which is the stacking faults formed by the growth of SiC grains during the ablation process. The diffraction peaks at 2θ=25.7° and 43.1° belong to the (002) and (100) reflections of graphite, indicating that the PR matrix has been graphitized during the ablation process.

[0119] Fig. 9 (b)~ Fig. 9 In (f), the XRD and EDS mapping results show that compared with the smooth carbon layer of pure PR, S0~S 30 The side of the carbon layer is covered with a SiO2 / SiC composite ceramic protective layer, which can help enhance the hybrid resin's ability to resist the impact of high-speed oxygen-containing hot air flow. 30 The side of the carbon layer of S0 is covered with a large number of SiO2 spheres with larger diameters. This may be because during the ablation process, the liquid SiO2 generated on the surface of the carbon layer of S0 is not able to resist the high-speed and high-pressure oxyacetylene flame, causing it to flow toward the original layer together with the hot air. These molten SiO2 washed down undergo nucleation and growth on the side of the carbon layer, and after the ablation is completed, as the temperature decreases, the surface tension of SiO2 increases, and it gradually cools to form spheres. 30 Zoom in on the red frame, Fig. 9 (d')~ Fig. 9 As shown in (f'), the diameter of the SiO2 spheres on the side of the carbon layer is significantly reduced, which may be related to the fact that the introduced phenyl groups are beneficial to increasing the viscosity of the SiO2 liquid film, thereby improving its ability to resist the impact of hot air flow.

[0120] The above experimental results show that the PMPI / PR hybrid resin of the present invention has good ablation resistance. 15 Best ablation resistance.

[0121] In summary, the present invention provides a copolymer, which can be mixed with a phenolic resin and imidized to obtain a hybrid resin with a double network structure. The copolymer and the phenolic resin in the hybrid resin have good compatibility, and the copolymer is evenly distributed in the phenolic resin; moreover, the hybrid resin undergoes graphitization and ceramicization during the ablation process, and has excellent ablation resistance. The present invention provides a concept and method for preparing a new type of ablation-resistant hybrid phenolic resin by copolymerization, and prepares a new type of ablation-resistant hybrid resin that is expected to meet the increasingly harsh flight environment in the future.

Claims

1. A copolymer for preparing ablative heat protection hybrid resin, characterized in that: Its structure is shown in Formula I: Wherein, x is selected from an integer of 0 to 6; y is selected from an integer of 3 to 18; z is selected from integers of 3-24.

2. The copolymer according to claim 1, characterized in that: x is an integer selected from 1 to 2; y is selected from an integer of 7 to 10; z is selected from integers of 8-12.

3. The copolymer according to claim 1 or 2, characterized in that: It is prepared from PMP, 3,3',4,4'-biphenyltetracarboxylic dianhydride and (3-aminopropyl)triethoxysilane as raw materials; The PMP is synthesized by using octaphenylcyclotetrasiloxane, octamethylcyclotetrasiloxane and 1,3-bis(3-aminopropyl)tetramethyldisiloxane as raw materials through anionic ring-opening polymerization.

4. The copolymer according to claim 3, characterized in that: The molar ratio of the amino group in the PMP to the anhydride in 3,3',4,4'-biphenyltetracarboxylic dianhydride is 1:1 to 1.1; The (3-aminopropyl)triethoxysilane is 0 to 40 mol% of the amino content in PMP; Preferably, The (3-aminopropyl)triethoxysilane is 20-40 mol% of the amino group content in PMP.

5. The copolymer according to claim 3, characterized in that: The molar ratio of octaphenylcyclotetrasiloxane, octamethylcyclotetrasiloxane and 1,3-bis(3-aminopropyl)tetramethyldisiloxane is 0-6:2-12:0-4; Preferably, the molar ratio of octaphenylcyclotetrasiloxane, octamethylcyclotetrasiloxane and 1,3-bis(3-aminopropyl)tetramethyldisiloxane is 0.5-3:7-10:1-3; More preferably, the molar ratio of octaphenylcyclotetrasiloxane, octamethylcyclotetrasiloxane and 1,3-bis(3-aminopropyl)tetramethyldisiloxane is 0.5-3:7-9.5:2; More preferably, the molar ratio of octaphenylcyclotetrasiloxane, octamethylcyclotetrasiloxane and 1,3-bis(3-aminopropyl)tetramethyldisiloxane is 1.5:8.5:

2.

