High-wear-resistance anti-crack mining engineering tire tread rubber
By using reinforced crack-resistant resin and modified reinforcement filler in the tread glue, the wear and tear problems of mining engineering tire tread glue under harsh working conditions is solved, achieving higher wear resistance and resistance The crack performance extends the service life of the tire.
Patent Information
- Application Number
- CN202411183016.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-22
AI Technical Summary
Mining engineering tire tread glue is prone to wear and tear under harsh working conditions, resulting in a short service life and difficulty in taking into account both wear resistance and heat generation performance.
Reinforced crack-resistant resin and modified reinforcement filler are used to enhance the mechanical properties and wear resistance of the tread glue through its unique molecular structure and nanoscale dispersion characteristics, prevent crack propagation and reduce tearing risks.
It significantly improves the wear resistance, crack resistance and cut resistance of the tread glue, extends the service life of the tire, reduces the failure rate, and ensures reliability under mine conditions.
Smart Images

Figure BDA0005012752650000021 
Figure BDA0005012752650000031 
Figure BDA0005012752650000032
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of tread rubbers, and in particular to a highly wear-resistant and crack-resistant mining engineering tire tread rubber. Background Art
[0002] Due to the large amount of gravel on mining and transportation roads, the heavy load of mining vehicles and the long operation time, mining engineering tires have extremely high requirements for tread wear resistance and crack resistance, especially in extremely harsh working conditions such as underground mines. The failure rate of tires due to severe wear and tear and cutting cracks is as high as more than 50%. At the same time, in order to prevent shoulder delamination problems, the heat generation performance of the tire must also be taken into account. It is difficult to achieve a good balance between the two, which seriously restricts the service life of the product. Summary of the invention
[0003] The technical problem to be solved by the present invention is: to overcome the shortcomings of the prior art and provide a highly wear-resistant and crack-resistant mining engineering tire tread rubber, which can significantly improve the wear resistance and damage resistance of the tread rubber, reduce the problem of low product life due to low wear resistance and easy tearing, thereby providing a longer product life, improving mining efficiency, and bringing higher value to customers.
[0004] The technical solution of the present invention is:
[0005] A highly wear-resistant and crack-resistant mining engineering tire tread rubber comprises the following components in parts by weight: 100 parts of a rubber component, 40-50 parts of carbon black, 15-25 parts of a modified reinforcing filler QINAI N9, 3-5 parts of a tackifying resin, 4-6 parts of a reinforced anti-crack resin AT-KL, 3-5 parts of an antioxidant, 2-3 parts of microcrystalline wax, 3-4 parts of zinc oxide, 2-3 parts of stearic acid, 1.4-2 parts of sulfur and 1.2-2 parts of an accelerator.
[0006] Among them, the modified reinforcing filler is a flat silicate reinforcing filler prepared by double surface modification of natural clay. The trade name is Qinai N9, Shanghai Qixiang New Materials Technology Co., Ltd.
[0007] The reinforced anti-crack resin is a modified reinforced resin with functional groups, the trade name is AT-KL, produced by Jiangsu Kaou Chemical Co., Ltd.
[0008] Preferably, the rubber component is 40-60 parts of natural rubber and 40-60 parts of styrene-butadiene rubber.
[0009] Preferably, the carbon black is one or both of N115 carbon black and N220 carbon black.
[0010] Preferably, the tackifying resin is an alkylphenol tackifying resin TYC-0412 tackifying resin or a p-tert-octylphenol formaldehyde tackifying resin SL1801.
[0011] Preferably, the antioxidant is ketoamine antioxidant RD and p-phenylenediamine antioxidant 4020.
[0012] Preferably, the accelerator is a sulfenamide accelerator or a combination of a sulfenamide accelerator and a thiazole accelerator.
