Ultrahigh-strength steel and preparation method thereof
By controlling the content of rare earth RE and other elements in ultra-high strength steel and forming a specific composite structure, the problem of insufficient toughness of existing ultra-high strength steel is solved, and its application performance in high-end equipment is significantly improved.
Patent Information
- Application Number
- CN202411107010.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-13
AI Technical Summary
The existing ultra-high strength steel has low toughness, which limits its application in key components of high-end equipment, especially under strong fatigue or impact load conditions.
By controlling the content of rare earth RE in ultra-high strength steel and combining the content of solid solution oxygen, all sulfur and all nitrogen, specific chemical components and composite structures are formed, including rare earth sulfides, oxides and titanium nitrides and other inclusions. to form multi-stage complex structure to improve toughness.
The toughness of ultra-high strength steel is significantly improved, and the impact power is increased to 20~25J or above, far exceeding 2~3 times that of steel of the same strength grade. The heat treatment process is easy to operate and is less affected by the steel size effect.
Smart Images

Figure CN118996267A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of ultra-high strength steel, and in particular relates to an ultra-high strength steel and a preparation method thereof. Background Art
[0002] Ultra-high strength steel is the core material of key load-bearing components of high-end equipment, and its performance level is related to the safety of equipment service. Taking advanced aircraft landing gear and wind tunnel force measurement devices as examples, the increasingly severe fatigue or impact load conditions inside them have put forward higher requirements on the strength and toughness of ultra-high strength steel. Although the current commercial 18Ni series maraging steel has reached an ultra-high strength level of 2.0~2.4GPa, its toughness is insufficient (A KV <10J) limits its application in the above working conditions, making key components "unavailable". Therefore, it is urgent to develop steel with ultra-high strength and high toughness to solve the dilemma of material selection that restricts key components of high-end equipment.
[0003] At present, grain refinement and the introduction of austenite are the main ways to improve the toughness of ultra-high-strength steel. These approaches often rely on sufficient deformation and phase change regulation. During the preparation process, as the size of ultra-high-strength steel components (key load-bearing components for high-end equipment) increases, insufficient deformation or incomplete phase change is likely to occur, resulting in lower toughness of ultra-high-strength steel.
[0004] In view of this, it is necessary to provide an ultra-high strength steel and a preparation method thereof to solve the problem of low toughness of existing ultra-high strength steel. Summary of the invention
[0005] Therefore, the present invention provides an ultra-high strength steel and a preparation method thereof, which can solve the technical problem of low toughness of existing ultra-high strength steel.
[0006] In order to solve the above problems, the present invention provides an ultra-high strength steel, wherein the content of rare earth RE in the ultra-high strength steel satisfies the following formula:
[0007] -80<{[RE]-(a·T[O] s +b·T[S] m )} / (c·T[N] m )<200;
[0008] Wherein, [RE] is the content of rare earth RE in ultra-high strength steel;
[0009] T[O] s is the dissolved oxygen content in ultra-high strength steel;
[0010] T[S] m is the total sulfur content in ultra-high strength steel;
[0011] T[N]m is the total nitrogen content in ultra-high strength steel;
[0012] [RE], T[O] s , T[S] m , T[N] m All are measured in mass percentage;
[0013] a, b, and c are correction coefficient one, correction coefficient two, and correction coefficient three, respectively, and their values are 2 to 5, 1.5 to 2.5, and 0.5 to 1.5.
[0014] Further, the chemical composition of the ultra-high strength steel includes, by weight percentage: C≤0.01wt%, Ni: 17.0-18.5wt%, Co: 11.0-12.5wt%, Mo: 4.5-5.5wt%, Ti: 0.9-1.1wt%, S≤0.005wt%, P≤0.01wt%, O≤0.002wt%, N≤0.0015wt%, rare earth RE: 0.001-0.03wt%, and the balance is Fe;
[0015] Preferably, the rare earth RE is one of lanthanum La, cerium Ce and yttrium Y.
[0016] Furthermore, in the ultra-high strength steel: the mass percentage of O is ≤0.001wt%, the mass percentage of N is <0.001wt%, and the mass percentage of rare earth RE is 0.004-0.018wt%;
[0017] Preferably, the mass percentage of rare earth RE is 0.0040-0.014wt%.
[0018] Furthermore, more than 50% of the total number of inclusions in the ultra-high strength steel is of average equivalent diameter D m The inclusions are spherical, nearly spherical or granular and dispersedly distributed with a size of 1 to 5 μm; the dispersedly distributed inclusions include rare earth sulfide RE2S3, rare earth oxide RE2O3, titanium nitride TiN, and rare earth oxysulfur-titanium nitride.
