Iron-based rare earth boron isotropic magnetic iron alloy
By adjusting the crystal particle size of RE2Fe14B type square crystal compound and forming a grain boundary phase dominated by RE and Fe, combined with the addition of carbon and heavy rare earth elements, the fine structure of iron-based rare earth boron-based magnets was optimized, and the existing materials were solved. The trade-off relationship between coercive force and magnetic flux density achieves high-performance magnet characteristics and thermal resistance.
Patent Information
- Application Number
- CN202411049822.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-12
- Filing Date
- 2021-03-11
- Publication Date
- 2024-11-22
AI Technical Summary
While the existing iron-based rare earth boron-based isotropic magnet materials are difficult to maintain a high maximum energy product (BH)max while increasing the inherent coercive force HcJ and residual magnetic flux density Br, and there is a squareness of the demagnetization curve and heat resistance. Poor sex problem.
By adjusting the alloy composition, ensure that the average crystal particle size of the RE2Fe14B type square crystal compound is within the range of 10nm to 70nm, and a grain boundary phase dominated by RE and Fe is formed around it. Combined with the addition of carbon and heavy rare earth elements, the magnet is optimized. microstructure of the structure.
In brushless DC motors below 1 horsepower (750W), the magnetic characteristics of residual magnetic flux density Br, inherent coercive force HcJ and maximum energy product (BH)max are realized, while the thermal resistance and demagnetization curve are improved. Square degree.
Smart Images

Figure CN118996248A_ABST
Abstract
Description
[0001] This application is a divisional application of the invention patent application with Chinese application number 202180019945.6 (the invention name of the original application is "Iron-based rare earth boron-based isotropic magnet alloy", and the application date of the original application is March 11, 2021). Technical Field
[0002] The present invention relates to an iron-based rare earth boron isotropic magnet alloy, a method for producing the iron-based rare earth boron isotropic magnet alloy, and a method for producing a resin-bonded permanent magnet. Background Art
[0003] In recent years, fine crystalline isotropic magnets composed of hard magnetic phases such as Nd-Fe-B and Sm-Fe-N composed of fine grains with sizes ranging from nanometers to submicrometers, and nanocomposite isotropic magnets (hereinafter referred to as "nanocomposite magnets") have been developed, in which hard magnetic phases such as Nd-Fe-B and Sm-Fe-N composed of fine grains and soft magnetic phases such as Fe-B phase and α-Fe phase exist in the same metal structure. It has been clarified through computer simulations using micromagnetism that these rare earth iron-based isotropic magnets composed of grains with sizes ranging from nanometers to submicrometers have excellent magnetic properties due to their fine grains, so in addition to static magnetointeraction, each grain is magnetically coupled through exchange interaction, and are being put into practical use as high-performance permanent magnet materials.
[0004] Until now, fine crystalline rare earth iron-based isotropic magnets have been used as a resin-bonded magnet (commonly known as a bonded magnet) with a high degree of shape freedom, which is a characteristic of isotropy. After being crushed to an average particle size of about 50μm to 200μm, it is mixed with a thermosetting resin such as an epoxy resin or a thermoplastic resin such as a nylon system and polyphenylene sulfide (PPS). It is mainly used in the electronic component industry represented by optical drives, spindle motors for hard disks, vibration motors (pager motors) for mobile phones, and various sensors. In recent years, due to the high magnetic properties of fine crystalline rare earth iron-based isotropic magnets, it is expected to be used as a brushless DC motor of about 1 horsepower (750W) or less in automobiles (including electric vehicles and hybrid vehicles) and white appliances.
[0005] In particular, in order to achieve higher performance and higher efficiency for small motors in the 100W class, the trend has shifted from conventional brushed motors using ferrite magnets to brushless DC motors using bonded magnets. For bonded magnets using fine-crystalline rare earth iron-based isotropic magnet materials used in spindle motors, vibration motors, etc., magnet materials with better residual magnetic flux density Br, inherent coercive force HcJ and maximum energy product (BH)max are required.
[0006] In order to meet the requirements of magnetic properties, it is necessary to maximize the volume ratio of the ferromagnetic phase that exhibits hard or soft magnetic properties and minimize the volume ratio of the non-magnetic phase that forms the grain boundary of the hard magnetic phase. 14 The main phase is a B-type (RE is a rare earth element) compound, and there is a non-magnetic grain boundary phase containing boron surrounding the main phase, thereby adjusting the magnetic intercommunication between the main phase particles and obtaining an intrinsic coercive force HcJ of more than 700 kA / m that can be used in various high-performance motors. 14 In order to increase the volume ratio of B-type compounds, it is necessary to reduce the boron content. However, when the boron content is reduced excessively, the squareness of the demagnetization curve decreases, resulting in a decrease in the residual magnetic flux density Br and the maximum energy product (BH) max. Therefore, there is no practical material that can make the boron content ratio below 0.9 mass%. It is expected that the isotropic rare earth iron boron magnet material with excellent magnetic properties can be achieved by reducing the boron content concentration.
[0007] Nd2Fe 14 The isotropic magnet with B-type tetragonal compound as the main phase has a basic stoichiometric composition of Nd:Fe:B=11.76:Remainder:5.88, but in order to achieve a residual magnetic flux density Br≥0.85T that can be used in various high-performance motors, Nd≤11.76atomic% and B≤5.88atomic% are required. However, in this composition range, the inherent coercive force HcJ of 700kA / m or more required for the development of brushless DC motors of about 1 horsepower (750W) or less for automobiles (including electric vehicles and hybrid vehicles) and white appliances cannot be obtained.
[0008] In addition, Nd2Fe 14 In the isotropic iron-based rare earth nanocomposite magnet alloy with B-type tetragonal compound as the main phase, Nd2Fe 14 The B phase and the α-Fe phase or the Fe-B phase exist in the same metal structure in a nanometer-level crystal grain size, and thus the exchange interaction between the grains acts like a magnet, thus obtaining excellent permanent magnet properties. However, it is impossible to improve the RE2Fe 14 Therefore, no RE-Fe-B based isotropic permanent magnet material showing sufficient magnetic properties has been found.
[0009] Patent Document 1 discloses a method of using RE2Fe 14 B is an anisotropic sintered magnet with a tetragonal crystal structure as the main phase. The magnet is composed of micron-sized RE2Fe14 B is a metal structure composed of tetragonal crystal grains, and the magnetic moment is oriented in RE2Fe 14 B is a magnet with good magnetic properties because the C-axis of the tetragonal crystal is aligned. However, as an isotropic magnet with randomly arranged magnetic moments, good magnetic properties cannot be obtained and it cannot be used as a practical magnet.
[0010] Patent Document 2 discloses a RE2Fe2O3 composite material composed of at least 10 atomic % of rare earth elements, about 0.5 atomic % to about 10 atomic % of boron, and the remainder of iron. 14 B isotropic permanent magnets with a hard magnetic phase as the main phase of the tetragonal crystal structure have obtained a high intrinsic coercivity HcJ of up to 1460kA / m, but RE2Fe 14 The particle size of B-type grains is 20nm to 400nm, containing more than RE2Fe 14 The single domain crystal size of the B-type crystal grains is small. As a result, the magnetization is reduced. Even in the example with the best magnetic properties, the maximum residual magnetic flux density Br is only 0.83T, and the maximum energy product (BH)max is only 103kJ / m 3 Therefore, the magnetic properties required for the development of brushless DC motors of about 1 horsepower (750 W) or less for automobiles (including electric vehicles and hybrid vehicles) and white household appliances have not been achieved.
[0011] Patent Documents 3 and 4 disclose iron-based rare earth isotropic nanocomposite magnets. These iron-based rare earth isotropic nanocomposite magnets mainly contain α-Fe phase as a soft magnetic phase, so it is possible to obtain a high residual flux density Br of more than 0.9 T, but the squareness of the demagnetization curve is poor, and the demagnetization resistance and heat resistance are poor, so they are not suitable as permanent magnet materials used in automobiles and white appliances.
[0012] On the other hand, Patent Document 5 discloses that in an iron-based rare earth isotropic nanocomposite magnet mainly containing an iron-based boride phase as a soft magnetic phase, Ti is added to suppress the precipitation and growth of the α-Fe phase during the cooling process of the molten alloy, thereby making the Nd2Fe 14 The precipitation and growth of the B phase proceeds first. However, Ti is easily combined with boron (B), and the TiB2 phase is crystallized during the crystallization process, so Nd2Fe 14 There is a problem that the absolute amount of boron required for the formation of the B phase is reduced, and the expected intrinsic coercive force HcJ cannot be obtained according to the content concentration of the rare earth element.
[0013] Patent Document 6 discloses an iron-based rare earth isotropic nanocomposite magnet mainly containing an iron-based boride phase as a soft magnetic phase, and teaches that the following effects are obtained by adding Ti and carbon (C).
[0014] 1. The liquidus temperature of the molten alloy is reduced by 5°C or more (e.g., about 10°C or more and about 40°C or less). When the liquidus temperature of the molten alloy is reduced by adding carbon, the crystallization of the coarse TiB2 phase is suppressed even if the temperature of the molten alloy is reduced accordingly, so the viscosity of the molten alloy hardly increases. As a result, a stable molten alloy flow can be continuously formed during the rapid cooling process of the molten alloy.
