Ultrahigh-strength corrosion-resistant low-alloying Mg-Al-Mn-Y-Zr alloy and preparation method thereof

Through the smelting casting, solid solution treatment and low-temperature extrusion processes of Mg-Al-Mn-Y-Zr alloy, the problem of insufficient strength and corrosion resistance of magnesium alloy is solved, and a magnesium alloy with high strength and good corrosion resistance is realized. Reduce costs and expand the scope of application.

CN118996218AActive Publication Date: 2024-11-22TAIYUAN UNIVERSITY OF TECHNOLOGY
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411109536.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The absolute strength of magnesium alloy is not high and has poor corrosion resistance, which limits its application in high load and corrosive environments, and the high price of rare earth elements limits its industrial application.

Method used

Mg-Al-Mn-Y-Zr alloy is used to form a high-strength, good corrosion resistance magnesium alloy through melting casting, solid solution treatment and low-temperature extrusion processes. It has low cost, simple process and short process.

Benefits of technology

Magnesium alloys with high tensile strength, yield strength and corrosion resistance have been achieved, which reduces the preparation cost, expands the application range of magnesium alloys, and avoids the high cost of using rare earth elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996218A_ABST
    Figure CN118996218A_ABST
Patent Text Reader

Abstract

The invention provides an ultrahigh-strength corrosion-resistant low-alloying Mg-Al-Mn-Y-Zr alloy and a preparation method thereof, and belongs to the technical field of magnesium alloys. According to the invention, magnesium, aluminum, a magnesium-manganese intermediate alloy, a magnesium-yttrium intermediate alloy and a magnesium-zirconium intermediate alloy are used as raw materials, and are subjected to smelting casting, solution treatment and low-temperature extrusion to prepare the high-strength corrosion-resistant magnesium alloy. 0.1% of Mn; 0.1% of Y; 0.1% of Zr, with the balance being magnesium and unavoidable impurities. According to the prepared alloy, the ductility is 5%, the tensile strength is 501.3 MPa, the yield strength is 400.9 MPa, the corrosion rate in simulated body fluid is 0.07 mm / a, and the preparation method has the advantages of being low in cost, simple in technology, short in process and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of magnesium alloys, and in particular relates to an ultra-high-strength corrosion-resistant low-alloyed Mg-Al-Mn-Y-Zr alloy and a preparation method thereof. Background Art

[0002] Magnesium and magnesium alloys have high specific strength, specific stiffness, and good cutting performance, and have broad application prospects in aerospace, automobile, military and other fields; at the same time, magnesium alloys, as functional metal materials, have biodegradable properties and also have important application potential in the biomedical field. Because the absolute strength of magnesium alloys is not high and the corrosion resistance is poor, their application in high-load and corrosive environments is limited. Therefore, it is necessary to develop new high-strength and corrosion-resistant magnesium alloys to promote their application level.

[0003] In order to improve the corrosion resistance of magnesium alloys, for example, adding trace amounts of rare earth elements to AM60 can greatly improve the corrosion resistance. At present, some magnesium alloy materials have been developed and industrialized, but the strength of the above alloys is generally lower than 380MPa, which limits their application. How to improve the strength of magnesium and magnesium alloys has become a bottleneck problem that limits the widespread application of magnesium alloys. Designing the organizational structure and alloying is one of the most effective ways to improve the strength of magnesium alloys. Due to the high solid solubility of rare earth elements in magnesium, they have obvious aging strengthening characteristics and can form nano-scale second phase precipitation, thereby improving the strength of the alloy. Pan Hucheng et al. studied the tensile strength (UTS) and yield strength (YS) of Mg-13Gd alloy, reaching 493MPa and 458MPa respectively. The Mg-8Dy-5Cu-2Sn alloy studied by Liu Ke et al. achieved a tensile strength of 420MPa and a yield strength of 390MPa after homogenization and hot extrusion. Although rare earth magnesium alloys have excellent high strength, the high price of rare earth elements will limit their application in industry.

