Large-specification high-performance prestressed wire rod steel and production process thereof
By optimizing chemical composition and process flow, combined with 'Cr+V' microcombination and controlled rolling and cooling technology, the balance problem of large-scale prestressed coil steel between high strength and pulling performance is solved, and high strength is achieved Combined with good pulling performance and reduce production costs.
Patent Information
- Application Number
- CN202411365599.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-22
AI Technical Summary
The existing large-size prestressed coil steel is difficult to meet the requirements of its pulling performance while ensuring high strength, and the production cost is relatively high.
The mass percentage of chemical components is C: 0.80% to 0.84%, Si: 0.15% to 0.35%, Mn: 0.70% to 0.85%, P: ≤0.020%, S: ≤0.020%, Cr: 0.20% to 0.35%, V: 0.015%~0.030%, N≤0.0070% high-performance prestressed coil steel, through KR molten pretreatment, converter, LF refining furnace, continuous casting, rolling and insulation channel slow cooling production process, combined with 'Cr +V' microcombination and controlled rolling and cooling process to optimize steel composition and process flow.
The combination of high strength and good drawing performance is achieved, the soxanitization rate reaches more than 90%, reducing the generation of mesh cementite and reducing production costs.
Smart Images

Figure CN118996259A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of steel preparation, and in particular to a large-size high-performance prestressed wire rod steel and a production process thereof. Background Art
[0002] High performance, ultra-high strength, high area reduction, stable mechanical properties, excellent drawing performance, and delayed fracture resistance are the development direction of wire rods for prestressed steel wire and strand. High-performance wire rods for prestressed steel wire and strand are mainly used to produce low-relaxation prestressed plain round steel wire, 1570MPa-level low-relaxation prestressed spiral rib steel wire for high-speed rail track plates, and 1×19 structure 1860MPa-level prestressed steel strands. Large-size 14mm and 15mm prestressed steel wire rods are mainly used for high-speed rail track plates and 1570MPa-level high-strength prestressed steel wires.
[0003] Patent CN202310256782.4 discloses a large-size prestressed wire rod and its production process for producing prestressed steel wire above 1860MPa, which belongs to the field of steel production technology. The key points of its technical solution are that the chemical composition of the prestressed wire rod is calculated by weight percentage: C: 0.90-0.95%, Si: 0.60-0.70%, Mn: 0.40-0.50%, Cr: 0.20-0.25%, V: 0.020-0.040%, Al: 0.025-0.040%, Ti: 0.025 -0.040%, P≤0.010%, S≤0.0050%, N≤40ppm, TO: 10-30ppm, H≤1ppm, the rest are Fe and inevitable residual elements; (Cr+Mn+V*10)≤0.9, (Al+Ti) / N≥1.5, to achieve the effect of producing a cable wire rod with high strength, toughness and plasticity, simple composition, simplified process, green and low carbon, and high production efficiency by optimizing the design of the composition of prestressed wire rod without building new salt bath / lead bath equipment and using the existing rolling and air cooling equipment of the steel plant. This invention is "Cr+V+Al+Ti" microalloying, and its production cost is high. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a large-size high-performance prestressed wire rod steel and a production process thereof, which ensures the high strength of the wire rod while meeting its drawing performance.
[0005] To achieve the above object, the present invention adopts the following technical solutions:
[0006] A large-size high-performance prestressed wire rod steel, the chemical composition mass percentage of which is: C: 0.80%-0.84%, Si: 0.15%-0.35%, Mn: 0.70%-0.85%, P: ≤0.020%, S: ≤0.020%, Cr: 0.20%-0.35%, V: 0.015%-0.030%, N≤0.0070%, O≤0.0040%.
[0007] A large-size high-performance prestressed wire rod steel, performance indicators: tensile strength 1207 ~ 1238MPa, elongation after fracture 10.5% ~ 12.5%, cross-sectional shrinkage 23% ~ 25%, non-metallic inclusions A + C ≤ 1.5, B + D ≤ 1.5, wire rod diameter ≥ 14mm, troostitization rate reaches more than 90%.
[0008] Functions of chemical elements:
[0009] C: Carbon can increase the strength and hardness of steel, but as the carbon content increases, the plasticity and toughness of steel decrease. The C content is controlled at 0.80% to 0.84%.
[0010] Si: Silicon can also increase the strength and hardness of steel, reduce the plasticity and toughness of steel, and has a deoxidizing effect in the steelmaking process. The Si content is controlled at 0.15% to 0.35%.