[0015] 2. If the temperature of the molten alloy is lowered, sufficient cooling can be achieved on the surface of the cooling roll, thereby preventing winding on the cooling roll and making the structure of the rapidly solidified alloy uniform and fine.
[0016] 3. Due to the high concentration of (B+C) and high amorphous forming ability, even if the cooling rate of the molten alloy is as low as 10 2 ℃ / sec~10 4 ℃ / second, and it is easy to obtain a fine metal structure. Therefore, without precipitating a coarse α-Fe phase, it is possible to produce a Nd2Fe 14 B phase of the quenched alloy.
[0017] As described above, it is believed that in the iron-based rare earth isotropic nanocomposite magnet described in Patent Document 6, which requires the addition of Ti, the uniform and fine Nd2Fe 14 The hard magnetic phase of the B-type crystal structure and the soft magnetic phase composed of the Fe phase and the Fe-B phase coexist in the same metal structure, thereby obtaining excellent permanent magnet properties. However, Ti, which is an essential element, is a non-magnetic element and does not enter Nd2Fe as a compound. 14 The B phase, the Fe phase, and the Fe—B phase are dispersed in the grain boundaries, resulting in a decrease in magnetization and failure to achieve sufficient magnetic properties.
[0018] Prior art literature
[0019] Patent Literature
[0020] Patent Document 1: Japanese Patent Application Laid-Open No. 59-46008
[0021] Patent Document 2: Japanese Patent Application Laid-Open No. 60-9852
[0022] Patent Document 3: Japanese Patent Application Laid-Open No. 8-162312
[0023] Patent Document 4: Japanese Patent Application Laid-Open No. 10-53844
[0024] Patent Document 5: Japanese Patent Application Publication No. 2002-175908
[0025] Patent Document 6: Japanese Patent Application Publication No. 2003-178908 Summary of the invention
[0026] In order to be applied to various high-performance motors, the intrinsic coercivity HcJ ≥ 700 kA / m is a necessary condition, so it is necessary to make RE2Fe as the main phase 14 The composition ratio of the B phase is more than 70 volume %, and in order to obtain the desired residual magnetic flux density Br ≥ 0.85T, non-magnetic additive elements that do not form compounds such as Ti are suppressed as much as possible, and the interaction between each particle is utilized to the maximum extent. Therefore, there is a problem of miniaturizing the grain size to an average crystal grain size of more than 10nm and less than 70nm so that the exchange interaction can work effectively.
[0027] In addition, the inherent coercivity HcJ and the residual magnetic flux density Br are in a trade-off relationship. In order to increase the inherent coercivity HcJ, the increase in the magnetic flux density by RE2Fe 14 When the volume ratio of the main phase composed of B-type hard magnetic compounds is reduced, the residual magnetic flux density Br is reduced. Therefore, in order to suppress the reduction of the residual magnetic flux density Br, in addition to increasing the exchange interaction between the particles by using the above-mentioned uniform and fine metal organization, it is also necessary to make the grain boundary phase adjacent to the main phase a hard magnetic or semi-hard magnetic phase with high magnetization and a certain degree of anisotropic magnetic field.
[0028] The present inventors considered whether it is possible to 14 The main adjacent grain boundary phase composed of B-type hard magnetic compounds is hard magnetic or semi-hard magnetic to obtain a permanent magnet material with excellent magnetic properties that have not been available before. However, as mentioned above, it is difficult to suppress the decrease in residual magnetic flux density Br while maintaining a high inherent coercive force HcJ when adding elements such as Ti.
[0029] The present invention is made in view of the above situation, and its main purpose is to provide an iron-based rare earth boron isotropic magnet alloy that can improve the magnetic properties required for development as a brushless DC motor of about 1 horsepower (750W) or less for automobiles (including electric vehicles, hybrid vehicles) and white household appliances, namely, the residual magnetic flux density, the inherent coercive force HcJ and the maximum energy product (BH)max, a method for manufacturing the above-mentioned iron-based rare earth boron isotropic magnet alloy, and a method for manufacturing a resin-bonded permanent magnet containing the above-mentioned iron-based rare earth boron isotropic magnet alloy.
[0030] The iron-based rare earth boron-based isotropic magnet alloy of the present invention has the following alloy composition in the first embodiment: having a composition formula T 100-x-y-z (B 1-n C n ) x REy M z (T is at least one element selected from Fe, Co and Ni and is a transition metal element that must contain Fe, RE is at least one rare earth element that must contain Nd among Nd and Pr, and M is one or more metal elements selected from Al, Si, V, Cr, Ti, Mn, Cu, Zn, Ga, Zr, Nb, Mo, Ag, Hf, Ta, W, Pt, Au and Pb), and the composition ratios x, y and z respectively satisfy 4.2 atomic % ≤ x ≤ 5.6 atomic %, 11.5 atomic % ≤ y ≤ 13.0 atomic %, 0.0 atomic % ≤ z ≤ 5.0 atomic % and 0.0 ≤ n ≤ 0.5; and the metal structure is as follows: B contains a concentration lower than RE2Fe 14 The stoichiometric composition of the B-type tetragonal compound is RE2Fe with an average crystal particle size of 10 nm or more and less than 70 nm. 14 B-type tetragonal compound is the main phase, compared with RE2Fe 14 The single magnetic domain critical diameter of B-type tetragonal compounds is very small.
[0031] The iron-based rare earth boron-based isotropic magnet alloy of the present invention has the following alloy composition in the second embodiment: having a composition formula T 100-x-y-z (B 1-n C n ) x RE y M z (T is at least one element selected from Fe, Co and Ni and is a transition metal element that must contain Fe, RE is at least one rare earth element that must contain Nd among Nd and Pr, and M is one or more metal elements selected from Al, Si, V, Cr, Ti, Mn, Cu, Zn, Ga, Zr, Nb, Mo, Ag, Hf, Ta, W, Pt, Au and Pb), and the composition ratios x, y and z respectively satisfy the composition of 4.2 atomic % ≤ x ≤ 5.6 atomic %, 11.5 atomic % ≤ y ≤ 13.0 atomic %, 0.0 atomic % ≤ z ≤ 5.0 atomic % and 0.0 ≤ n ≤ 0.5, and have the following metal structure: B contains less than RE2Fe in concentration 14 The stoichiometric composition of the B-type tetragonal compound is RE2Fe with an average crystal particle size of 10 nm or more and less than 70 nm. 14 The B-type tetragonal compound is a main phase, and a grain boundary phase exists surrounding the main phase.
[0032] The method for producing an iron-based rare earth boron-based isotropic magnet alloy of the present invention comprises the following steps: a step of preparing a molten alloy having the following composition: 100-x-y-z (B 1-n C n )x RE y M z (T is at least one element selected from Fe, Co and Ni and is a transition metal element that must contain Fe, RE is a rare earth element that does not substantially contain at least one of La and Ce, and M is one or more metal elements selected from Al, Si, V, Cr, Ti, Mn, Cu, Zn, Ga, Zr, Nb, Mo, Ag, Hf, Ta, W, Pt, Au and Pb), and the composition ratios x, y and z respectively satisfy 4.2 atomic % ≤ x ≤ 5.6 atomic %, 11.5 atomic % ≤ y ≤ 13.0 atomic %, 0.0 atomic % ≤ z ≤ 5.0 atomic % and 0.0 ≤ n ≤ 0.5; the above-mentioned molten alloy is ejected from each orifice arranged at the front end of the nozzle at an average discharge rate of 200 g / min or more and less than 2000 g / min onto the surface of a rotating roller mainly composed of Cu, Mo, W or an alloy containing at least one of these metals, thereby producing a molten alloy having 1 volume % or more of RE2Fe 14 A step of rapidly solidifying the alloy by quenching any one of the crystalline phase and the amorphous phase of the B phase.
[0033] The manufacturing method of the resin-bonded permanent magnet of the present invention comprises in the first mode: a process of preparing iron-based rare earth boron isotropic magnet alloy powder manufactured by the manufacturing method of the above-mentioned iron-based rare earth boron isotropic magnet alloy; after adding thermosetting resin to the above-mentioned iron-based rare earth boron isotropic magnet alloy powder, filling it into a molding mold, and then forming a compressed molded body through compression molding, and then heat treating it above the polymerization temperature of the above-mentioned thermosetting resin.
[0034] The manufacturing method of the resin-bonded permanent magnet of the present invention in the second mode comprises: a process of preparing iron-based rare earth boron isotropic magnet alloy powder manufactured by the above-mentioned method of manufacturing iron-based rare earth boron isotropic magnet alloy; adding thermoplastic resin to the above-mentioned iron-based rare earth boron isotropic magnet alloy powder to make a compound for injection molding, and then performing injection molding.