[0004] Therefore, how to obtain magnesium alloys with high strength, good plasticity and excellent intrinsic corrosion resistance through low alloying and corresponding preparation process technology improvements is of great significance to expanding the application scope of magnesium alloys. Summary of the invention

[0005] In view of this, the object of the present invention is to provide an ultra-high strength, corrosion-resistant, low-alloyed Mg-Al-Mn-Y-Zr alloy and a preparation method thereof. The obtained alloy has low preparation cost and has high tensile strength, yield strength and corrosion resistance.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] In a first aspect, the present invention provides an ultra-high strength corrosion-resistant low-alloyed Mg-Al-Mn-Y-Zr alloy, comprising the following components in weight percentage:

[0008] Al: 0.1%; Mn: 0.1%; Y: 0.1%; Zr: 0.1%, and the rest is magnesium and unavoidable impurities.

[0009] Preferably, the high-strength, corrosion-resistant, low-alloyed magnesium-aluminum-manganese-yttrium-zirconium alloy is made of the following metal raw materials in parts by weight:

[0010] Mg 509.5-514.5 parts, Al 0.5-0.6 parts, magnesium-manganese master alloy 5.5-6.0 parts, magnesium-yttrium master alloy 1.8-2.0 parts, magnesium-zirconium master alloy 1.8-2.0 parts

[0011] The magnesium-manganese mass ratio of the magnesium-manganese master alloy is 9:1;

[0012] The mass ratio of magnesium to yttrium in the magnesium-yttrium master alloy is 7:3;

[0013] The magnesium-zirconium mass ratio of the magnesium-zirconium master alloy is 7:3.

[0014] In a second aspect, the present invention provides a method for preparing the above-mentioned high-strength, corrosion-resistant, low-alloyed magnesium-aluminum-manganese-yttrium-zirconium alloy, comprising the following steps:

[0015] 1) removing the oxide layer of the metal raw material and drying it, and then weighing the metal raw material according to the weight portion;

[0016] 2) placing Mg metal in a smelting furnace under a protective atmosphere, then placing Al metal after keeping the temperature at a first temperature, then placing a magnesium-manganese master alloy after keeping the temperature at a second temperature, then placing a magnesium-yttrium master alloy after keeping the temperature at a third temperature, then placing a magnesium-zirconium master alloy after keeping the temperature at a fourth temperature, and then placing a magnesium-zirconium master alloy after keeping the temperature at a fifth temperature to obtain a molten alloy;

[0017] 3) After the alloy liquid is subjected to a first cooling, a refining agent is added, and stirring, heat preservation, a second cooling, and casting are performed in sequence to obtain an ingot;

[0018] 4) subjecting the ingot to a solution treatment to obtain a solid solution ingot;

[0019] 5) After removing the oxide layer from the solid solution ingot, the ingot is subjected to extrusion treatment to obtain a high-strength, corrosion-resistant, low-alloyed magnesium-aluminum-manganese-yttrium-zirconium alloy.

[0020] Preferably, the protective atmosphere in step 2) is a mixture of SF6 and CO2 in a volume ratio of 40:1.

[0021] Preferably, in step 2), the first temperature is 710-715°C, and the insulation time is 25-30 min; the second temperature is 720-725°C, and the insulation time is 20-25 min; the third temperature is 720-725°C, and the insulation time is 20-25 min; the fourth temperature is 720-725°C, and the insulation time is 20-25 min; the fifth temperature is 750-755°C, and the insulation time is 20-25 min.

[0022] In the present invention, during the entire smelting process, Mg, Al, Mn, Y and Zr undergo an alloying reaction, and the reaction equation is as follows:

[0023] Mg+Al+Mn+Y+Zr→α-Mg+Mg 17 Al 12 ;

[0024] In the formula, α-Mg is the α magnesium phase, Mg 17 Al 12 It is a magnesium-aluminum phase.

[0025] Preferably, the amount of the refining agent in step 3) is 1-2 wt % of the alloy liquid.

[0026] Preferably, the refining agent in step 3) is composed of the following raw materials in weight percentage: MgCl2 46%, KCl 40%, BaCl2 8%, CaF2 5%.

[0027] Preferably, in step 3), the first cooling temperature is 740-745°C; the stirring time is 2-5 min; the heat preservation temperature is 750-755°C, and the heat preservation time is 20-25 min; and the second cooling temperature is 710-715°C.