[0019] Furthermore, the ultra-high strength steel has a complex phase structure and original austenite grains with a grain size greater than or equal to 8, the complex phase structure includes martensite, nano-precipitated phase and reversed austenite; the martensite includes martensite lath bundles;
[0020] The nano-precipitated phase includes a Ni3Ti phase and a molybdenum-rich phase, and the equivalent diameter of the nano-precipitated phase is 5 to 50 nm;
[0021] In the multiphase structure, the volume percentage of the reversed austenite is 5 to 20 vol.%;
[0022] Preferably, the volume percentage of the reversed austenite is 10-15 vol.%.
[0023] Preferably, the average size of the martensitic lath bundles is less than or equal to 5 μm.
[0024] Furthermore, the properties of the ultra-high strength steel are as follows: yield strength ≥2.1 GPa, tensile strength ≥2.2 GPa, elongation after fracture ≥9%, cross-sectional shrinkage ≥50%, and V-notch impact energy ≥20-25 J.
[0025] In another aspect, the present invention provides a method for preparing the ultra-high strength steel as described in any one of the above, comprising the following steps:
[0026] Smelting: preparing materials according to the chemical composition of the ultra-high strength steel, performing smelting treatment, and obtaining steel ingots after casting;
[0027] Annealing: annealing the steel ingot; the annealing time t h >(1.5D I ) / 100h, where D I is the cross-sectional size of the steel ingot obtained after casting, in mm;
[0028] Forging: Forging the annealed steel ingot to obtain forged material;
[0029] Solution heat treatment: The forging material is subjected to solution heat treatment; the time of the solution treatment is t s >(1.5~2.5)D b / 100h, where D b It is the cross-sectional dimension of the forging material obtained after forging, in mm;
[0030] Aging treatment: The forged material after the solution heat treatment is subjected to aging treatment to obtain the ultra-high strength steel.
[0031] Furthermore, the drawing ratio Y in the forging process is ≥10, where Y=(D I / D b ) 2 .
[0032] Further, vacuum induction refining (VIM) or vacuum induction refining (VIM) + vacuum arc remelting (VAR) is used for smelting;
[0033] Preferably, rare earth RE is added during VIM refining; the refining time t1 before adding rare earth RE is ≥ 60 min, and the refining time t2 after adding rare earth RE is ≥ 30 min;
[0034] Preferably, the vacuum degree P during VIM refining is v≤1~5Pa;
[0035] Preferably, the steel tapping time after the smelting process is completed is t3≤30min.
[0036] Furthermore, the annealing temperature is 1000-1100° C.; and / or
[0037] The forging temperature is 800-1200° C.; and / or
[0038] The temperature of the solution heat treatment is 800-900°C; and / or
[0039] The temperature of the aging treatment is 460-540° C.; the time of the aging treatment is 1-16 hours.
[0040] Based on the above method, "rare earth modified inclusions" are combined with "constructing a multi-level complex phase structure" to obtain an ultra-high purity multi-level complex phase structure. Without damaging precipitation strengthening, the V-notch impact toughness of 2.2GPa ultra-high strength steel is increased to 20-25J and above through multiple toughening mechanisms such as alleviating stress concentration, inhibiting crack nucleation and hindering crack propagation. This is 2-3 times the impact toughness of existing steels of the same strength grade. In addition, the heat treatment process is easy to operate and is less affected by the "size effect" of the steel.
[0041] The ultra-high strength steel and the preparation method thereof provided by the present invention have the following beneficial effects:
[0042] 1. The present invention limits the content of rare earth RE by the content of O, S and N in ultra-high strength steel, promotes the nucleation of inclusions TiN in the steel and inhibits their aggregation and growth, and at the same time, part of TiN forms a complex with RE-OS to jointly improve the morphology and distribution of inclusions in the steel, that is, the quadrilateral TiN inclusions in the steel are transformed into finer spherical or nearly spherical or granular rare earth sulfides, rare earth oxides and titanium nitrides or rare earth oxygen sulfur-titanium nitride complexes that are dispersed, thereby alleviating stress concentration during deformation and further improving the matrix toughness of the ultra-high strength steel.
[0043] 2. Further, the chemical composition of the ultra-high strength steel of the present invention includes: C≤0.01wt%, Ni: 17.0-18.5wt%, Co: 11.0-12.5wt%, Mo: 4.5-5.5wt%, Ti: 0.9-1.1wt%, S≤0.005wt%, P≤0.01wt%, O≤0.002wt%, N≤0.0015wt%, rare earth RE: 0.001-0.03wt%, and the balance is Fe; according to the above chemical composition, a phase transformation is performed to obtain The multi-level complex phase structure of "martensite + nano-precipitation phase + austenite" can effectively inhibit crack nucleation and hinder crack propagation, further improving the toughness and plasticity of ultra-high strength steel; specifically, after aging treatment, the matrix will precipitate nano-scale precipitation phases, such as Ni3Ti or Mo-rich phase; at the same time, due to the addition of rare earths, the size of the martensite lath bundles can be refined, and the Mo, Ni and Ti elements in the steel matrix can be segregated (i.e., chemical heterogeneity is formed), thereby promoting the formation of reversed austenite. More reversed austenite is beneficial to the plasticity and toughness of ultra-high strength steel.