[0035] According to the present invention, it is possible to provide an iron-based rare earth boron isotropic magnet alloy that can improve the magnetic properties required for the development of brushless DC motors of about 1 horsepower (750W) or less in automobiles (including electric vehicles and hybrid vehicles) and white appliances, namely, residual magnetic flux density Br, inherent coercive force HcJ, and maximum energy product (BH)max. In addition, according to the present invention, it is possible to provide a method for manufacturing the above-mentioned iron-based rare earth boron isotropic magnet alloy. Furthermore, according to the present invention, it is possible to provide a method for manufacturing a resin-bonded permanent magnet containing the above-mentioned iron-based rare earth boron isotropic magnet alloy. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a cross-sectional view schematically showing an example of the iron-based rare earth boron-based isotropic magnet alloy of the present invention.
[0037] Figure 2 (a) is a diagram showing the structure of a heat treatment furnace for flash annealing, and (b) is a diagram showing the state of a rapidly solidified alloy moving inside a furnace tube.
[0038] Figure 3 This is a conceptual diagram of the thermal history of flash annealing performed in the present invention.
[0039] Figure 4 The bright field image and element mapping of the iron-based rare earth boron-based isotropic magnet alloy obtained in Example 13 were observed using a transmission electron microscope.
[0040] Figure 5 This is a bright field image and element mapping of the iron-based rare earth boron-based isotropic magnet alloy obtained in Comparative Example 38 observed using a transmission electron microscope.
[0041] Figure 6 This is the powder X-ray diffraction pattern of the rapidly solidified alloy obtained in Example 13.
[0042] Figure 7 This is a powder X-ray diffraction pattern of the rapidly solidified alloy obtained in Example 13 after flash annealing (crystallization heat treatment).
[0043] Figure 8 This is a powder X-ray diffraction pattern of the rapidly solidified alloy obtained in Comparative Example 38 after flash annealing (crystallization heat treatment). DETAILED DESCRIPTION
[0044] The following describes the iron-based rare earth boron isotropic magnet alloy of the present invention, the method for manufacturing the iron-based rare earth boron isotropic magnet alloy of the present invention, and the method for manufacturing the resin-bonded permanent magnet of the present invention. It should be noted that the present invention is not limited to the following configurations, and can be appropriately changed without departing from the scope of the present invention. In addition, the configuration obtained by combining multiple preferred configurations described below is also the present invention.
[0045] The iron-based rare earth boron-based isotropic magnet alloy of the present invention is characterized in that, in a first embodiment, it has the following alloy composition: 100-x-y-z (B 1-n C n ) x RE y M z(T is at least one element selected from Fe, Co and Ni and is a transition metal element that must contain Fe, RE is at least one rare earth element that must contain Nd among Nd and Pr, and M is one or more metal elements selected from Al, Si, V, Cr, Ti, Mn, Cu, Zn, Ga, Zr, Nb, Mo, Ag, Hf, Ta, W, Pt, Au and Pb), and the composition ratios x, y and z respectively satisfy 4.2 atomic % ≤ x ≤ 5.6 atomic %, 11.5 atomic % ≤ y ≤ 13.0 atomic %, 0.0 atomic % ≤ z ≤ 5.0 atomic % and 0.0 ≤ n ≤ 0.5; and the metal structure is as follows: B contains a concentration lower than RE2Fe 14 The stoichiometric composition of the B-type tetragonal compound is RE2Fe with an average crystal particle size of 10 nm or more and less than 70 nm. 14 B-type tetragonal compound is the main phase, compared with RE2Fe 14 The single magnetic domain critical diameter of B-type tetragonal compounds is very small.
[0046] The iron-based rare earth boron-based isotropic magnet alloy of the present invention is characterized in that it has the following alloy composition: having a composition formula T 100-x-y-z (B 1-n C n ) x RE y M z (T is at least one element selected from Fe, Co and Ni and is a transition metal element that must contain Fe, RE is at least one rare earth element that must contain Nd among Nd and Pr, and M is one or more metal elements selected from Al, Si, V, Cr, Ti, Mn, Cu, Zn, Ga, Zr, Nb, Mo, Ag, Hf, Ta, W, Pt, Au and Pb), and the composition ratios x, y and z respectively satisfy 4.2 atomic % ≤ x ≤ 5.6 atomic %, 11.5 atomic % ≤ y ≤ 13.0 atomic %, 0.0 atomic % ≤ z ≤ 5.0 atomic % and 0.0 ≤ n ≤ 0.5; and the metal structure is as follows: B contains a concentration lower than RE2Fe 14 The stoichiometric composition of the B-type tetragonal compound is RE2Fe with an average crystal particle size of 10 nm or more and less than 70 nm. 14 An example of the iron-based rare earth boron-based isotropic magnet alloy of the present invention is shown in FIG. Figure 1 .
[0047] In the second embodiment of the present invention, the iron-based rare earth boron-based isotropic magnet alloy preferably has a ratio of RE2Fe 14The single magnetic domain critical diameter of B-type tetragonal compound is fine metal structure, surrounded by RE2Fe 14 The grain boundary phase of the main phase composed of the B-type tetragonal compound contains RE and Fe as main components.
[0048] In the second embodiment of the iron-based rare earth boron isotropic magnet alloy of the present invention, it is preferred that the RE2Fe 14 The grain boundary phase containing RE and Fe as main components of the main phase composed of the B-type tetragonal compound is a ferromagnetic phase.
[0049] In the second embodiment of the iron-based rare earth boron isotropic magnet alloy of the present invention, it is preferred that the RE2Fe 14 The width of the grain boundary phase mainly composed of RE and Fe in the main phase composed of the B-type tetragonal compound is 1 nm or more and less than 10 nm.
[0050] The iron-based rare earth boron-based isotropic magnet alloy of the present invention is characterized by a low boron content, so that RE2Fe 14 The boron (B) content of the alloy composition range of the magnet alloy with B phase as the main phase is about 2.5% of RE2Fe 14 The stoichiometric composition of the B phase is in the range of 4.2 atomic % to 5.6 atomic %. Furthermore, in the iron-based rare earth boron-based isotropic magnet alloy of the present invention, rare earth elements (RE) and iron (Fe) are in excess in the same alloy structure to form RE2Fe2O3 as the main phase. 14 The B phase is a grain boundary phase composed of an excess amount of RE and Fe which is not necessary for the B phase. Therefore, the iron-based rare earth boron-based isotropic magnet alloy of the present invention has RE2Fe surrounding an average crystal grain size of 10 nm or more and less than 70 nm. 14 The B phase has RE and Fe as main components and has a unique fine metal structure of a grain boundary phase having a width of 1 nm or more and less than 10 nm.
[0051] The present inventors have found that by realizing the above-mentioned unique uniform and fine metal structure, RE2Fe 14 The B phase is combined with the grain boundary phase composed mainly of RE and Fe uniformly around the main phase by strong exchange interaction in addition to static magnetointeraction, and acts as a hard magnetic phase that is integrated with the grain boundary phase (for example, α-Fe phase) having a saturation magnetization intensity equal to or greater than that of the main phase, thereby preventing RE2Fe from being damaged. 14 In the case of the inherent coercive force HcJ of the B phase, a high residual magnetic flux density Br and a high maximum energy product (BH)max based on the improved squareness of the demagnetization curve are obtained. In particular, it is believed that having the grain boundary phase as described above helps to show a high inherent coercive force HcJ, and it is believed that having a small average crystal grain size as described above helps to show a high residual magnetic flux density Br and inherent coercive force HcJ.
[0052] When the boron content is less than 4.2 atomic %, the RE2Fe 14 The formation of B phase, therefore, the intrinsic coercivity HcJ and the residual flux density Br are significantly reduced. In addition, when the boron content exceeds 5.6 atomic%, it becomes 14 B single phase or RE2Fe 14 There is a non-magnetic B-rich phase metal structure around the B phase. Therefore, although a high inherent coercivity HcJ can be maintained, the residual magnetic flux density Br and the maximum energy product (BH)max do not increase, and sufficient magnetic properties cannot be obtained, such as residual magnetic flux density Br: 0.85T or more, inherent coercivity HcJ: 700kA / m or more and less than 1400kA / m, maximum energy product (BH)max: 120kJ / m 3 The above magnetic properties.
[0053] On the other hand, it is believed that when the boron content is set to 4.2 atomic % to 5.6 atomic %, the RE2Fe 14 When the B phase is generated, a grain boundary phase mainly composed of RE and Fe is uniformly generated, so the above-mentioned magnetic properties are obtained.
[0054] Patent Documents 2, 3, 4, 5 and 6 all disclose RE2Fe 14 B-type tetragonal compound is responsible for the intrinsic coercivity HcJ of the microcrystalline isotropic permanent magnet material, but the size of the intrinsic coercivity HcJ depends largely on RE2Fe 14 Volume ratio of B-type tetragonal compound, RE2Fe 14 The higher the volume ratio of the B phase, the higher the intrinsic coercivity HcJ, and RE2Fe 14 The lower the volume ratio of the B phase is, the lower the intrinsic coercive force HcJ is.