[0013] Compared with the prior art, the present invention has the following beneficial effects:
[0014] 1. Compared with conventional tire tread rubber, the tread rubber prepared by the present invention adopts a reinforced anti-crack resin and a modified reinforcing filler. The reinforced anti-crack resin, due to its unique molecular structure, can absorb and disperse energy when the material is subjected to stress, thereby effectively preventing the expansion of cracks, which is particularly important in the face of sharp stones and cutting materials commonly found in mining areas; and the addition of highly dispersible modified reinforcing fillers not only enhances the mechanical properties of the tread rubber, but also improves its wear resistance. The tread rubber of the present invention provides excellent wear resistance and anti-crack performance while ensuring heat generation performance, ensuring the reliability of vehicles under harsh road conditions such as mines, reducing tire failure rates, and making tires have a longer service life.
[0015] 2. The tread rubber of the present invention is used for tires of mining engineering vehicles, and exhibits higher wear resistance, crack resistance and cut resistance than ordinary tires. When the vehicle is driving on an unpaved road covered with ore fragments, the wear level of the tire is significantly improved, and the heat generation is less affected. In addition, the tread rubber of the present invention also effectively reduces the risk of tire tread tearing due to the sharp edges of the ore, which has a positive effect on reducing the failure rate of tire use and extending the service life. DETAILED DESCRIPTION
[0016] In order to enable persons skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention.
[0017] Examples 1-3 and Comparative Examples 1-3
[0018] The tread rubber formulations of Examples 1-3 and Comparative Examples 1-3 are shown in Table 1:
[0019] Table 1 Tread rubber formulations of Examples 1-3 and Comparative Examples 1-3
[0020]
[0021]
[0022] The preparation method of the tread rubber of Examples 1-3 and Comparative Examples 1-3 comprises the following steps:
[0023] S1 one-stage mixing
[0024] 100 parts of rubber component, 30 parts of carbon black, Qinai N9, AT-KL, TYC-0412, zinc oxide, stearic acid and microcrystalline wax were put into an internal mixer and mixed at a speed of 40 rpm. The mixture was lifted and pressed every 30 seconds. When the temperature of the rubber material reached 160°C, the rubber was discharged and the sheets were dropped. After cooling at room temperature for 5 hours, a masterbatch was obtained, which was then mixed in two stages.
[0025] S2 two-stage mixing
[0026] The first-stage masterbatch of step S1 and the remaining carbon black and antioxidant are put into an internal mixer, mixed at a speed of 36 rpm, and the lump is lifted and pressed every 30 seconds. When the temperature of the rubber material reaches 150°C, the rubber is discharged and the sheets are dropped. After cooling at room temperature for 4 hours, the second-stage masterbatch is obtained, and then the masterbatch is finally refined;
[0027] S3 Final Refining
[0028] The second-stage masterbatch of step S2, sulfur and accelerator are put into an internal mixer and mixed at a speed of 26 rpm. The mixture is lifted and pressed at intervals of 25 s, 25 s and 20 s respectively. When the mixing time reaches 120 s, the rubber is discharged and sliced. After being left to cool, the mixed rubber for tread of mining engineering tire is obtained.
[0029] The mining engineering tire tread rubbers prepared in Examples 1-3 and Comparative Examples 1-3 were subjected to high temperature vulcanization to prepare test samples, and then performance tests were performed. The test results are shown in Table 2:
[0030] Table 2 Physical properties test results of mining engineering tire tread rubber prepared in Examples 1-3 and Comparative Examples 1-3
[0031]
[0032]
[0033] Test sample vulcanization conditions: 147°C × 60min.
[0034] By comparing Example 1 with Comparative Example 1, it can be seen that when the modified reinforcing filler Qinai N9 and the reinforced anti-crack resin AT-KL are added to the tire tread rubber at the same time, the tensile strength and the tensile stress of the rubber are not much different, the hardness decreases, and the basic physical properties remain basically unchanged; the tear strength is increased by about 18%, the cutting performance is increased by about 27%, and the wear performance is increased by about 28%, the cutting resistance and wear performance of the rubber are significantly improved, and the heat generation performance remains basically unchanged.