[0044] 3. Furthermore, by controlling the target cross-sectional size of the material before and after forging, a larger drawing ratio is obtained, and a larger deformation amount is achieved, so that the coarse grains can be fully broken, and the deformation energy storage is used to promote recrystallization, thereby improving the grain grade and obtaining a structure with a prior austenite grain size greater than or equal to level 8. The refined prior austenite grains are a sufficient condition for obtaining finer martensite subgrains, and the martensite lath bundle, as one of the key subgrain components, is the smallest toughening unit for controlling ultra-high strength steel. The fine martensite lath bundle achieves toughening by hindering crack propagation and increasing its path. Therefore, limiting the prior austenite grain grade and obtaining a smaller martensite lath bundle can further improve the toughness of ultra-high strength steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. The drawings described below are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.
[0046] Figure 1 : is the morphology of the original austenite grains of the ultra-high strength steel in the embodiments of the present invention and the comparative examples:
[0047] Figure 2 is the inverse pole figure of the aged martensite of the ultra-high strength steel in the embodiment of the present invention and the comparative example;
[0048] Figure 3 is a typical aged multi-stage complex structure diagram of ultra-high strength steel in an embodiment of the present invention;
[0049] Figure 4 is the SEM morphology and composition distribution of RE-OS-TiN in Example 3;
[0050] Figure 5 is a scanning electron microscope morphology and composition distribution of inclusions in the ultra-high strength steel in comparative example 1;
[0051] Figure 6 These are the metallographic and scanning electron microscope images of the undissolved single RE particles in Comparative Example 3. DETAILED DESCRIPTION
[0052] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. The drawings described below are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.
[0053] In order to meet the performance requirements of ultra-high strength steel for large-size components of high-end equipment under strong fatigue or impact load conditions, the purpose of the present invention is to provide an ultra-high strength steel and a preparation method thereof. The specific scheme is as follows:
[0054] An ultra-high strength steel, wherein the content of rare earth RE in the ultra-high strength steel satisfies the following formula:
[0055] -80<{[RE]-(a·T[O] s +b·T[S] m )} / (c·T[N] m )<200;
[0056] Wherein, [RE] is the content of rare earth RE in ultra-high strength steel;
[0057] T[O] s is the dissolved oxygen content in ultra-high strength steel;
[0058] T[S] m is the total sulfur content in ultra-high strength steel;
[0059] T[N] m is the total nitrogen content in ultra-high strength steel;
[0060] [RE], T[O] s , T[S] m , T[N] m All are measured in mass percentage;
[0061] a, b, and c are correction coefficient one, correction coefficient two, and correction coefficient three, respectively, and their values are 2 to 5, 1.5 to 2.5, and 0.5 to 1.5.
[0062] Rare earth RE and O mainly form RE2O3 and RE-OS-TiN, rare earth RE and S mainly form RE2S3 and RE-OS-TiN, and rare earth RE and N mainly form RE-OS-TiN; therefore, the contents of the four elements are limited, taking into full consideration the consumption of rare earth RE by the chemical reaction between RE and O and S in steel, as well as the necessary content of RE required for the participation of TiN modification effect.
[0063] In some embodiments, the chemical composition of the ultra-high strength steel includes, by weight percentage: C≤0.01wt%, Ni: 17.0-18.5wt%, Co: 11.0-12.5wt%, Mo: 4.5-5.5wt%, Ti: 0.9-1.1wt%, S≤0.005wt%, P≤0.01wt%, O≤0.002wt%, N≤0.0015wt%, rare earth RE: 0.001-0.03wt%, and the balance is Fe;
[0064] Preferably, the rare earth RE is one of lanthanum La, cerium Ce and yttrium Y.
[0065] In some embodiments, in the ultra-high strength steel: the mass percentage of O is ≤0.001wt%, the mass percentage of N is <0.001wt%, and the mass percentage of rare earth RE is 0.004-0.018wt%;
[0066] Preferably, the mass percentage of rare earth RE is 0.004-0.014wt%.
[0067] In some embodiments, more than 50% of the total number of inclusions in the ultra-high strength steel have an average equivalent diameter D m The steel comprises spherical, nearly spherical or granular inclusions with a size of 1 to 5 μm and dispersedly distributed; the dispersedly distributed inclusions include rare earth sulfide RE2S3, rare earth oxide RE2O3, titanium nitride TiN, and rare earth oxysulfur-titanium nitride; preferably, more than 75% of the total number of inclusions in the steel are the above-mentioned dispersedly distributed inclusions; more preferably, more than 95% of the total number of inclusions in the steel are the above-mentioned dispersedly distributed inclusions.