[0055] On the other hand, the anisotropic RE2Fe 14 In the B sintered magnet, RE2Fe 14 B-type tetragonal compounds contain heavy rare earth elements such as Dy and Tb, which can increase the RE2Fe 14 The anisotropic magnetic field of the B-type tetragonal compound is improved to achieve the improvement of the intrinsic coercive force HcJ. 14 B-type tetragonal compound as the main phase, but the main phase size of anisotropic sintered magnet is about 1μm~10μm, which is RE2Fe 14Therefore, the anisotropic sintered magnet is in a multi-domain state before magnetization, and the magnetic moments are aligned in the magnetization direction (C-axis direction) by magnetization, becoming a single domain state, showing permanent magnet characteristics. Therefore, the intrinsic coercive force HcJ of the anisotropic sintered magnet represents the ability to keep the magnetic moments aligned in the same direction, so the RE2Fe 14 The anisotropic magnetic field of the B-type tetragonal compound increases, thereby increasing the intrinsic coercive force HcJ.
[0056] In the iron-based rare earth boron-based isotropic magnet alloy characterized by the low boron content of the present invention, a unique metal structure having a grain boundary phase with RE and Fe as the main components is realized, so that when a heavy rare earth element such as Dy is added to the alloy composition, not only RE2Fe 14 The anisotropic magnetic field of the B-type tetragonal compound is increased, and the anisotropic magnetic field of the grain boundary phase is also increased. Therefore, it is found that the demagnetization of the magnetic moment of the main phase below the single magnetic domain crystal grain size can be suppressed by the grain boundary phase, and by adding the conventional fine crystalline isotropic RE2Fe 14 Heavy rare earth elements that have no effect in B permanent magnet materials can achieve an increase in the inherent coercive force HcJ. Therefore, according to the iron-based rare earth boron-based isotropic magnet alloy of the present invention, a high-performance isotropic RE2Fe2O3 magnet with high inherent coercive force HcJ that has never been obtained before is obtained without causing a significant decrease in the residual magnetic flux density Br. 14 B. Permanent magnet.
[0057] In addition, it was found that the iron-based rare earth boron isotropic magnet alloy characterized by the low boron content concentration of the present invention can achieve an increase in the inherent coercive force HcJ without causing a decrease in the residual magnetic flux density Br by replacing a portion of the boron (B) with carbon (C). Furthermore, the effect of improving the inherent coercive force HcJ can be increased by combining carbon (C) substitution and heavy rare earth element addition.
[0058] [Alloy composition]
[0059] The alloy composition of the iron-based rare earth boron-based isotropic magnet alloy of the present invention has the following composition: 100-x-y-z (B 1-n C n ) x RE y M z(T is at least one element selected from Fe, Co and Ni and is a transition metal element that must contain Fe, RE is at least one rare earth element that must contain Nd among Nd and Pr, and M is one or more metal elements selected from Al, Si, V, Cr, Ti, Mn, Cu, Zn, Ga, Zr, Nb, Mo, Ag, Hf, Ta, W, Pt, Au and Pb), and the composition ratios x, y and z satisfy 4.2 atomic % ≤ x ≤ 5.6 atomic %, 11.5 atomic % ≤ y ≤ 13.0 atomic %, 0.0 atomic % ≤ z ≤ 5.0 atomic % and 0.0 ≤ n ≤ 0.5 respectively. It should be noted that the composition of the magnet alloy of the present invention is analyzed by ICP mass spectrometry. In addition, combustion-infrared absorption method can be used in combination as needed.
[0060] The transition metal element T containing Fe as an essential element accounts for the balance of the above-mentioned elements. Even if a part of Fe is replaced with one or two of Co and Ni, which are also ferromagnetic elements like Fe, the desired hard magnetic properties can be obtained. However, when the substitution amount of Fe exceeds 30%, it leads to a significant decrease in the magnetic flux density, so the preferred substitution amount is in the range of 0% to 30%. It should be noted that the addition of Co not only helps to improve the magnetization, but also reduces the viscosity of the molten alloy and is effective in stabilizing the discharge rate from the nozzle when the molten alloy is quenched. The more preferred Co substitution amount is 0.5% to 30%. From the perspective of cost-effectiveness, the more preferred Co substitution amount is 0.5% to 10%.
[0061] In the iron-based rare earth boron-based isotropic magnet alloy of the present invention, when the composition ratio x of B+C is less than 4.2 atomic %, the RE2Fe 14 The amount of B+C required for the formation of B-type tetragonal compounds reduces the magnetic properties and significantly reduces the amorphous forming ability. Therefore, when the molten alloy is rapidly solidified, the α-Fe phase precipitates, resulting in the loss of the squareness of the demagnetization curve. In addition, when the composition ratio x of B+C exceeds 5.6 atomic%, the grain boundary phase with RE and Fe as the main components is not generated, and the above-mentioned magnetic properties may not be ensured. Therefore, the composition ratio x is limited to the range of 4.2 atomic% to 5.6 atomic%. The composition ratio x is preferably 4.2 atomic% to 5.2 atomic%, and more preferably 4.4 atomic% to 5.0 atomic%.
[0062] In the iron-based rare earth boron-based isotropic magnet alloy of the present invention, by replacing a part of B with C, the melting point of the molten alloy becomes lower, and the loss of refractory used during rapid solidification is reduced, so that the process cost of rapid solidification can be reduced, and the effect of improving the inherent coercive force HcJ can be obtained. However, when the substitution rate of C to B exceeds 50%, the amorphous forming ability is greatly reduced, so it is not preferred. Therefore, the substitution rate of C to B is limited to the range of 0% to 50%, that is, 0.0≤n≤0.5. It should be noted that from the perspective of the effect of improving the inherent coercive force HcJ, the substitution rate of C to B is preferably 2% to 30%, and more preferably 3% to 15%.
[0063] In the iron-based rare earth boron-based isotropic magnet alloy of the present invention, when the composition ratio y of at least one rare earth element RE, which must contain at least Nd in Nd and Pr, is less than 11.5 atomic %, a grain boundary phase mainly composed of RE and Fe is not generated, and the above-mentioned magnetic properties may not be ensured. In addition, if the composition ratio y exceeds 13.0 atomic %, it will lead to a decrease in magnetization. Therefore, the composition ratio y is limited to the range of 11.5 atomic % to 13.0 atomic %. In addition, from the viewpoint of stably ensuring the inherent coercive force HcJ, the composition ratio y is preferably RE2Fe 14 The stoichiometric composition of the B-type tetragonal compound is 11.76 to 13.0 atomic %, and more preferably 11.76 to 12.5 atomic % from the viewpoint of ensuring a high residual magnetic flux density Br.
[0064] In addition, in order to obtain a higher intrinsic coercivity HcJ, the rare earth RE can be RE y =(Nd 1-l Pr l ) y , at this time, l is limited to 0.05 to 0.7. It should be noted that if the substitution rate l of Pr for Nd is too low, the effect of improving HcJ is small. In addition, when l is too high, the absolute value of the temperature coefficient β of the coercive force of the magnet alloy becomes small, so there is a concern that the heat resistance is reduced. Therefore, l is preferably 0.15 to 0.6, and more preferably 0.2 to 0.5.
[0065] In the iron-based rare earth boron-based isotropic magnet alloy of the present invention, one or more metal elements M selected from Al, Si, V, Cr, Ti, Mn, Cu, Zn, Ga, Zr, Nb, Mo, Ag, Hf, Ta, W, Pt, Au and Pb can be added. By adding the metal element M, the amorphous forming ability is improved, the inherent coercive force HcJ is improved due to the uniform refinement of the metal structure after the crystallization heat treatment, the squareness of the demagnetization curve is improved, and the magnetic properties are improved. However, if the composition ratio z of these metal elements M exceeds 5.0 atomic%, the magnetization is reduced, so the composition ratio z is limited to the range of 0.0 atomic% to 5.0 atomic%. In addition, the composition ratio z is preferably 0.0 atomic% to 4.0 atomic%, and more preferably 0.0 atomic% to 3.0 atomic%.
[0066] [Metallic structure]
[0067] In the iron-based rare earth boron-based isotropic magnet alloy of the present invention, if RE2Fe 14 If the average crystal grain size of the B-type tetragonal compound is less than 10 nm, the intrinsic coercivity HcJ decreases. If it becomes 70 nm or more, the squareness of the demagnetization curve decreases due to the decrease in the exchange interaction between the crystal particles. Therefore, in order to achieve, for example, a residual magnetic flux density Br of 0.85 T or more, an intrinsic coercivity HcJ of 700 kA / m or more and less than 1400 kA / m, and a maximum energy product (BH) max of 120 kJ / m 3 The above magnetic properties, RE2Fe 14 The average crystal particle size of the B-type tetragonal compound is limited to the range of 10 nm or more and less than 70 nm. 14 The average crystal particle size of the B-type tetragonal compound is preferably 15 nm to 60 nm, more preferably 15 nm to 50 nm.
[0068] RE2Fe 14 The average crystal particle size of the B-type tetragonal compound refers to the average value of the circle-equivalent diameters of particles existing in the field of view when the particle sizes of particles at three or more locations are measured by the line segment method using a transmission electron microscope (TEM).