6. The copolymer according to claim 3, characterized in that: The preparation method of the PMP comprises the following steps: Octaphenylcyclotetrasiloxane, octamethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)tetramethyldisiloxane and a catalyst are mixed, nitrogen is introduced, and the mixture is reacted to obtain the product; Preferably, the catalyst is selected from tetramethylammonium hydroxide; And / or, vacuuming is performed before introducing nitrogen; And / or, the reaction is carried out at 100-120° C. for 1-5 hours, and then the temperature is raised to 150-200° C. and maintained for 0.5-5 hours; More preferably, the mass of the catalyst is 0.5-5 wt % of the total mass of octaphenylcyclotetrasiloxane and octamethylcyclotetrasiloxane.

7. The method for preparing the copolymer according to any one of claims 1 to 6, characterized in that: It includes the following steps: (1) In a solvent, 3,3',4,4'-biphenyltetracarboxylic dianhydride and PMP are mixed and reacted; (2) adding (3-aminopropyl)triethoxysilane and continuing the reaction to obtain; Preferably, In step (1), the solvent is tetrahydrofuran; And / or, in step (1), the reaction temperature is 30 to 50° C., and the reaction time is 1 to 5 hours; And / or, in step (2), the reaction temperature is 30 to 50° C., and the reaction time is 1 to 5 hours; More preferably, In step (1), the mass ratio of the solvent to PMP is (1-5):

1.

8. Use of the copolymer and resin according to any one of claims 1 to 6 as raw materials in the preparation of ablative heat protection hybrid resin; Preferably, the resin is a phenolic resin.

9. An ablative heat protection hybrid resin, characterized in that: It is prepared by mixing the copolymer described in any one of claims 1 to 6 with a resin, and then curing and imidizing. Preferably, the mass ratio of the copolymer to the resin is 1:1 to 5; And / or, the reaction is carried out in a solvent; And / or, the reaction temperature is 80-100°C; the reaction time is 1-10h; And / or, the curing and imidization procedures are sequentially maintained at 100-120° C. for 0.1-1 h, 130-170° C. for 1-5 h, 180-190° C. for 1-5 h, and 200-220° C. for 1-5 h; More preferably, the resin is a phenolic resin; And / or, the mass ratio of the copolymer to the resin is 1:2; And / or, the solvent is anhydrous ethanol; And / or, the solvent is removed by vacuuming before curing and imidization; And / or, the curing and imidization procedures are sequentially maintained at 120° C. for 0.5 h, 160° C. for 1 h, 180° C. for 1 h, and 200° C. for 2 h.

10. Use of the copolymer according to any one of claims 1 to 6 or the ablative heat protection hybrid resin according to claim 9 in the preparation of ablative resistant materials; Preferably, the ablation-resistant material is an ablation-resistant material used in extreme environments.

Citation Information

Patent Citations

  • Modified carboxyl-terminated hyperbranched polyamide resin, as well as preparation method and application thereof

    CN103113578A

  • Polyimide-based carbon aerogel as well as preparation method and application thereof

    CN115818616A

  • Polyamic acid resin, preparation method thereof and positive photosensitive resin composition

    CN116082636A

  • Resin composition, cured film, method for producing relief pattern of cured film, electronic component, semiconductor device, method for producing electronic component, and method for producing semiconductor device

    JP2019123864A

Cited By

  • Ablation / heat insulation integrated organic silicon hybrid phenolic aerogel composite material as well as preparation method and application thereof

    CN118165527A

  • Ablation / thermal insulation integrated organic silicon hybrid phenolic aerogel composite material, and preparation method and use thereof

    CN118165527B

  • Ablation-resistant hybrid resin containing covalent-ionic bicontinuous network as well as preparation method and application of ablation-resistant hybrid resin

    CN119875137A