[0068] In some embodiments, the ultra-high strength steel has a complex phase structure and original austenite grains with a grain size greater than or equal to 8, the complex phase structure includes martensite, nano-precipitated phase and reversed austenite; the martensite includes martensite lath bundles;
[0069] The nano-precipitated phase comprises a Ni3Ti phase and a molybdenum-rich phase, the equivalent diameter of the nano-precipitated phase is 5-50nm, and the nano-precipitated phase is dispersed in the ultra-high strength steel matrix.
[0070] In the complex phase structure, the volume percentage of reversed austenite is 5-20 vol%;
[0071] Preferably, the volume percentage of reversed austenite is 5 to 15 vol%, and more preferably 10 to 15 vol%.
[0072] The original austenite grain size is greater than or equal to level 8; preferably, greater than or equal to level 9; more preferably, greater than or equal to level 10;
[0073] The average size of the martensite lath bundle is less than or equal to 5 μm; preferably, less than or equal to 2.5 μm; more preferably, less than or equal to 1.5 μm. The martensite lath bundle is a type of martensite subgrain between the martensite lath block and the martensite lath, which is a region surrounded by high-angle grain boundaries of 55 to 65 degrees.
[0074] Generally, for ultra-high strength steel, the full refinement of the martensite multi-level structure (original austenite grains, martensite lath blocks, martensite lath bundles and martensite laths, etc.) helps to improve toughness and plasticity; specifically, the refinement of the original austenite grains is a sufficient condition for obtaining finer martensite subgrains, and the martensite lath bundles are considered to be the smallest toughening unit controlling such ultra-high strength steels, which achieves toughening by hindering crack propagation and increasing its path. Therefore, considering the toughening effect that mainly controls the matrix multi-level structure, the size of the original austenite grains and martensite lath bundles is limited.
[0075] In some embodiments, the properties of the ultra-high strength steel are as follows: yield strength ≥ 2.1 GPa, tensile strength ≥ 2.2 GPa, elongation after fracture ≥ 9%, cross-sectional reduction ≥ 50%, and V-notch impact energy ≥ 20 J.
[0076] In another aspect, the present invention provides a method for preparing the ultra-high strength steel of any one of the above items, comprising the following steps:
[0077] Smelting: The materials are prepared according to the chemical composition of ultra-high strength steel, and then smelted and cast to obtain steel ingots. High-purity metal materials that have been fully degreased and dried are used in the smelting process.
[0078] Annealing: Annealing (homogenization) of the steel ingot; the holding time of annealing treatment is t h >(1.5D I ) / 100h, where D I is the cross-sectional size of the steel ingot obtained after casting, in mm;
[0079] Forging: Forging the annealed steel ingot to obtain forged material;
[0080] Solution heat treatment: Solution heat treatment of forgings; the time of solution treatment t s >(1.5~2.5)D b / 100h, where D b It is the cross-sectional dimension of the forging material obtained after forging, in mm;
[0081] Aging treatment: The forged material after solution heat treatment is subjected to aging treatment to obtain ultra-high strength steel.
[0082] In some embodiments, the drawing ratio Y in the forging process is ≥ 10, where Y = (D I / D b ) 2 The target cross-sectional dimensions of the material before and after forging (i.e. D I and D b ), on the one hand, determines the time of annealing and solution heat treatment, on the other hand, can obtain a larger drawing ratio and achieve a larger deformation, thereby ensuring that the coarse grains can be fully broken, and the deformation energy storage is used to promote recrystallization, thereby improving the grain grade and obtaining a structure with a prior austenite grain size greater than or equal to level 8.
[0083] The steel ingots smelted by VIM or VIM+VAR are generally cylindrical ingots, so the above cross-sectional dimensions are diameters.
[0084] In some embodiments, vacuum induction refining (VIM) or vacuum induction refining (VIM) + vacuum arc remelting (VAR) is used for smelting;
[0085] Preferably, rare earth RE is added during VIM refining; the refining time t1 before adding rare earth RE is ≥ 60 min, and the refining time t2 after adding rare earth RE is ≥ 30 min;
[0086] Preferably, the vacuum degree P during VIM refining is v ≤1~5Pa;
[0087] Preferably, the steel tapping time after the smelting process is completed is t3≤30min.