[0011] Mn: Manganese can improve the strength of steel, and can combine with sulfur to form manganese sulfide to eliminate the "hot brittleness" of steel, and can improve the hardenability and wear resistance of steel. The Mn content is controlled at 0.70% to 0.85%.
[0012] P / S: Phosphorus and sulfur are harmful elements in steel. Phosphorus dissolves in ferrite. Although it can improve the strength and hardness of steel, its biggest harm is serious segregation, increased temper brittleness, and significantly reduced plasticity and toughness of steel, making steel easy to crack during cold processing, which is the so-called "cold brittleness" phenomenon; sulfur reduces the plasticity of steel, increases the brittleness of steel, and deteriorates the quality of steel. P≤0.020%, S≤0.020%.
[0013] Cr: Chromium is a carbide-forming element. When properly matched with carbon and manganese, it can improve the hardenability of steel, strengthen the matrix, refine the grains, improve the strength, hardness, hardenability and wear resistance of steel, and improve the corrosion resistance and oxidation resistance of steel. The addition of a small amount of chromium can increase the solubility of vanadium in austenite and enhance the solid solution strengthening effect of vanadium. Cr: 0.20-0.35%.
[0014] V: Vanadium is an excellent deoxidizer for steel. It can refine the grain size and improve the strength and toughness. The nitride formed by vanadium and nitrogen has a solid solution strengthening effect. V: 0.015% to 0.030%.
[0015] N: forms nitride with V to increase strength. N≤0.0070%.
[0016] A large-size high-performance prestressed wire rod production process, the steps are: KR molten iron pretreatment, converter, LF refining furnace, continuous casting, rolling, insulation channel slow cooling, the specific steps include:
[0017] 1) KR hot metal pretreatment: spray desulfurizer into the hot metal ladle for desulfurization. After treatment, the S content of hot metal is required to be ≤0.030%;
[0018] 2) Converter process:
[0019] Converter smelting: scrap steel accounts for 10% to 12%, molten iron accounts for 88% to 90%, and the use of desulfurized slag steel and nickel-copper scrap steel is prohibited; smelting is carried out in a top-bottom combined blowing converter, the tapping temperature is 1600 to 1650°C, the tapping end point [C] is 0.05 to 0.08%, and P ≤ 0.012%;
[0020] Ladle alloying: The alloying sequence is ferrosilicon, silicon manganese, high carbon ferrochrome, ferrovanadium, low nitrogen carburizer, no deoxidizer, argon blowing time ≥ 5min,
[0021] Static argon blowing: argon blowing time ≥ 3min, temperature after treatment 1500℃~1520℃;
[0022] 3) LF furnace refining: maintain a slight positive pressure of 40-70 kPa in the furnace, use submerged arc heating, add 6.5-8.0 kg / t of active lime, 1-2.5 kg / t of fluorite to make white slag refining, and add 1.0-1.2 kg / t of manganese silicon, 1.25-1.82 kg / t of ferrosilicon, fine-tune the alloy, blow argon time ≥15 min, and the LF furnace leaving the station temperature is 1520℃~1535℃;
[0023] 4) Continuous casting: adopt the whole process protection casting process, use high carbon steel protection slag for crystallizer protection slag, the platform ladle temperature is 1535℃~1545℃, the middle ladle temperature is 1490℃~1512℃, the superheat is maintained at 20℃~30℃, the pulling speed is 2.0~2.2m / min, the pulling speed is constant, and the billet is slowly cooled in the insulation pit for more than 72h after it comes off the line.
[0024] 5) Rolling process:
[0025] Heating: Heating by walking beam furnace, preheating section 860℃~900℃, heating section 1100℃~1140℃, soaking section 1130℃~1170℃, heating time 1.5~2.5h;
[0026] Rolling: Rough rolling temperature: 1000℃~1040℃; Finishing rolling inlet temperature: 900℃~940℃; Wire laying temperature: 840℃~880℃, Air-cooled roller speed: Head roller speed 0.65~0.75m / s; Roller speed increase 2~5%. Insulation cover fully open; Fan cooling: 1~5 fans, each fan has a wind volume of 224000~225000m 3 / h, 6 to 11 fans, each with a wind volume of 147500 to 148000m 3 / h;
[0027] 6) Insulation and slow cooling: After rolling, the wire rod passes through an insulation channel for slow cooling.
[0028] In step 1), the desulfurizing agent comprises: 90% to 95% lime powder and 5% to 10% fluorite powder.