[0069] It should be noted that the above-mentioned RE2Fe 14When the width of the grain boundary phase composed of the main phase of the B-type tetragonal compound, which is mainly composed of RE and Fe, is less than 1nm, the binding force acting between the main phase particles increases, resulting in a decrease in the inherent coercive force HcJ. In addition, if the width of the grain boundary phase becomes greater than 10nm, the reverse coupling between particles is weakened, and the squareness of the demagnetization curve decreases. Therefore, the width of the grain boundary phase is preferably greater than 1nm and less than 10nm, more preferably 2nm to 8nm, and further preferably 2nm to 5nm. It should be noted that the width of the grain boundary phase is obtained by image analysis of a bright field image taken using a scanning transmission electron microscope under the conditions of an acceleration voltage of 200kV and an observation magnification of 900,000 times.
[0070] In the iron-based rare earth boron-based isotropic magnet alloy of the present invention, in the second embodiment, the RE2Fe 14 In the composition ratio of the grain boundary phase composed of RE and Fe as the main components of the main phase composed of the B-type tetragonal compound, it is preferred that the ratio of the main phase is 70 volume % or more and less than 99 volume %, and the ratio of the grain boundary phase is 1 volume % or more and less than 30 volume %. Thus, for example, it is easy to achieve a residual magnetic flux density Br of 0.85T or more, an inherent coercive force HcJ of 700kA / m or more and less than 1400kA / m, and a maximum energy product (BH)max of 120kJ / m 3 The ratio of the main phase is preferably 80% by volume or more and less than 99% by volume, and more preferably 90% by volume or more and less than 98% by volume. It should be noted that the composition ratio of the main phase to the grain boundary phase is obtained by image analysis of a bright field image taken using a scanning transmission electron microscope at an acceleration voltage of 200 kV and an observation magnification of 900,000 times.
[0071] [Magnetic properties]
[0072] The iron-based rare earth boron-based isotropic magnet of the present invention can exhibit, for example, a residual magnetic flux density Br of 0.85 T or more, an intrinsic coercive force HcJ of 700 kA / m or more and less than 1200 kA / m, and a maximum energy product (BH)max of 120 kJ / m, as described below. 3The above magnetic properties, but when used in various rotating machines for electrical equipment and white appliances with a power of less than 1 horsepower (750W), when it becomes a magnetic circuit structure that easily applies a reverse magnetic field to permanent magnets such as surface magnet type rotors (SPM type rotors), the inherent coercive force HcJ is preferably 800kA / m or more, and more preferably 950kA / m or more. It should be noted that when the inherent coercive force HcJ is more than 1400kA / m, the magnetization is significantly reduced, so the inherent coercive force HcJ is preferably less than 1300kA / m, and more preferably less than 1250kA / m. In addition, for the residual magnetic flux density Br, when a magnet embedded rotor (IPM type rotor) is used, it can be driven at a higher operating point (magnetic permeability) than the SPM type. Therefore, although the residual magnetic flux density Br is as high as possible, if the balance with the inherent coercive force HcJ is considered, the residual magnetic flux density Br is preferably more than 0.87T, and more preferably more than 0.9T.
[0073] It should be noted that the reason why the residual magnetic flux density Br is taken as an example and is made 0.85T or more is that when the isotropic bonded magnet is used in a DC brushless motor, the operating point (magnetic permeability Pc) of the magnet becomes about 3 to 10. Therefore, if the residual magnetic flux density Br is ≥ 0.85T, then within the Pc range, the maximum energy product (BH) max is 300kJ / m 3 The above-mentioned effective magnetic flux Bm is at the same level as the anisotropic Nd-Fe-B sintered magnet. It should be noted that the residual magnetic flux density Br is more preferably 0.86T or more.
[0074] In addition, the reason why the inherent coercive force HcJ is taken as an example and is made 700kA / m or more is that when the inherent coercive force HcJ is less than 700kA / m, when it is applied to a DC brushless motor as an isotropic bonded magnet, the heat resistance temperature of the motor cannot be guaranteed to be 100°C, and the desired motor characteristics may not be obtained due to thermal demagnetization. In addition, the reason why the inherent coercive force HcJ is made less than 1400kA / m is that when the inherent coercive force HcJ is more than 1400kA / m, it is difficult to magnetize, and it is difficult to perform multi-pole magnetization for ensuring Pc: 3 to 10.
[0075] Furthermore, the maximum energy product (BH)max is taken as an example and is set to 120 kJ / m 3 The reason for the above is that the maximum energy product (BH)max is less than 120kJ / m 3 When the squareness ratio of the demagnetization curve (residual magnetization Jr / saturation magnetization intensity Js) becomes less than 0.8, when it is used as an isotropic bonded magnet in a DC brushless motor, the magnetic properties are reduced due to the reverse magnetic field generated when the motor is operating, and the desired motor characteristics may not be obtained.
[0076] The method for producing the iron-based rare earth boron-based isotropic magnet alloy of the present invention is characterized by comprising the steps of: preparing a molten alloy having the following composition: 100-x-y-z (B 1-n C n ) x RE y M z (T is at least one element selected from Fe, Co and Ni and is a transition metal element that must contain Fe, RE is at least one rare earth element that does not substantially contain La and Ce, and M is one or more metal elements selected from Al, Si, V, Cr, Ti, Mn, Cu, Zn, Ga, Zr, Nb, Mo, Ag, Hf, Ta, W, Pt, Au and Pb), and the composition ratios x, y and z respectively satisfy 4.2 atomic % ≤ x ≤ 5.6 atomic %, 11.5 atomic % ≤ y ≤ 13.0 atomic %, 0.0 atomic % ≤ z ≤ 5.0 atomic % and 0.0 ≤ n ≤ 0.5; the above-mentioned molten alloy is ejected from each orifice arranged at the front end of the nozzle at an average discharge rate of 200 g / min or more and less than 2000 g / min onto the surface of a rotating roller mainly composed of Cu, Mo, W or an alloy containing at least one of these metals, thereby producing a molten alloy having 1 volume % or more of RE2Fe 14 The process of rapidly solidifying the alloy of any one of the crystalline phase and the amorphous phase of the B phase. It should be noted that RE is a rare earth element substantially free of La and Ce, and as an example, it can be at least one rare earth element of Nd and Pr that must contain Nd. The details are as described above.
[0077] [Quick cooling of molten alloy]
[0078] In the method for producing an iron-based rare earth boron-based isotropic magnet alloy of the present invention, after the prepared raw materials are melted to have a predetermined alloy composition to form a molten alloy, the molten alloy is ejected from each orifice disposed at the front end of the nozzle at an average discharge rate of 200 g / min or more and less than 2000 g / min onto the surface of a rotating roller mainly composed of Cu, Mo, W or an alloy containing at least one of these metals, thereby producing a magnet having a content of 1 volume % or more of RE2Fe 14If the average discharge rate of the rapidly solidified alloy of any one of the crystalline phase and the amorphous phase of the B phase is less than 200 g / min, the productivity is poor. When it is above 2000 g / min, it becomes a molten alloy rapidly cooled alloy structure containing a coarse α-Fe phase. Therefore, even if a crystallization heat treatment is performed, the above-mentioned magnetic properties may not be obtained. Therefore, the average discharge rate of each orifice arranged at the front end of the nozzle is limited to a range of more than 200 g / min and less than 2000 g / min. It should be noted that the average discharge rate is preferably 300 g / min to 1500 g / min, and more preferably 400 g / min to 1300 g / min.
[0079] The hole for discharging the molten alloy at the front end of the nozzle is not a circular orifice, and a slit shape is allowed as long as the hole shape can ensure the prescribed discharge rate, regardless of the shape of square, triangle, ellipse, etc. In addition, the nozzle material is allowed as long as it is a refractory material that does not react or is difficult to react with the molten alloy, but it is preferably a ceramic material, SiC, C or BN that has little loss to the nozzle hole during the discharge of the molten alloy, more preferably BN, and more preferably hard BN containing additives.
[0080] When making the above-mentioned rapid solidification alloy, the viscosity of the molten alloy is suppressed by preventing oxidation of the molten alloy, and a stable discharge rate can be maintained, so the rapid solidification atmosphere is preferably an oxygen-free or low-oxygen atmosphere. In order to achieve this atmosphere, it is necessary to evacuate the rapid solidification device to below 20Pa, preferably below 10Pa, and more preferably below 1Pa, and then introduce an inert gas into the rapid solidification device, so that the oxygen concentration in the rapid solidification device is below 500ppm, preferably below 200ppm, and more preferably below 100ppm, and then implement rapid solidification. As an inert gas, rare gases such as helium and argon, and nitrogen can be used, but nitrogen is easier to react with rare earth elements and iron, so rare gases such as helium and argon are preferred, and argon is more preferred from a cost perspective.