[0088] Generally speaking, for high Co-Ni maraging type ultra-high strength steel, after the VIM+VAR two-in-one special metallurgy process, the main type of inclusions in the steel is quadrilateral TiN, which has an adverse effect on the toughness and plasticity of the steel matrix; adding RE in the VIM process can promote the nucleation of TiN and inhibit its aggregation and growth. At the same time, part of TiN can form a complex with RE-OS to jointly improve the morphology and distribution of inclusions, thereby alleviating the stress concentration during deformation and ensuring the toughness and plasticity of the matrix.
[0089] On the other hand, after adding rare earth RE, martensite lath bundles with a small average grain size (less than or equal to 5μm) can be obtained after solution heat treatment, and the Mo, Ni and Ti elements in the steel matrix are segregated (i.e., chemical heterogeneity is formed), thereby promoting the formation of reversed austenite; thus, a multi-level complex phase structure of "martensite + nano-precipitation phase + austenite" is formed, which can effectively inhibit crack nucleation and hinder crack propagation, and further improve the toughness and plasticity of ultra-high strength steel.
[0090] Refining the molten steel for a long time before adding rare earth RE can fully purify the molten steel and reduce the oxygen content in the steel. Increasing the refining time after adding RE can promote the full fusion of RE with the molten steel and promote the modification effect of inclusions. The vacuum degree directly affects the RE oxidation rate and the removal rate of gas elements in the molten steel, and the steel tapping time also affects the amount of RE oxidized in the molten steel. Therefore, the above factors are considered to jointly determine the RE burnout amount and the final RE recovery rate during the smelting process.
[0091] In some embodiments, the annealing temperature is 1000-1100° C.; and / or
[0092] The forging temperature is 800-1200°C; and / or
[0093] The temperature of the solution heat treatment is 800-900°C; and / or
[0094] The temperature of the aging treatment is 460-540°C; the time of the aging treatment is 1-16 hours.
[0095] The present invention is further described below in conjunction with specific examples and comparative examples. The rare earth RE is high-purity metal lanthanum La (purity ≥ 99.5%).
[0096] Example 1
[0097] This embodiment provides a method for preparing ultra-high strength steel, comprising the following steps:
[0098] Smelting: VIM smelting was carried out according to the chemical composition of Table 1, and a steel ingot with a diameter of 300 mm was obtained after casting; high-purity metal materials that had been fully degreased and dried were used in the smelting process; the refining time before adding rare earth lanthanum La was 70 min, and the refining time after adding it was 40 min. The vacuum degree during the refining process was 3 Pa, and the steel tapping time after the refining was 20 min.
[0099] Annealing: The steel ingot with a diameter of 300 mm was annealed at 1100 °C for 6 h;
[0100] Forging: The annealed steel ingot is forged to obtain a forged material with a diameter of 70 mm, the initial forging temperature is 1150°C, and the final forging temperature is 830°C;
[0101] Solution heat treatment: Forgings are subjected to solution heat treatment at 820°C for 2h;
[0102] Aging treatment: The forged material after solution heat treatment was aged at 480°C for 4 h to obtain ultra-high strength steel.
[0103] Table 1 Chemical composition of ultra-high strength steel in Example 1 (unit: wt%)
[0104] C Ni Co Mo Ti O N S P La Fe 0.003 17.9 11.1 4.87 0.98 0.0017 0.0007 0.0012 0.004 0.0059 margin
[0105] As shown in Table 1, in this embodiment, [La] is 0.0059 wt%, T[O] s 0.0017wt%, T[S] m 0.0012wt%, T[N] m is 0.0007wt%, and the correction coefficients a, b, and c are 3, 2, and 1, respectively. Substituting the above data into {[RE]-(a·T[O] s +b·T[S] m )} / (c·T[N] m ) is approximately -2.3.
[0106] Table 2 shows the main inclusion distribution of the ultra-high strength steel prepared in this embodiment, from which it can be seen that the composition of the inclusions in the steel of this embodiment is mainly TiN, RE2S3 and RE2O3, and the proportions of the three inclusions are 59%, 34% and 7% respectively. The proportion of fine inclusions with a size in the range of 1 to 5 μm is 98.6%, and only 1.4% of the inclusions are 5 to 10 μm in size, and there are no larger inclusions larger than 10 μm.
[0107] Figure 1 a shows the morphology of the solid solution state original austenite in this embodiment. The intercept method is used to evaluate the original austenite grain grade as level 10, and the drawing and forging ratio Y is calculated to be 18.4≥10.
[0108] After aging treatment, the matrix is a refined multi-level martensite structure. Figure 2 a shows that the average size of the martensite lath bundle is 1.5 μm, and the X-ray diffraction experiment determines that the steel contains 13.7% reversed austenite. Figure 3 (a, b) show the organization of martensite lath bundles. Figure 3 (c, d) show the distribution of the nano-precipitated Ni3Ti and Mo-rich phase (indicated by the arrows) after aging, as well as the reversed austenite in the form of long strips or spheres. The properties of the ultra-high strength steel of this embodiment are shown in Table 15.