[0028] Preferably, the method of the solution treatment in step 4) is: firstly perform a primary solution treatment and then perform a secondary solution treatment, followed by water quenching;

[0029] The primary solution treatment temperature is 320°C and the holding time is 1h;

[0030] The secondary solution treatment temperature is 500°C and the holding time is 3 hours. By adopting the above technical solution, the difference between the two holding temperatures is reduced through the two-stage solution treatment, which is conducive to the control of temperature stability; on the other hand, there will be a second phase in the alloy of this design, and this solution treatment method can allow as much of the second phase as possible to melt into the magnesium matrix.

[0031] Preferably, the extrusion treatment method in step 5) is: raising the temperature of the extrusion die to 225-230°C, placing the sample in a heat preservation state for 55-60 minutes, and then extruding at an extrusion temperature of 225°C, an extrusion rate of 0.1 mm / s, and an extrusion ratio of 16:1.

[0032] Preferably, during the preparation process, a protective coating is evenly applied on the surfaces of the crucible, crucible tongs and stirring rod; the protective coating is prepared by mixing talcum powder, water and water glass in a mass volume ratio of 80g:250mL:20g.

[0033] Contains at least the following beneficial technical effects:

[0034] The present invention uses magnesium, aluminum, magnesium-manganese master alloy, magnesium-yttrium master alloy, and magnesium-zirconium master alloy as raw materials, and is prepared into a high-strength and corrosion-resistant magnesium alloy through smelting casting, solid solution treatment, and low-temperature extrusion. During the hot extrusion process, the second phase is broken into fine particles and evenly distributed in the magnesium matrix, so that the matrix is ​​strengthened, and dynamic recrystallization can be promoted to make the organization more refined. The additional strain hardening ability provided by the heterogeneous structure composed of deformed grains and fine grains enhances the tensile strength and yield strength of the magnesium alloy. At the same time, compared with rare earth magnesium alloys and complex and expensive large plastic deformation technical means, the present invention has the advantages of low cost, simple process, short process, etc., so that it has certain economic benefits and application potential. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 is the X-ray diffraction intensity spectrum of the magnesium-aluminum-manganese-yttrium-zirconium alloy prepared in Example 1;

[0036] Figure 2 The electron backscatter diffraction (EBSD) grain boundary image of the magnesium-aluminum-manganese-yttrium-zirconium alloy prepared in Example 1;

[0037] Figure 3 is a potentiodynamic polarization curve of the magnesium-aluminum-manganese-yttrium-zirconium alloy prepared in Example 1;

[0038] Figure 4 This is a diagram of the tensile properties of the magnesium-aluminum-manganese-yttrium-zirconium alloy prepared in Example 1. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] The term "include" or "comprising" in the present invention is an open description containing the specified components or steps described, and other specified components or steps that will not be substantially affected.

[0041] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0042] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.

[0043] The protective coating used in the following embodiments of the present invention is prepared by mixing talcum powder, water and water glass in a mass volume ratio of 80g:250mL:20g, and the protective coating is evenly applied on the surfaces of the crucible, crucible tongs and stirring rod before preparation; the magnesium-manganese mass ratio of the magnesium-manganese master alloy used is 9:1; the magnesium-yttrium mass ratio of the magnesium-yttrium master alloy is 7:3; the magnesium-zirconium mass ratio of the magnesium-zirconium master alloy is 7:3; the purity of each metal raw material used is greater than 99.99%.

[0044] Example 1

[0045] This embodiment provides an ultra-high strength corrosion-resistant low-alloyed Mg-Al-Mn-Y-Zr alloy, comprising the following preparation steps:

[0046] 1) removing the oxide layer from the metal raw materials and drying them, weighing 514.5 parts of Mg, 0.55 parts of Al, 5.5 parts of magnesium-manganese master alloy, 1.83 parts of magnesium-yttrium master alloy, and 1.83 parts of magnesium-zirconium master alloy;