[0081] In the process of making a quenched solidified alloy, the rotating roller that quenches the molten alloy has Cu, Mo, W or an alloy containing at least one of these metals as the main component, but it is preferred to have a substrate containing such a main component. This is because these substrates have excellent thermal conductivity and durability. In addition, by implementing Cr, Ni or a combination of plating on the surface of the substrate of the rotating roller, the heat resistance and hardness of the substrate surface of the rotating roller can be improved, and the melting and degradation of the substrate surface of the rotating roller during quenched solidification can be suppressed. It should be noted that the diameter of the rotating roller is, for example, Φ200mm to Φ20000mm. As long as the quenched solidification time is a short time of less than 10 seconds, there is no need to water-cool the rotating roller. When the quenched solidification time exceeds 10 seconds, it is preferred to flow cooling water inside the rotating roller to suppress the temperature rise of the rotating roller substrate. The water cooling capacity of the rotating roller is preferably calculated based on the solidification latent heat per unit time and the discharge rate, and appropriately optimized and adjusted.
[0082] [Flash Annealing]
[0083] The method for manufacturing an iron-based rare earth boron-based isotropic magnet alloy of the present invention preferably further comprises a step of performing flash annealing, that is, after the above-mentioned rapidly solidified alloy reaches a certain temperature range of the crystallization temperature to 850°C at a heating rate of 10°C / second or more and less than 200°C / second, it is rapidly cooled after 0.1 second or more and less than 7 minutes, and by performing the above-mentioned flash annealing, the following metal structure is formed: B content is lower than RE2Fe 14 The stoichiometric composition of the B-type tetragonal compound is RE2Fe with an average crystal particle size of 10 nm or more and less than 70 nm. 14 The main phase is a tetragonal compound of type B, and there is a grain boundary phase with a width of 1 nm or more and less than 10 nm, which is mainly composed of RE and Fe and surrounds the main phase. 14 The single magnetic domain critical diameter of B-type tetragonal compounds is very small.
[0084] When the heating rate during flash annealing (crystallization heat treatment) is less than 10°C / second, the grains grow excessively and a fine metal structure cannot be obtained, resulting in a decrease in the inherent coercive force HcJ and residual magnetic flux density Br. When the heating rate is more than 200°C / second, the grains do not grow in time and will not become RE2Fe with an average crystal grain size of more than 10nm and less than 70nm required for permanent magnet performance. 14 The main phase is a tetragonal compound of type B, and there is a grain boundary phase with a width of 1 nm or more and less than 10 nm, which is mainly composed of RE and Fe and surrounds the main phase. 14The metal structure with a fine single magnetic domain critical diameter of the B-type tetragonal compound leads to a decrease in magnetic properties in the same manner as when the temperature is less than 10°C / second. Therefore, the heating rate is preferably 10°C / second or more and less than 200°C / second, more preferably 30°C / second to 200°C / second, and further preferably 40°C / second to 180°C / second.
[0085] In the flash annealing (crystallization heat treatment) of the method for manufacturing the iron-based rare earth boron-based isotropic magnet alloy of the present invention, in order to obtain good magnetic properties, it is preferred to immediately perform rapid cooling after reaching the crystallization heat treatment temperature (holding temperature) in a certain temperature range of the crystallization temperature to 850°C. If described in detail, after reaching the above-mentioned crystallization heat treatment temperature, the holding time until rapid cooling is substantially sufficient to be more than 0.1 seconds. If it is held for more than 7 minutes, the uniform and fine metal structure is damaged, resulting in a decrease in various magnetic properties, so it is not preferred. Therefore, the holding time is preferably 0.1 seconds or more and less than 7 minutes, more preferably 0.1 seconds to 2 minutes, and further preferably 0.1 seconds to 30 seconds.
[0086] In the flash annealing (crystallization heat treatment) of the method for manufacturing the iron-based rare earth boron-based isotropic magnet alloy of the present invention, it is preferred to cool the rapidly solidified alloy to below 400°C at a cooling rate of 2°C / sec to 200°C / sec. If the cooling rate is less than 2°C / sec, the coarsening of the crystal structure proceeds, and when it exceeds 200°C / sec, the alloy may oxidize. Therefore, the cooling rate is preferably 2°C / sec to 200°C / sec, more preferably 5°C / sec to 200°C / sec, and further preferably 5°C / sec to 150°C / sec.
[0087] In order to prevent oxidation of the rapidly solidified alloy, the atmosphere of the above-mentioned flash annealing (crystallization heat treatment) is preferably an inert gas atmosphere. As the inert gas, rare gases such as helium and argon, and nitrogen can be used, but nitrogen is more likely to react with rare earth elements and iron, so rare gases such as helium and argon are preferred, and argon is more preferred from the perspective of cost.
[0088] [Crushing and molding]
[0089] The method for producing an iron-based rare earth boron isotropic magnet alloy of the present invention may further include the step of producing an iron-based rare earth boron isotropic magnet alloy powder by pulverizing the above-mentioned rapidly solidified alloy or the above-mentioned rapidly solidified alloy subjected to the above-mentioned flash annealing.
[0090] The rapidly solidified alloy obtained through the above process can be roughly cut or crushed into a thin strip of thin strips, for example, less than 50 mm before flash annealing (crystallization heat treatment). Furthermore, by crushing the magnet alloy of the present invention after flash annealing (crystallization heat treatment) into a magnet alloy powder with an appropriate average powder particle size in the range of 20 μm to 200 μm, the magnet alloy powder can be used to manufacture various resin-bonded permanent magnets (commonly known as plastic magnets or bonded magnets) through known processes.
[0091] The manufacturing method of the resin-bonded permanent magnet of the present invention is characterized in the first mode by comprising the following steps: a step of preparing iron-based rare earth boron isotropic magnet alloy powder manufactured by the above-mentioned method of manufacturing iron-based rare earth boron isotropic magnet alloy; and a step of adding a thermosetting resin to the above-mentioned iron-based rare earth boron isotropic magnet alloy powder, filling it into a molding mold, and then performing heat treatment above the polymerization temperature of the above-mentioned thermosetting resin after forming a compression molded body through compression molding.
[0092] The manufacturing method of the resin-bonded permanent magnet of the present invention is characterized in the second mode by comprising the following steps: a step of preparing iron-based rare earth boron isotropic magnet alloy powder manufactured by the above-mentioned method of manufacturing iron-based rare earth boron isotropic magnet alloy; and a step of adding thermoplastic resin to the above-mentioned iron-based rare earth boron isotropic magnet alloy powder to make a compound for injection molding, and then performing injection molding.
[0093] When making the above-mentioned resin-bonded permanent magnet, iron-based rare earth nanocomposite magnet powder is mixed with epoxy resin, polyamide, polyphenylene sulfide (PPS), liquid crystal polymer, acrylic acid, polyether, etc., and molded into a desired shape. At this time, for example, mixed magnet powder mixed with permanent magnet powders such as SmFeN magnet powder and hard ferrite magnet powder can be used.
[0094] The resin-bonded permanent magnet can be used to manufacture a brushless DC motor of about 1 horsepower (750 W) or less, which can be used for various rotating motors for automobiles (including electric vehicles and hybrid vehicles) and white appliances, as well as various magnetic sensors.
[0095] When the magnet alloy powder of the present invention is used for injection molding bonded magnets, it is preferably crushed to an average particle size of 100 μm or less, and the more preferred average crystal particle size of the powder is 20 μm to 100 μm. In addition, when used for compression molding bonded magnets, it is preferably crushed to an average particle size of 200 μm or less, and the more preferred average crystal particle size of the powder is 50 μm to 150 μm. It is further preferred that the particle size distribution has two peaks and the average crystal particle size is 80 μm to 130 μm.
[0096] In addition, by subjecting the surface of the magnet alloy powder of the present invention to surface treatments such as coupling treatment and chemical conversion treatment (including phosphoric acid treatment and glass film treatment), the moldability of the resin-bonded permanent magnet during molding, the corrosion resistance and heat resistance of the obtained resin-bonded permanent magnet can be improved regardless of the molding method. In addition, the corrosion resistance and heat resistance of the resin-bonded permanent magnet can be improved in the same way as the surface treatment of the magnet alloy powder by subjecting the surface of the resin-bonded permanent magnet after molding to surface treatments such as resin coating, chemical conversion treatment, and plating.
[0097] It should be noted that the method for manufacturing the iron-based rare earth boron isotropic magnet alloy of the present invention is not limited to the above method, and other manufacturing methods can be used as long as the iron-based rare earth boron isotropic magnet alloy having the above composition, average crystal grain size, etc. can be manufactured. For example, if flash annealing is used, RE2Fe with an average crystal grain size of 10 nm or more and less than 70 nm can be formed. 14 The fine metal structure with B-type tetragonal compound as the main phase is formed, but the formation of such a fine metal structure is not limited to flash annealing, and other methods can also be used. For example, even when a normal annealing process is adopted instead of flash annealing, the surface speed of the rotating roller that rapidly cools the molten alloy is adjusted to make the rapidly solidified alloy structure into a homogeneous fine metal structure composed of crystal grains about 5% to 20% smaller than the alloy structure that obtains the best magnetic properties. Good magnetic properties can also be obtained.
[0098] Example
[0099] Hereinafter, examples of the present invention will be described, but it should be noted that the present invention is not limited to these examples.