[0035] Comparing Example 1 with Comparative Examples 2-3, it can be seen that when the modified reinforcing filler Qinai N9 and the reinforced anti-crack resin AT-KL are added to the rubber compound at the same time, the advantages shown by the rubber compound are more obvious than those of the rubber compound in which only one of the materials is added.
[0036] Qinai N9 is a flat silicate reinforcing filler prepared by two surface modification methods, chemical modification and intercalation technology, which can significantly improve the performance of silicate mineral powder. In the chemical modification process, the silicate surface is treated with a silane coupling agent, and its hydrolyzable groups react with the hydroxyl groups on the silicate surface to form hydrogen bonds, and further undergo condensation and dehydration reactions when heated to form covalent bonds, which not only enhances the binding force between silicates and organic polymer materials, but also improves the cross-linking of materials and the strength of rubber. The intercalation technology utilizes the weak binding force between silicate layers, inserts organic molecules such as long-chain alkyl quaternary ammonium salts or silane coupling agents, realizes the transition from hydrophilicity to hydrophobicity, and effectively increases the interlayer spacing, providing insertion space for the molecular chains of polymer materials such as rubber, thereby achieving uniform dispersion at the nanoscale. The reinforced anti-crack resin AT-KL carries a variety of functional groups such as amino, carboxylic acid and epoxy groups. These functional groups enhance the bonding between the resin and the rubber, forming a more stable network structure and improving the mechanical properties and durability of the rubber. Specifically, the amino and carboxylic acid groups enhance the interaction between the filler and the rubber matrix by forming hydrogen bonds or chemically reacting with the active groups in the rubber, thereby improving the cohesion and crack resistance of the rubber. At the same time, the epoxy groups react with the active hydrogen in the rubber molecular chain to form chemical bonds, further enhancing the crosslinking density and crack resistance of the rubber. When these two materials are used together, the nano-scale dispersion characteristics of Qinai N9 interact with the multifunctional groups of AT-KL, not only providing a more uniform stress distribution at the microscopic level, but also enhancing the overall cohesion of the material through chemical bonds and physical entanglement. This synergistic effect improves the mechanical properties of the material, especially in terms of wear resistance and crack (tear) resistance, making the composite material less likely to be damaged when subjected to external forces, and the expansion and tearing of cracks are effectively suppressed, significantly improving the wear and crack resistance of the tread.
Claims
1. A highly wear-resistant and crack-resistant mining engineering tire tread rubber, characterized in that: The invention comprises the following components in parts by weight: 100 parts of rubber component, 40-50 parts of carbon black, 15-25 parts of modified reinforcing filler Qi Nai N9, 3-5 parts of tackifying resin, 4-6 parts of reinforced anti-crack resin AT-KL, 3-5 parts of antioxidant, 2-3 parts of microcrystalline wax, 3-4 parts of zinc oxide, 2-3 parts of stearic acid, 1.4-2 parts of sulfur and 1.2-2 parts of accelerator.
2. The highly wear-resistant and crack-resistant mining engineering tire tread rubber according to claim 1, characterized in that: The rubber component comprises 40-60 parts of natural rubber and 40-60 parts of styrene-butadiene rubber.
3. The highly wear-resistant and crack-resistant mining engineering tire tread rubber according to claim 1, characterized in that: The carbon black is one or both of N115 carbon black and N220 carbon black.
4. The highly wear-resistant and crack-resistant mining engineering tire tread rubber according to claim 1, characterized in that: The tackifying resin is alkylphenol tackifying resin TYC-0412 tackifying resin or p-tert-octylphenol formaldehyde tackifying resin SL1801.
5. The highly wear-resistant and crack-resistant mining engineering tire tread rubber according to claim 1, characterized in that: The antioxidants are ketoamine antioxidant RD and p-phenylenediamine antioxidant 4020.
6. The highly wear-resistant and crack-resistant mining engineering tire tread rubber according to claim 1, characterized in that: The accelerator is a sulfenamide accelerator or a combination of a sulfenamide accelerator and a thiazole accelerator.