[0047] 2) Preheat the crucible to 300°C, put the magnesium metal block in the crucible, and then put them into a resistance furnace together, and introduce a protective gas formed by a mixture of SF6 and CO2 in a volume ratio of 40:1, wait for the temperature to rise to 710°C, keep it warm for 25 minutes, put the Al metal block in it, raise the furnace temperature to 720°C, keep it warm for 20 minutes, then add the magnesium-manganese master alloy to the crucible and raise the furnace temperature to 720°C, keep it warm for 20 minutes, then add the magnesium-yttrium master alloy to the crucible, then raise the furnace temperature to 720°C, keep it warm for 20 minutes, then add the magnesium-zirconium master alloy to the crucible and raise the furnace temperature to 750°C, keep it warm for 20 minutes, so that the four alloy elements Al, Mn, Y, and Zr have enough time to be fully diffused in the molten magnesium alloy liquid, so that the alloy components are homogenized to obtain the alloy liquid;

[0048] 3) After the insulation is completed, the furnace temperature is adjusted to 740°C, the alloy liquid is vigorously stirred, and the refining agent is slowly added at the same time. The whole process is maintained for 1-2 minutes until a mirror surface appears on the surface of the alloy liquid; the refining agent is composed of the following raw materials in weight percentage: MgCl2 46%, KCl 40%, BaCl2 8%, CaF2 5%; after the refining is completed, the furnace temperature is heated to 740°C and kept warm for 20 minutes. After the insulation is completed, the furnace temperature is waited to drop to 710°C, and then casting is started into a preheated and dried metal mold (the mold preheating temperature is 180°C), and finally a cylindrical ingot is cast;

[0049] 4) using wire cutting to cut off the shrinkage cavity and the bottom of the cylindrical ingot, performing mechanical processing before solution treatment, and then performing a primary solution treatment and a secondary solution treatment, followed by water quenching to obtain a solution state ingot;

[0050] The primary solution treatment temperature is 320°C and the holding time is 1h;

[0051] The secondary solution treatment temperature is 500° C. and the holding time is 3 hours.

[0052] 5) First, the oxide scale on the surface of the solid solution ingot is removed by turning to make the surface bright; then the extrusion temperature is set to 225°C, and when the temperature is reached, the polished sample is placed in a resistance furnace for insulation for 30 minutes. After the insulation is completed, the insulated sample is placed in a mold for extrusion. The extrusion temperature is 225°C, the extrusion rate is 0.1 mm / s, and the extrusion ratio is 16:1, and finally a high-strength, corrosion-resistant, low-alloyed magnesium-aluminum-manganese-yttrium-zirconium alloy is obtained.

[0053] The obtained high-strength, corrosion-resistant low-alloyed magnesium-aluminum-manganese-yttrium-zirconium alloy comprises Al: 0.1%, Mn: 0.1%, Y: 0.1%, Zr: 0.1%, unavoidable impurities < 0.05%, and the rest is magnesium.

[0054] Example 2

[0055] 1) removing the oxide layer from the metal raw materials and drying them, weighing 509.5 parts of Mg, 0.5 parts of Al, 5.5 parts of magnesium-manganese master alloy, 1.8 parts of magnesium-yttrium master alloy, and 1.8 parts of magnesium-zirconium master alloy;

[0056] 2) Preheat the crucible to 300°C, put the magnesium metal block in the crucible, and then put them into a resistance furnace together, and introduce a protective gas formed by a mixture of SF6 and CO2 in a volume ratio of 40:1, wait for the temperature to rise to 710°C, keep it warm for 25 minutes, put the Al metal block in it, raise the furnace temperature to 720°C, keep it warm for 20 minutes, then add the magnesium-manganese master alloy to the crucible and raise the furnace temperature to 720°C, keep it warm for 20 minutes, then add the magnesium-yttrium master alloy to the crucible, then raise the furnace temperature to 720°C, keep it warm for 20 minutes, then add the magnesium-zirconium master alloy to the crucible and raise the furnace temperature to 750°C, keep it warm for 20 minutes, so that the four alloy elements Al, Mn, Y, and Zr have enough time to be fully diffused in the molten magnesium alloy liquid, so that the alloy components are homogenized to obtain the alloy liquid;