[0029] In step 2), the target amount of alloy added is: 10-10.5 kg / t steel of silicon manganese, 1.0-1.2 kg / t steel of ferrosilicon, 3.5-3.7 kg / t steel of high carbon ferrochrome, 0.40-0.45 kg / t steel of ferrovanadium, and 850-880 kg / t steel of low nitrogen recarburizer.
[0030] In step 4), before casting begins, the tundish is cleaned with argon, the purge time is ≥ 2 min, the electromagnetic stirring current of the crystallizer is 320 A, the frequency is 3 Hz, and it rotates continuously, and the terminal electromagnetic stirring current is 400 A, and the frequency is 8 Hz.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] The present invention adopts the production process of "KR molten iron pretreatment + converter + LF refining furnace + continuous casting + controlled rolling and controlled cooling + slow cooling in an insulation channel". Through the "Cr+V" micro-combination and controlled rolling and controlled cooling process, the high strength of the wire rod is met, the sorbitization rate reaches more than 90%, the generation of network cementite is reduced, and good drawing performance is achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is the metallographic organization diagram of the present invention.
[0034] Figure 2 This is the metallographic diagram of the decarburized layer. DETAILED DESCRIPTION
[0035] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0036] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and the like are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, features defined as "first", "second", and the like may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means more than two.
[0037] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.
[0038] A large-size high-performance prestressed wire rod steel, the chemical composition mass percentage is: C: 0.80% ~ 0.84%, Si: 0.15% ~ 0.35%, Mn: 0.70% ~ 0.85%, P: ≤ 0.020%, S: ≤ 0.020%, Cr: 0.20% ~ 0.35%, V: 0.015% ~ 0.030%, N ≤ 0.0070%, O ≤ 0.0040%. Performance indicators: tensile strength 1207 ~ 1238MPa, elongation after fracture 10.5 ~ 12.5%, cross-sectional shrinkage 23 ~ 25%, non-metallic inclusions A + C ≤ 1.5, B + D ≤ 1.5, wire rod diameter ≥ 14mm, troostitization rate reaches more than 90%.
[0039] A large-size high-performance prestressed wire rod production process, the process steps are: KR molten iron pretreatment, converter, LF refining furnace, continuous casting, rolling, insulation channel slow cooling, including:
[0040] 1) KR molten iron pretreatment: spray desulfurizer into the molten iron ladle for desulfurization. The desulfurizer composition is 90% to 95% lime powder and 5% to 10% fluorite powder. After treatment, the molten iron S is required to be ≤ 0.030%.
[0041] 2) Converter process
[0042] Converter smelting: scrap steel accounts for about 10-12%, molten iron accounts for about 88%-90%, 5 tons of slag steel is used, and desulfurized slag steel and nickel-copper scrap steel are prohibited; top and bottom double-blowing converter is used for smelting, the tapping temperature is 1600-1650℃, the tapping end point [C] is 0.05%-0.08%, P≤0.012%, and slag is strictly prohibited: avoid spot blowing. Ensure that the end point carbon content and temperature are hit once, and if secondary spot blowing occurs, the cover must be lowered first;
[0043] Ladle alloying: The alloying sequence is ferrosilicon, silicomanganese, high carbon ferrochrome, ferrovanadium, and low nitrogen carburizer. No deoxidizer is added. The argon blowing time is ≥5 minutes. The target amount of alloy added per ton of steel is: 10-10.5kg / t of silicomanganese, 1.0-1.2kg / t of ferrosilicon, 3.5-3.7kg / t of high carbon ferrochrome, 0.40-0.45kg / t of ferrovanadium, and 850-880kg / t of low nitrogen carburizer.