[0109] Table 2 Types of inclusions and number / proportion of different sizes in Example 1
[0110]
[0111] Example 2
[0112] This embodiment provides a method for preparing ultra-high strength steel, comprising the following steps:
[0113] Smelting: VIM smelting was carried out according to the chemical composition of Table 3, and a steel ingot with a diameter of 300 mm was obtained after casting; high-purity metal materials that had been fully degreased and dried were used in the smelting process; the refining time before adding rare earth lanthanum La was 65 min, and the refining time after adding it was 35 min. The vacuum degree during the refining process was 2.5 Pa, and the steel tapping time after the refining was 15 min.
[0114] Annealing: The steel ingot with a diameter of 300 mm was annealed at 1150°C for 6 h;
[0115] Forging: The annealed steel ingot is forged to obtain a forged material with a diameter of 70 mm, the initial forging temperature is 1150°C, and the final forging temperature is 830°C;
[0116] Solution heat treatment: Forgings are subjected to solution heat treatment at 820°C for 2h;
[0117] Aging treatment: The forged material after solution heat treatment was aged at 480°C for 4 h to obtain ultra-high strength steel.
[0118] Table 3 Chemical composition of ultra-high strength steel in Example 2 (unit: wt%)
[0119] C Ni Co Mo Ti O N S P La Fe 0.0054 18.0 11.1 4.96 0.97 0.0011 0.0006 0.0012 0.004 0.0041 margin
[0120] As shown in Table 3, in this embodiment, [La] is 0.0041wt%, T[O] s 0.0011wt%, T[S] m 0.0012wt%, T[N] m is 0.0006wt%, and the correction coefficients a, b, and c are 2, 1.5, and 0.5, respectively. Substituting the above data into {[RE]-(a·T[O] s +b·T[S] m )} / (c·T[N] m ) is approximately 0.33.
[0121] Table 4 shows the main inclusion distribution of the ultra-high strength steel prepared in this embodiment, from which it can be seen that the composition of the inclusions in the steel of this embodiment is mainly TiN, RE2S3 and RE2O3, and the proportions of the three inclusions are 81%, 12% and 5% respectively. The proportion of fine inclusions with a size in the range of 1 to 5 μm is 99.6%, and only 0.4% of the inclusions are 5 to 10 μm in size, and there are no larger inclusions larger than 10 μm.
[0122] Figure 1 b shows the morphology of the solid solution state original austenite in this embodiment. The intercept method is used to evaluate the original austenite grain grade as 9.5, and the drawing and forging ratio Y is calculated to be 18.4≥10.
[0123] After aging treatment, the matrix is a refined multi-level martensite structure. Figure 2 b shows that the average size of the martensite lath bundle is 4.5 μm, and the X-ray diffraction experiment determines that the steel contains 5.3% reversed austenite. The properties of the ultra-high strength steel of this embodiment are shown in Table 15.
[0124] Table 4 Types of inclusions and number / proportion of different sizes in Example 2
[0125]
[0126] Example 3
[0127] This embodiment provides a method for preparing ultra-high strength steel, comprising the following steps:
[0128] Smelting: VIM smelting was carried out according to the chemical composition of Table 5, and a steel ingot with a diameter of 300 mm was obtained after casting; high-purity metal materials that had been fully degreased and dried were used in the smelting process; the refining time before adding rare earth lanthanum La was 80 min, and the refining time after adding it was 50 min. The vacuum degree during the refining process was 3.5 Pa, and the steel tapping time after the refining was 10 min.
[0129] Annealing: The steel ingot with a diameter of 300 mm was annealed at 1150°C for 8 h;
[0130] Forging: The annealed steel ingot is forged to obtain a forged material with a diameter of 80 mm, the initial forging temperature is 1180°C, and the final forging temperature is 850°C;
[0131] Solution heat treatment: The forgings are subjected to solution heat treatment at 850°C for 3h;
[0132] Aging treatment: The forged material after solution heat treatment is aged at 500°C for 2h to obtain ultra-high strength steel.
[0133] Table 5 Chemical composition of ultra-high strength steel in Example 3 (unit: wt%)
[0134] C Ni Co Mo Ti O N S P La Fe 0.0060 17.9 11.1 4.90 1.04 0.0014 0.0008 0.0021 0.004 0.013 margin
[0135] It can be seen from Table 5 that in this embodiment, [La] is 0.013wt%, T[O] s 0.0014wt%, T[S] m 0.0021wt%, T[N] m is 0.0008wt%, and the correction coefficients a, b, and c are 5, 2.5, and 1.5, respectively. Substituting the above data into {[RE]-(a·T[O] s +b·T[S] m )} / (c·T[N] m ) is approximately 0.625.