[0057] 3) After the insulation is completed, the furnace temperature is adjusted to 740°C, the alloy liquid is stirred up and down with a stirring rod, and the refining agent is slowly added at the same time. The whole process is maintained for 1 minute until a mirror surface appears on the surface of the alloy liquid; the refining agent is composed of the following raw materials in weight percentage: MgCl2 38%, KCl 32%, BaCl2 5%, CaF2 3%; after the refining is completed, the furnace temperature is heated to 740°C and kept warm for 20 minutes. After the insulation is completed, the furnace temperature is waited to drop to 710°C, and then casting is started into a preheated and dried metal mold (the mold preheating temperature is 180°C), and finally a cylindrical ingot is cast;

[0058] 4) using wire cutting to cut off the shrinkage cavity and the bottom of the cylindrical ingot, performing mechanical processing before solution treatment, and then performing a primary solution treatment and a secondary solution treatment, followed by water quenching to obtain a solution state ingot;

[0059] The primary solution treatment temperature is 320°C and the holding time is 1h;

[0060] The secondary solution treatment temperature is 500° C. and the holding time is 3 hours.

[0061] 5) First, the oxide scale on the surface of the solid solution ingot is removed by turning to make the surface bright; then the extrusion temperature is set to 225°C, and when the temperature is reached, the polished sample is placed in a resistance furnace for insulation for 30 minutes. After the insulation is completed, the insulated sample is placed in a mold for extrusion. The extrusion temperature is 225°C, the extrusion rate is 0.1 mm / s, and the extrusion ratio is 16:1, and finally a high-strength, corrosion-resistant, low-alloyed magnesium-aluminum-manganese-yttrium-zirconium alloy is obtained.

[0062] The obtained high-strength, corrosion-resistant low-alloyed magnesium-aluminum-manganese-yttrium-zirconium alloy comprises Al: 0.1%, Mn: 0.1%, Y: 0.1%, Zr: 0.1%, unavoidable impurities < 0.05%, and the rest is magnesium.

[0063] Example 3

[0064] 1) removing the oxide layer from the metal raw materials and drying them, weighing 514.5 parts of Mg, 0.6 parts of Al, 6.0 parts of magnesium-manganese master alloy, 2.0 parts of magnesium-yttrium master alloy, and 2.0 parts of magnesium-zirconium master alloy;

[0065] 2) Preheat the crucible to 300°C, put the magnesium metal block in the crucible, and then put them into a resistance furnace, and introduce a protective gas formed by a mixture of SF6 and CO2 in a volume ratio of 40:1. When the temperature rises to 715°C, keep it warm for 30 minutes, put the Al metal block in it, raise the furnace temperature to 725°C, keep it warm for 25 minutes, then add the magnesium-manganese master alloy to the crucible and raise the furnace temperature to 725°C, keep it warm for 25 minutes, then add the magnesium-yttrium master alloy to the crucible, then raise the furnace temperature to 725°C, keep it warm for 25 minutes, then add the magnesium-zirconium master alloy to the crucible and raise the furnace temperature to 755°C, keep it warm for 25 minutes, so that the four alloy elements Al, Mn, Y, and Zr have enough time to be fully diffused in the molten magnesium alloy liquid, so that the alloy components are homogenized to obtain the alloy liquid;

[0066] 3) After the insulation is completed, the furnace temperature is adjusted to 745°C, the alloy liquid is stirred up and down with a stirring rod, and the refining agent is slowly added at the same time. The whole process is maintained for 2 minutes until a mirror surface appears on the surface of the alloy liquid; the refining agent is composed of the following raw materials in weight percentage: MgCl2 46%, KCl 40%, BaCl2 8%, CaF2 5%; after the refining is completed, the furnace temperature is heated to 745°C and kept warm for 25 minutes. After the insulation is completed, the furnace temperature is waited to drop to 715°C, and then casting is started into a preheated and dried metal mold (the mold preheating temperature is 200°C), and finally a cylindrical ingot is cast;

[0067] 4) using wire cutting to cut off the shrinkage cavity and the bottom of the cylindrical ingot, performing mechanical processing before solution treatment, and then performing a primary solution treatment and a secondary solution treatment, followed by water quenching to obtain a solution state ingot;

[0068] The primary solution treatment temperature is 320°C and the holding time is 1h;

[0069] The secondary solution treatment temperature is 500° C. and the holding time is 3 hours.