[0044] Static argon blowing: argon blowing time ≥ 3min, medium blowing for 2min first, then weak blowing; the temperature after treatment is 1500℃~1520℃;
[0045] 3) LF furnace refining: The furnace is kept at a slight positive pressure of 40-70 kPa, and submerged arc heating is adopted, the arc light does not leak out, and active lime 6.5-8.0 kg / t steel, fluorite 1-2.5 kg / t steel are added to make white slag refining, and manganese silicon 1.0-1.2 kg / t steel, ferrosilicon 1.25-1.82 kg / t steel are added, the alloy is fine-tuned, the soft blowing time is ≥15 min, and the LF furnace leaving the station temperature is 1520℃~1535℃;
[0046] 4) Continuous casting: adopt the whole process protection casting process and clean the tundish with argon before casting, and the purge time is ≥2min. The crystallizer electromagnetic stirring current is 320A, frequency is 3Hz, continuous rotation, the end electromagnetic stirring current is 400A, frequency is 8Hz, positive and negative rotation, the crystallizer protective slag uses high carbon steel protective slag, the platform ladle temperature is 1535℃~1545℃, the tundish temperature is 1490℃~1512℃, the superheat is maintained at 20℃~30℃, the pulling speed is 2.0~2.2m / min, the pulling speed is constant, the liquid level fluctuation is reduced, and the billet is slowly cooled in the insulation pit for more than 72h after it comes off the line;
[0047] 5) Rolling process:
[0048] Heating: Heating by walking beam furnace, preheating section 860℃~900℃, heating section 1100℃~1140℃, soaking section 1130℃~1170℃, heating time 1.5~2.5h;
[0049] Rolling: Rough rolling temperature: 1000℃~1040℃; Finishing rolling inlet temperature: 900℃~940℃; Wire laying temperature: 840℃~880℃, Air-cooled roller speed: Head roller speed 0.0.65~0.75m / s; Roller speed increase 2~5%. Insulation cover fully open; Fan cooling: High air volume cooling, 1~5 fans, each fan has an air volume of 224000~225000m 3 / h, 6 to 11 fans, each with a wind volume of 147500 to 148000m 3 / h;
[0050] 6) Insulation and slow cooling: After rolling, the wire rod passes through the insulation channel for slow cooling, which ensures the effective release of organizational stress and internal stress, thereby ensuring the performance of the product and the requirements of the performance difference of the wire rod.
[0051] Example The chemical composition of SWRH82B-G-YL hot-rolled wire rod is shown in Table 1;
[0052] Table 1: Chemical composition %
[0053] C Si Mn P S Cr V O N Example 1 0.81 0.28 0.77 0.009 0.008 0.32 0.016 0.0031 0.0029 Example 2 0.82 0.25 0.78 0.012 0.014 0.32 0.017 0.0035 0.0025 Example 3 0.84 0.18 0.80 0.010 0.012 0.25 0.020 0.0028 0.0030 Example 4 0.83 0.26 0.82 0.008 0.010 0.28 0.025 0.0031 0.0035 Example 5 0.80 0.30 0.75 0.015 0.016 0.30 0.030 0.0030 0.0040
[0054] Production process of the embodiment: blast furnace hot metal → KR hot metal pretreatment (desulfurization, slag removal) → 100t converter (top and bottom combined blowing) → ladle bottom blowing argon → LF furnace refining → 150*150mm eight-strand billet continuous casting (electromagnetic stirring of the crystallizer and electromagnetic stirring at the end of solidification) → billet slow cooling → walking beam heating furnace heating → wire rod rolling → wire laying → inspection → coiling → slow cooling in the insulation channel → sampling, inspection, judgment → packaging, and delivery to the warehouse. Among them:
[0055] Rolling process: Rough rolling temperature: 1020℃~1040℃; Finishing rolling inlet temperature: 930℃~940℃; Wire laying temperature: 840℃~860℃, Air-cooled roller speed: Head roller 0.65~0.75m / s; Roller speed increase 2~5%. Insulation cover fully open; Fan high air volume cooling: 1~5 fans, each fan has an air volume of 224000m 3 / h, single duct, motor power 315kW (variable frequency); 6 to 11 fans, each with an air volume of 147,900m 3 / h, single duct, motor power 160kW (non-variable frequency).
[0056] The results of the macroscopic defect inspection of the ingot after continuous casting during the production process are shown in Table 2;
[0057] Table 2: Results of macroscopic defects inspection of ingots:
[0058]
[0059] The performance indicators of produced wire rod are shown in Table 3;
[0060] Table 3: Wire rod performance indicators
[0061] Tensile strength / MPa Elongation after break / % Sectional shrinkage / % Example 1 1216 12.2 23 Example 2 1232 12.5 23 Example 3 1238 12 25 Example 4 1217 10.5 24 Example 5 1221 12.5 23
[0062] The microstructure and non-metallic inclusions of the produced wire rod are shown in Table 4;
[0063] Table 4: Microstructure and non-metallic inclusions:
[0064]
[0065]
[0066] By metallographic organization Figure 1 It can be seen that it is composed of S+P+C, and the troostitization rate reaches more than 90%. Figure 2 The visible decarburization layer is 0.05 to 0.08 mm.