[0136] Table 6 shows the main inclusion distribution of the ultra-high strength steel prepared in this embodiment. It can be seen that the composition of the inclusions in the steel of this embodiment is mainly TiN, RE2S3 and RE2O3, and the proportions of the three inclusions are 12%, 40% and 47% respectively. The proportion of fine inclusions in the range of 1 to 5 μm is 97.4%, and only 2.6% of the inclusions are 5 to 10 μm in size, and there are no larger inclusions larger than 10 μm. In addition, scanning electron microscopy and surface distribution spectrum ( Figure 4 ) Composite inclusions of RE-OS-TiN can be observed, which are nearly spherical or ellipsoidal and less than 5 μm in size. The above situation also exists in other embodiments, which will not be presented one by one.
[0137] Figure 1 c shows the morphology of the solid solution state original austenite in this embodiment. The intercept method is used to evaluate the original austenite grain grade as 10.5, and the drawing and forging ratio Y is calculated to be 14.1≥10.
[0138] After aging treatment, the matrix is a refined multi-level martensite structure. Figure 2 c shows that the average size of the martensite lath bundle is 1.3 μm, and the X-ray diffraction experiment determines that the steel contains 5.8% reversed austenite. The properties of the ultra-high strength steel of this embodiment are shown in Table 15.
[0139] Table 6 Types of inclusions and number / proportion of different sizes in Example 3
[0140]
[0141] Example 4
[0142] This embodiment provides a method for preparing ultra-high strength steel, comprising the following steps:
[0143] Smelting: VIM smelting was carried out according to the chemical composition of Table 7, and a steel ingot with a diameter of 300 mm was obtained after casting; high-purity metal materials that had been fully degreased and dried were used in the smelting process; the refining time before adding rare earth lanthanum La was 85 min, and the refining time after adding it was 55 min. The vacuum degree during the refining process was 3 Pa, and the steel tapping time after the refining was 12 min.
[0144] Annealing: The steel ingot with a diameter of 300 mm was annealed at 1150°C for 8 h;
[0145] Forging: The annealed steel ingot is forged to obtain a forged material with a diameter of 80 mm, the initial forging temperature is 1180°C, and the final forging temperature is 850°C;
[0146] Solution heat treatment: The forgings are subjected to solution heat treatment at 850°C for 3h;
[0147] Aging treatment: The forged material after solution heat treatment is aged at 500°C for 2h to obtain ultra-high strength steel.
[0148] Table 7 Chemical composition of ultra-high strength steel in Example 4 (unit: wt%)
[0149] C Ni Co Mo Ti O N S P La Fe 0.0064 17.8 11.1 4.86 1.03 0.0014 0.0005 0.0017 0.004 0.018 margin
[0150] It can be seen from Table 7 that in this embodiment, [La] is 0.018wt%, T[O] s 0.0014wt%, T[S] m 0.0017wt%, T[N] m is 0.0005wt%, and the correction coefficients a, b, and c are 4, 2, and 1, respectively. Substituting the above data into {[RE]-(a·T[O] s +b·T[S] m )} / (c·T[N] m ) is about 18.
[0151] Table 8 shows the main inclusion distribution of the ultra-high strength steel prepared in this embodiment, from which it can be seen that the composition of the inclusions in the steel of this embodiment is mainly TiN, RE2S3 and RE2O3, and the proportions of the three inclusions are 8%, 29% and 62% respectively. The proportion of fine inclusions with a size in the range of 1 to 5 μm is 98.1%, and only 1.9% of the inclusions are 5 to 10 μm in size, and there are no larger inclusions larger than 10 μm.
[0152] Figure 1 d shows the morphology of the solid solution state original austenite in this embodiment. The intercept method is used to evaluate the original austenite grain grade as 9.5, and the drawing and forging ratio Y is calculated to be 14.1≥10.
[0153] After aging treatment, the matrix is a refined multi-level martensite structure. Figure 2 d shows that the average size of the martensite lath bundle is 1.1 μm, and the X-ray diffraction experiment determines that the steel contains 5.1% reversed austenite. The properties of the ultra-high strength steel of this embodiment are shown in Table 15.
[0154] Table 8 Types of inclusions and number / proportion of different sizes in Example 4
[0155]
[0156]
[0157] Comparative Example 1
[0158] This comparative example provides a method for preparing ultra-high strength steel, comprising the following steps:
[0159] Smelting: VIM smelting was carried out according to the chemical composition of Table 9, and a steel ingot with a diameter of 300 mm was obtained after casting; high-purity metal materials that had been fully degreased and dried were used in the smelting process; the total refining time was 90 min, the vacuum degree during the refining process was 3.5 Pa, and the steel tapping time after the refining was 15 min.