[0070] 5) First, the oxide scale on the surface of the solid solution ingot is removed by turning to make the surface bright; then the extrusion temperature is set to 225°C, and when the temperature is reached, the polished sample is placed in a resistance furnace for insulation for 30 minutes. After the insulation is completed, the insulated sample is placed in a mold for extrusion. The extrusion temperature is 225°C, the extrusion rate is 0.1 mm / s, and the extrusion ratio is 16:1, and finally a high-strength, corrosion-resistant, low-alloyed magnesium-aluminum-manganese-yttrium-zirconium alloy is obtained.

[0071] The obtained high-strength, corrosion-resistant low-alloyed magnesium-aluminum-manganese-yttrium-zirconium alloy comprises Al: 0.1%, Mn: 0.1%, Y: 0.1%, Zr: 0.1%, unavoidable impurities < 0.05%, and the rest is magnesium.

[0072] Comparative Example 1

[0073] The preparation method of this comparative example is the same as that of Example 1, except that the raw materials are 514.5 parts of Mg, 0.275 parts of Al, 5.5 parts of magnesium-manganese master alloy, 1.83 parts of magnesium-yttrium master alloy, and 1.83 parts of magnesium-zirconium master alloy.

[0074] Comparative Example 2

[0075] The preparation method of this comparative example is the same as that of Example 1, except that the raw materials are 514.5 parts of Mg, 1.1 parts of Al, 5.5 parts of magnesium-manganese master alloy, 1.83 parts of magnesium-yttrium master alloy, and 1.83 parts of magnesium-zirconium master alloy.

[0076] Experimental Example 1

[0077] Table 1 Mechanical properties and electrochemical properties of each experimental alloy

[0078]

[0079] Experimental Example 2

[0080] 1. XRD test was performed on the high-strength, toughness and corrosion-resistant magnesium alloy obtained in Example 1. Figure 1 As shown, the ordinate is the diffraction intensity, and the abscissa is the diffraction angle 2θ. The ultra-high strength and toughness corrosion-resistant magnesium alloy is mainly composed of α-Mg and Mg 17 Al 12 phase composition, and no diffraction peaks of other phases were observed.

[0081] 2. The high-strength, toughness and corrosion-resistant magnesium alloy prepared in Example 1 was subjected to microstructural testing. Figure 2 As shown, it can be observed that the microstructure of the high-strength, toughness and corrosion-resistant magnesium alloy is composed of long deformed grains and smaller equiaxed grains.

[0082] 3. The tensile properties of the high-strength, toughness and corrosion-resistant magnesium alloy prepared in Example 1 were tested. Figure 3As shown, the room temperature tensile yield strength of the high-strength, toughness, and corrosion-resistant magnesium alloy is 400.9 MPa, the tensile strength is 501.3 MPa, and the elongation is 5%.

[0083] 4. The corrosion resistance of the high-strength and tough corrosion-resistant magnesium alloy obtained in Example 1 was tested. Figure 4 As shown in the figure, the potentiodynamic polarization curve of the high-strength, tough and corrosion-resistant magnesium alloy was fitted with the cathode branch by Tafel using CorShow software, and the corrosion potential of the alloy was -1.44 V, the cathode branch slope was about 132.5 mV, and the corrosion current was 3.08 μA / cm 2 The corrosion rate is about 0.07mm / a.

[0084] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. An ultra-high strength, corrosion-resistant, low-alloyed Mg-Al-Mn-Y-Zr alloy, characterized in that: The composition includes the following weight percentages: Al: 0.1%; Mn: 0.1%; Y:0.1%; Zr: 0.1%, and the remainder is magnesium and unavoidable impurities.

2. The high-strength, corrosion-resistant, low-alloyed magnesium-aluminum-manganese-yttrium-zirconium alloy according to claim 1, characterized in that: High-strength, corrosion-resistant, low-alloyed magnesium-aluminum-manganese-yttrium-zirconium alloy is made of the following metal raw materials in parts by weight: Mg 509.5-514.5 parts, Al 0.5-0.6 parts, magnesium-manganese master alloy 5.5-6.0 parts, magnesium-yttrium master alloy 1.8-2.0 parts, magnesium-zirconium master alloy 1.8-2.0 parts; The magnesium-manganese mass ratio of the magnesium-manganese master alloy is 9:1; The mass ratio of magnesium to yttrium in the magnesium-yttrium master alloy is 7:3; The magnesium-zirconium mass ratio of the magnesium-zirconium master alloy is 7:

3.