[0067] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and basic spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A large-size high-performance prestressed wire rod steel, characterized in that: The chemical composition mass percentage is: C: 0.80%~0.84%, Si: 0.15%~0.35%, Mn: 0.70%~0.85%, P: ≤0.020%, S: ≤0.020%, Cr: 0.20%~0.35%, V: 0.015%~0.030%, N≤0.0070%, O≤0.0040%.
2. The large-size high-performance prestressed wire rod steel according to claim 1, characterized in that: Performance indicators: tensile strength 1207~1238MPa, elongation after fracture 10.5%~12.5%, cross-sectional shrinkage 23%~25%, non-metallic inclusions A+C≤1.5, B+D≤1.5, wire rod diameter ≥14mm, and troostitization rate of more than 90%.
3. The large-size high-performance prestressed wire rod production process according to claim 1 is characterized in that: The steps are: KR molten iron pretreatment, converter, LF refining furnace, continuous casting, rolling, and slow cooling in the insulation channel. The specific steps include: 1) KR hot metal pretreatment: spray desulfurizer into the hot metal ladle for desulfurization. After treatment, the S content of hot metal is required to be ≤0.030%; 2) Converter process: Converter smelting: scrap steel accounts for 10% to 12%, molten iron accounts for 88% to 90%, top and bottom double-blown converter is used for smelting, tapping temperature is 1600℃ to 1650℃, tapping end point [C] is 0.05% to 0.08%, P ≤ 0.012%; Ladle alloying: The alloying sequence is ferrosilicon, silicon manganese, high carbon ferrochrome, ferrovanadium, low nitrogen carburizer, no deoxidizer, argon blowing time ≥ 5min, Static argon blowing: argon blowing time ≥ 3min, temperature after treatment 1500℃~1520℃; 3) LF furnace refining: maintain a slight positive pressure of 40-70 kPa in the furnace, use submerged arc heating, add 6.5-8.0 kg / t of active lime, 1-2.5 kg / t of fluorite to make white slag refining, and add 1.0-1.2 kg / t of manganese silicon, 1.25-1.82 kg / t of ferrosilicon, fine-tune the alloy, blow argon time ≥15 min, and the LF furnace leaving the station temperature is 1520℃~1535℃; 4) Continuous casting: adopt the whole process protection casting process, use high carbon steel protection slag for crystallizer protection slag, the platform ladle temperature is 1535℃~1545℃, the middle ladle temperature is 1490℃~1512℃, the superheat is maintained at 20℃~30℃, the pulling speed is 2.0~2.2m / min, the pulling speed is constant, and the billet is slowly cooled in the insulation pit for more than 72h after it comes off the line. 5) Rolling process: Heating: Heating by walking beam furnace, preheating section 860℃~900℃, heating section 1100℃~1140℃, soaking section 1130℃~1170℃, heating time 1.5~2.5h; Rolling: Rough rolling temperature: 1000℃~1040℃; Finishing rolling inlet temperature: 900℃~940℃; Wire laying temperature: 840℃~880℃, Air-cooled roller speed: Head roller speed 0.65~0.75m / s; Roller speed increase 2%~5%. Insulation cover fully open; Fan cooling: 1~5 fans, each fan has a wind volume of 224000~225000m 3 / h, 6 to 11 fans, each with a wind volume of 147500 to 148000m 3 / h; 6) Slow cooling in the insulation channel: After rolling, the wire rod passes through the insulation channel for slow cooling.
4. The large-size high-performance prestressed wire rod production process according to claim 3 is characterized in that: In step 1), the desulfurizing agent comprises: 90% to 95% lime powder and 5% to 10% fluorite powder.
5. The production process of large-size high-performance prestressed wire rod steel according to claim 3 is characterized in that: In step 2), the target amount of alloy added is: 10-10.5 kg / t steel of silicon manganese, 1.0-1.2 kg / t steel of ferrosilicon, 3.5-3.7 kg / t steel of high carbon ferrochrome, 0.40-0.45 kg / t steel of ferrovanadium, and 850-880 kg / t steel of low nitrogen recarburizer.
6. The large-size high-performance prestressed wire rod production process according to claim 3 is characterized in that: In step 4), before casting begins, the tundish is cleaned with argon, the purge time is ≥ 2 min, the electromagnetic stirring current of the crystallizer is 320 A, the frequency is 3 Hz, and it rotates continuously, and the terminal electromagnetic stirring current is 400 A, and the frequency is 8 Hz.
Citation Information
Cited By
High-strength plastic tire cord steel and preparation method thereof
CN122147007A