[0100] (Example)
[0101] 100 g of raw materials containing additive elements such as Co, Al, Si, V, Cr, Ti, Mn, Cu, Zn, Ga, Zr, Nb, Mo, Ag, Hf, Ta, W, Pt, Au, and Pb in addition to the main elements of Nd, Pr, Dy, B, C, and Fe with a purity of 99.5% or more so as to form an alloy composition as described in Table 1 were placed in an alumina melting crucible and then placed on a working coil in a vacuum melting furnace. Then, the vacuum melting furnace was evacuated to a pressure of 0.02 Pa or less, and argon gas was introduced to atmospheric pressure, and a molten alloy was prepared by high-frequency induction heating. Thereafter, the molten alloy was cast into a water-cooled copper mold to prepare a master alloy.
[0102] Next, the obtained master alloy was cut into appropriate sizes, and 40 g was inserted into a transparent quartz nozzle having orifices with different diameters (0.7 mm to 1.2 mm) appropriately arranged at the bottom so as to achieve the average discharge rate recorded in Table 1 (in Table 1, simply expressed as "discharge rate"), and then set on the working coil in the single-roll quenching device. Then, after the vacuum melting furnace was evacuated to below 0.02 Pa, argon gas was introduced until the quenching atmosphere pressure recorded in Table 1, and the master alloy was remelted by high-frequency induction heating. The molten alloy was discharged from the nozzle orifice at a jet pressure of 30 kPa onto the surface of a rotating roller rotating at the roller surface speed (Vs) recorded in Table 1 to produce a quenched solidified alloy. It should be noted that at this time, the distance between the nozzle tip and the rotating roller surface was 0.8 mm. In addition, the main component of the rotating roller is copper. In addition, the obtained quenched solidified alloy has a content of Nd2Fe of more than 1 volume %. 14 The B phase is either a crystalline phase or an amorphous phase.
[0103] Figure 6 The powder X-ray diffraction pattern of the rapidly solidified alloy obtained in Example 13 is shown in FIG. Figure 6 , confirming that Nd2Fe 14 Phase B.
[0104] The rapidly solidified alloy obtained in the above process is coarsely crushed to less than a few mm to prepare a rapidly solidified alloy powder. Then, a flash annealing furnace (crystallization heat treatment furnace, furnace core tube: made of transparent quartz and with an outer diameter of 15 mm × an inner diameter of 12.5 mm × a length of 1000 mm, a heating area of 300 mm, and a cooling area of 500 mm for the cooling fan) is used to put the coarse powder of the rapidly solidified alloy into the raw material hopper, and then heat treatment is carried out at a workpiece cutting speed of 20 g / min. It should be noted that the inclination angle of the furnace core tube, the rotation speed of the furnace core tube, and the vibration frequency of the furnace core tube are appropriately adjusted together with the heat treatment temperature and heat treatment time recorded in Table 2 so as to achieve the heating rate recorded in Table 2. As a result, the rapidly solidified alloy powder passes through the furnace core tube while undergoing a combination of stirring based on the rotation of the furnace core tube and jumping phenomena based on the vibration of the furnace core tube, so that the rapidly solidified alloy powder stone is placed under specific heat treatment conditions in which each powder is subjected to a heat history instead of being subjected to a heat history as a whole. The heat treatment furnace and the heat history in the flash annealing process are respectively at Figure 2 and Figure 3 An example is shown in FIG.
[0105] The phase composition of the rapidly solidified alloy powder after flash annealing (crystallization heat treatment) was confirmed by powder X-ray diffraction, and the presence of Nd2Fe 14 Phase B. Figure 7The powder X-ray diffraction pattern of the rapidly solidified alloy obtained in Example 13 after flash annealing (crystallization heat treatment) is shown as a representative example. Figure 6 The α-Fe peak not seen in the flash annealing (crystallization heat treatment) Figure 7 It can be seen that it is confirmed to be Nd2Fe 14 A metallic structure in which B phase and α-Fe phase exist in a mixture.
[0106] Figure 4 The bright field image and element mapping of the iron-based rare earth boron-based isotropic magnet alloy obtained in Example 13 observed by transmission electron microscopy are shown as a representative example. According to the bright field image, the presence of Nd2Fe 14 B phase and surrounding Nd2Fe 14 In addition, in the element mapping, it can be confirmed that the grain boundary of the main phase composed of the main constituent elements of Nd, Fe, and B has a grain boundary phase where Nd and Fe are concentrated. Based on the above-mentioned powder X-ray diffraction results, it is estimated that the Fe present in the grain boundary exists as an α-Fe phase. It should be noted that the present inventors have confirmed that the following Figure 4 That grain boundary phase.
[0107] The iron-based rare earth boron isotropic magnet alloy obtained by flash annealing (crystallization heat treatment) described in Table 2 was made into a sample for magnetic property evaluation with a length of about 7 mm × a width of about 0.9 mm to 2.3 mm × a thickness of 18 μm to 25 μm, and then magnetized in the long side direction with a pulsed magnetic field of 3.2 MA / m. Thereafter, in order to suppress the influence of the demagnetization field, the sample for magnetic property evaluation was set in the long side direction, and then the room temperature magnetic properties were measured using a vibrating sample magnetometer (VSM), and the results are shown in Table 3. As can be seen from Table 3, the alloy composition and preparation method described in Examples 1 to 39 obtained the above-mentioned residual magnetic flux density Br: 0.85 T or more, the inherent coercive force HcJ: 700 kA / m or more and less than 1400 kA / m, and the maximum energy product (BH) max: 120 kJ / m 3 The magnetic properties are as described above. In particular, it is found that Examples 32 to 39 containing Pr have higher intrinsic coercive forces HcJ than Examples 1 to 31.
[0108] Next, the magnetic powder obtained in Example 13 after flash annealing (crystallization heat treatment) was crushed into an average particle size of 125 μm using a pin mill. Then, 2 mass% of epoxy resin diluted with methyl ethyl ketone (MEK) was added to the crushed magnetic powder, mixed and kneaded, and 0.1 mass% of calcium stearate was added as a lubricant to prepare a composite for compression molding bonded magnets.
[0109] The above-mentioned compression molded bonded magnet composite was heated to 1568 MPa (16 ton / cm 2 ) pressure to obtain a compression molded body with a diameter of 10 mm × height of 7 mm, and then subject the compression molded body to a curing heat treatment (curing) at 180°C × 1 hour in an argon atmosphere, thereby obtaining an isotropic compression molded bonded magnet. It should be noted that the obtained isotropic compression molded bonded magnet has a molded body density of 6.3 g / cm 3 (The true specific gravity of magnetic powder is 7.5g / cm 3 ), and the magnetic powder filling rate is 84 volume %.
[0110] The magnetic properties of the isotropic compression molded bonded magnet obtained by using the magnetic powder of Example 13 were measured by a BH tracer after magnetization in the long side direction by applying a pulse magnetic field of 3.2MA / m. The results showed that the residual magnetic flux density Br: 0.74T, the inherent coercive force HcJ: 1028kA / m, and the maximum energy product (BH) max: 89.4kJ / m 3 Magnetic properties.
[0111] Next, the flash annealed (crystallization heat treated) magnetic powder obtained in Example 13 was crushed into an average particle size of 75 μm using a pin mill. Then, the crushed magnetic powder was sprayed with 0.75 mass% of a titanate coupling agent while being heated and stirred, and after the coupling treatment, 0.5 mass% of stearic acid amide and 4.75 mass% of nylon 12 resin powder as a lubricant were added and mixed, and then a continuous extruder was used to prepare a composite for injection molding bonded magnets at an extrusion temperature of 170°C.
[0112] The above-mentioned compound for injection molded bonded magnet was injection molded at an injection temperature of 250°C to produce an isotropic injection molded bonded magnet having a shape of 10 mm in diameter and 7 mm in height. The obtained isotropic injection molded bonded magnet had a molded body density of 4.6 g / cm 3 (The true specific gravity of magnetic powder is 7.5g / cm 3 ), so the magnetic powder filling rate is 61 volume %.
[0113] The magnetic properties of the isotropic injection molded bonded magnet obtained by using the magnetic powder of Example 13 were measured by using a BH tracer after magnetization in the long side direction by applying a pulse magnetic field of 3.2MA / m. The results showed a residual magnetic flux density Br: 0.54T, an inherent coercive force HcJ: 1014kA / m, and a maximum energy product (BH) max: 63.4kJ / m 3 The magnetic properties of the magnets are comparable to those of commonly used isotropic Nd-Fe-B compression molded bonded magnets even when injection molded.
[0114] (Comparative Example)
[0115] 100 g of raw materials containing additive elements such as Co, Si, Ti, and Zr in addition to the main elements of Nd, Dy, B, and Fe with a purity of 99.5% or more to form the alloy composition described in Table 1 were placed in an alumina melting crucible and then placed in a working coil in a vacuum melting furnace. Then, the vacuum melting furnace was evacuated to 0.02 Pa or less, and argon gas was introduced to normal pressure, and then a molten alloy was made by high-frequency induction heating. Thereafter, the molten alloy was cast into a water-cooled copper mold to make a master alloy.