3. The method for preparing the high-strength, corrosion-resistant, low-alloyed magnesium-aluminum-manganese-yttrium-zirconium alloy according to claim 2, characterized in that: The following steps are involved: 1) removing the oxide layer of the metal raw material and drying it, and then weighing the metal raw material according to the weight portion; 2) placing Mg metal in a smelting furnace under a protective atmosphere, then placing Al metal after keeping the temperature at a first temperature, then placing a magnesium-manganese master alloy after keeping the temperature at a second temperature, then placing a magnesium-yttrium master alloy after keeping the temperature at a third temperature, then placing a magnesium-zirconium master alloy after keeping the temperature at a fourth temperature, and then placing a magnesium-zirconium master alloy after keeping the temperature at a fifth temperature to obtain a molten alloy; 3) After the alloy liquid is subjected to a first cooling, a refining agent is added, and stirring, heat preservation, a second cooling, and casting are performed in sequence to obtain an ingot; 4) subjecting the ingot to a solution treatment to obtain a solid solution ingot; 5) After removing the oxide layer from the solid solution ingot, the ingot is subjected to extrusion treatment to obtain a high-strength, corrosion-resistant, low-alloyed magnesium-aluminum-manganese-yttrium-zirconium alloy.

4. The preparation method according to claim 2, characterized in that: In the step 2), the protective atmosphere is formed by mixing SF6 and CO2 in a volume ratio of 40:

1.

5. The preparation method according to claim 2, characterized in that: In the step 2), the first temperature is 710-715°C, and the insulation time is 25-30 minutes; the second temperature is 720-725°C, and the insulation time is 20-25 minutes; the third temperature is 720-725°C, and the insulation time is 20-25 minutes; the fourth temperature is 720-725°C, and the insulation time is 20-25 minutes; the fifth temperature is 750-755°C, and the insulation time is 20-25 minutes.

6. The preparation method according to claim 2, characterized in that: The amount of the refining agent used in step 3) is 1-2 wt% of the alloy liquid.

7. The preparation method according to claim 2, characterized in that: In the step 3), the refining agent is composed of the following raw materials in weight percentage: MgCl2 38-46%, KCl 32-40%, BaCl2 5-8%, and CaF2 3-5%.

8. The preparation method according to claim 2, characterized in that: In the step 3), the temperature of the first cooling is 740-745°C; the stirring time is 2-5 minutes; the insulation temperature is 750-755°C, and the insulation time is 20-25 minutes; the temperature of the second cooling is 710-715°C.

9. The preparation method according to claim 2, characterized in that: The method of the solid solution treatment in step 4) is: firstly perform a primary solid solution treatment and then perform a secondary solid solution treatment and then perform water quenching; The primary solution treatment temperature is 320°C and the holding time is 1h; The secondary solution treatment temperature is 500° C. and the holding time is 3 hours.

10. The preparation method according to claim 2, characterized in that: The extrusion treatment method in step 5) is: raising the temperature of the extrusion die to 225-230° C., placing the sample in a heat preservation state for 55-60 minutes, and then extruding at an extrusion temperature of 225° C., an extrusion rate of 0.1 mm / s, and an extrusion ratio of 16:1.

Citation Information

Patent Citations

  • Low-cost high-performance Mg-Al-Mn magnesium alloy

    CN105603281A

  • High-strength-and-ductility heat resistance pressure casting Mg-Y alloy and preparing method thereof

    CN109868402A

  • High-strength and high-corrosion-resistance ternary magnesium alloy and preparation method thereof

    CN111304510A

  • Mg-Zn-Y-Ca-Zr magnesium alloy with high strength and plasticity, weak texture and low alloy content and preparation method of Mg-Zn-Y-Ca-Zr magnesium alloy

    CN115233060A