[0116] Next, the obtained mother alloy was cut into appropriate sizes, and 40 g was inserted into a transparent quartz nozzle with orifices having different diameters (0.7 mm to 1.2 mm) appropriately arranged at the bottom so as to achieve the average discharge rate (simply indicated as "discharge rate" in Table 1), and then set in a working coil in a single roll quenching device. Then, after the vacuum melting furnace was evacuated to 0.02 Pa or less, argon gas was introduced to the quenching atmosphere pressure described in Table 1, and the mother alloy was remelted by high-frequency induction heating. The molten alloy was discharged from the nozzle hole at a spray pressure of 30 kPa onto the surface of a rotating roll rotating at the roll surface speed (Vs) described in Table 1 to produce a quenched solidified alloy. It should be noted that at this time, the distance between the nozzle tip and the rotating roll surface was 0.8 mm.
[0117] The rapidly solidified alloy obtained in the above process was coarsely crushed to a few mm or less to prepare a rapidly solidified alloy powder, and then the coarse powder of the rapidly solidified alloy was put into a raw material hopper using a flash annealing furnace (crystallization heat treatment furnace, furnace core tube: transparent quartz and outer diameter 15mm×inner diameter 12.5mm×length 1000mm, heating area 300mm, cooling area 500mm of the cooling fan), and then heat treated at a workpiece cutting speed of 20g / min. It should be noted that the furnace core tube inclination angle, furnace core tube rotation speed and furnace core tube vibration frequency were appropriately adjusted together with the heat treatment temperature and heat treatment time recorded in Table 2 so as to achieve the heating rate recorded in Table 2.
[0118] The phase composition of the rapidly solidified alloy powder after flash annealing (crystallization heat treatment) was confirmed by powder X-ray diffraction, and the presence of Nd2Fe 14 Phase B. Figure 8 The powder X-ray diffraction pattern of the rapidly solidified alloy obtained in Comparative Example 7 after flash annealing (crystallization heat treatment) is shown as a representative example. Figure 8 , confirming that Comparative Example 7 is Nd2Fe 14 A single-phase metal structure with phase B as the main phase.
[0119] Figure 5 The bright field image and element mapping of the iron-based rare earth boron-based isotropic magnet alloy obtained in Comparative Example 7 observed by transmission electron microscopy are shown as a representative example. In the bright field image, Nd2Fe 14 B phase, but no clear grain boundary phase can be confirmed. In addition, according to element mapping, it can be seen that there is no grain boundary phase in which Nd and Fe are concentrated as seen in Example 13 at the grain boundary of the main phase composed of the main constituent elements of Nd, Fe, and B. This is also the case in other comparative examples.
[0120] The iron-based rare earth boron isotropic magnet alloy obtained by flash annealing (crystallization heat treatment) described in Table 2 was made into a sample for magnetic property evaluation with a length of about 7 mm × a width of about 0.9 mm to 2.3 mm × a thickness of 18 μm to 25 μm, and then magnetized in the long side direction with a pulsed magnetic field of 3.2 MA / m. Thereafter, in order to suppress the influence of the demagnetization field, the sample for magnetic property evaluation was set in the long side direction, and the room temperature magnetic properties were measured by a vibrating sample magnetometer (VSM), and the results are shown in Table 3. It can be seen from Table 3 that the above-mentioned residual magnetic flux density Br: 0.85 T or more, inherent coercive force HcJ: 700 kA / m or more and less than 1400 kA / m, and maximum energy product (BH) max: 120 kJ / m cannot be obtained by the alloy composition and preparation method described in Comparative Examples 1 to 12. 3 The above magnetic properties.
[0121] [Table 1]
[0122]
[0123] [Table 2]
[0124]
[0125] [Table 3]
[0126]
[0127] Explanation of symbols
[0128] 1Raw material hopper
[0129] 2Raw material supply feeder
[0130] 3 Furnace core tube
[0131] 3a Enlarged view of furnace core tube
[0132] 3b furnace core tube cross-section enlarged view
[0133] 4 Tubular furnace
[0134] 5Cooling Tower
[0135] 6. Recovery hopper
[0136] 7 Vibrator
[0137] 8 Furnace core tube rotation motor
[0138] 9 Furnace core tube rotation axis
[0139] 10 device racks
[0140] 11 Furnace core tube tilt angle
[0141] 12 Cooling fan wind
[0142] 13 Rapidly solidified alloy powder (workpiece)
[0143] 14 Workpiece moving direction
[0144] 15 Workpiece jumping phenomenon
[0145] 16 Heating speed
[0146] 17. Maintain Temperature
[0147] 18 Cooling speed
[0148] 21 Main Phase
[0149] 22 Grain boundary phase
Claims
1. An iron-based rare earth boron-based isotropic magnet alloy having the following alloy composition: having a composition formula T 100-x-y-z (B 1-n C n ) x RE y M z It indicates that, T is at least one element selected from Fe, Co and Ni and is a transition metal element that must contain Fe, RE is at least one rare earth element that must contain Nd among Nd and Pr, M is one or more elements selected from Al, Si, V, Cr, Ti, Mn, Cu, Zn, Ga, Zr, Nb, Mo, Ag, Hf, Ta, W, Pt, Au and Pb, and The composition ratios x, y and z satisfy 4.2 atomic % ≤ x ≤ 5.6 atomic %, 11.5 atomic % ≤ y ≤ 13.0 atomic %, 0.0 atomic % ≤ z ≤ 5.0 atomic % and 0.0 ≤ n ≤ 0.5 respectively; And has the following metal structure: B contains a concentration lower than RE2Fe 14 The stoichiometric composition of the B-type tetragonal compound is RE2Fe with an average crystal particle size of 10 nm or more and less than 70 nm. 14 The B-type tetragonal compound is the main phase, and there is a grain boundary phase as a ferromagnetic phase. 14 The single magnetic domain critical diameter of B-type tetragonal compounds is very small.
2. The iron-based rare earth boron-based isotropic magnet alloy according to claim 1, wherein: Surrounded by RE2Fe 14 The grain boundary phase of the main phase composed of the B-type tetragonal compound contains RE and Fe as main components.
3. The iron-based rare earth boron-based isotropic magnet alloy according to claim 2, wherein: Surrounded by RE2Fe 14 The width of the grain boundary phase mainly composed of RE and Fe in the main phase composed of the B-type tetragonal compound is 1 nm or more and less than 10 nm.
4. The iron-based rare earth boron-based isotropic magnet alloy according to claim 2 or 3, wherein: Surrounded by RE2Fe 14 In the composition ratio of the main phase composed of the B-type tetragonal compound and the grain boundary phase mainly composed of RE and Fe, the ratio of the main phase is 70 volume % or more and less than 99 volume %, and the ratio of the grain boundary phase is 1 volume % or more and less than 30 volume %.
5. The iron-based rare earth boron-based isotropic magnet alloy according to any one of claims 1 to 3, wherein: The residual magnetic flux density Br is 0.85T or more, the intrinsic coercive force HcJ is 700kA / m or more and less than 1400kA / m, and the maximum energy product (BH)max is 120kJ / m 3 The above magnetic properties.
6. The iron-based rare earth boron-based isotropic magnet alloy according to any one of claims 1 to 3, wherein: The RE contains at least Nd and Pr.
7. An iron-based rare earth boron-based isotropic magnet alloy having the following alloy composition: having a composition formula T 100-x-y-z (B 1-n C n ) x RE y M z It indicates that, T is at least one element selected from Fe, Co and Ni and is a transition metal element that must contain Fe, RE is at least one rare earth element that must contain Nd among Nd and Pr, M is one or more elements selected from Al, Si, V, Cr, Ti, Mn, Cu, Zn, Ga, Zr, Nb, Mo, Ag, Hf, Ta, W, Pt, Au and Pb, and The composition ratios x, y and z satisfy 4.2 atomic % ≤ x ≤ 5.6 atomic %, 11.5 atomic % ≤ y ≤ 13.0 atomic %, 0.0 atomic % ≤ z ≤ 5.0 atomic % and 0.0 ≤ n ≤ 0.5 respectively; And has the following metal structure: B contains a concentration lower than RE2Fe 14 The stoichiometric composition of the B-type tetragonal compound is RE2Fe with an average crystal particle size of 10 nm or more and less than 70 nm. 14 The B-type tetragonal compound is the main phase, and there is a grain boundary phase with a width of 1 nm or more and less than 10 nm surrounding the main phase. 14 The single magnetic domain critical diameter of B-type tetragonal compounds is very small.
Citation Information
Patent Citations
Permanent magnet material, permanent magnet and manufacture of permanent magnet
JP1996162312A
Permanent magnet having plural ferromagnetic phases, and its manufacturing method
JP2002175908A
Nanocomposite magnet and its manufacturing method
JP2003178908A
Cited By
Corrosion-resistant magnetic temperature compensation alloy and preparation method thereof
CN120485661A
A corrosion-resistant magnetic temperature compensation alloy and its preparation method
CN120485661B