[0160] Annealing: The steel ingot with a diameter of 300 mm was annealed at 1150°C for 8 h;
[0161] Forging: The annealed steel ingot is forged to obtain a forged material with a diameter of 80 mm, the initial forging temperature is 1180°C, and the final forging temperature is 850°C;
[0162] Solution heat treatment: The forgings are subjected to solution heat treatment at 850°C for 3h;
[0163] Aging treatment: The forged material after solution heat treatment is aged at 500°C for 2h to obtain ultra-high strength steel.
[0164] Table 9 Chemical composition of ultra-high strength steel in comparative example 1 (unit: wt%)
[0165] C Ni Co Mo Ti O N S P Fe 0.0060 17.8 11.2 4.89 0.95 0.0011 0.0007 0.0016 0.004 margin
[0166] Table 10 shows the main inclusion distribution of the ultra-high strength steel prepared in this comparative example. Figure 5 The SEM morphology and composition distribution of inclusions in the ultra-high strength steel prepared in this comparative example are shown in Table 10 and Figure 5 It can be seen that the composition of inclusions in this comparative steel is mainly TiN ( Figure 5), accounting for 99wt%, the proportion of fine inclusions in the range of 1 to 5μm is 93.8%, only 6.2% of the inclusions are 5 to 10μm in size, and there are no larger inclusions larger than 10μm.
[0167] Figure 1 e shows the morphology of the solid solution state original austenite in this comparative example. The intercept method is used to evaluate the original austenite grain grade as 8.5, and the calculated drawing and forging ratio Y=14.1≥10.
[0168] After aging treatment, the matrix is a refined multi-level martensite structure. Figure 2 e shows that the average size of the martensite lath bundle is 5.5 μm, and the X-ray diffraction experiment determines that the steel contains 3.2% reversed austenite. The properties of the ultra-high strength steel of this comparative example are shown in Table 15.
[0169] Table 10 Inclusion types and number / proportion of different sizes in comparative example 1
[0170]
[0171] Comparative Example 2
[0172] This comparative example provides a method for preparing ultra-high strength steel, comprising the following steps:
[0173] Smelting: VIM smelting was carried out according to the chemical composition of Table 11, and a steel ingot with a diameter of 300 mm was obtained after casting; high-purity metal materials that had been fully degreased and dried were used in the smelting process; the refining time before adding rare earth lanthanum La was 70 min, and the refining time after adding it was 40 min. The vacuum degree during the refining process was 3 Pa, and the steel tapping time after the refining was 20 min.
[0174] Annealing: The steel ingot with a diameter of 300 mm was annealed at 1100 °C for 6 h;
[0175] Forging: The annealed steel ingot is forged to obtain a forged material with a diameter of 100 mm. The initial forging temperature is 1180°C and the final forging temperature is 900°C.
[0176] Solution heat treatment: Forgings are subjected to solution heat treatment at 820°C for 3h;
[0177] Aging treatment: The forged material after solution heat treatment is aged at 500°C for 2h to obtain ultra-high strength steel.
[0178] Table 11 Chemical composition of ultra-high strength steel in comparative example 2 (unit: wt%)
[0179] C Ni Co Mo Ti O N S P La Fe 0.0079 17.7 11.1 5.03 1.01 0.0007 0.0009 0.0013 0.004 0.0065 margin
[0180] Table 12 shows the main inclusion distribution of the ultra-high strength steel prepared in this comparative example, from which it can be seen that the composition of the inclusions in the comparative steel is mainly TiN, RE2S3 and RE2O3, and the proportions of the three inclusions are 56%, 36% and 8% respectively. The proportion of fine inclusions in the size range of 1 to 5 μm is 98%, only 2.0% of the inclusions are 5 to 10 μm in size, and there are no larger inclusions larger than 10 μm.
[0181] Figure 1 f shows the morphology of the solid solution state original austenite in this comparative example. The intercept method is used to evaluate the original austenite grain grade as level 6, and the calculated drawing and forging ratio Y=9<10.
[0182] After aging treatment, the matrix is a refined multi-level martensite structure. Figure 2 f shows that the average size of the martensite lath bundle is 8 μm, and the X-ray diffraction experiment determines that the steel contains 5.5% reversed austenite. The properties of the ultra-high strength steel of this comparative example are shown in Table 15.
[0183] Table 12 Types and number / proportion of inclusions of different sizes in comparative example 2
[0184]
[0185] Comparative Example 3
[0186] This comparative example provides a method for preparing ultra-high strength steel, comprising the following steps:
[0187] Smelting: VIM smelting was carried out according to the chemical composition of Table 13, and a steel ingot with a diameter of 300 mm was obtained after casting; high-purity metal materials that had been fully degreased and dried were used in the smelting process; the refining time before adding rare earth lanthanum La was 85 min, and the refining time after adding it was 55 min. The vacuum degree during the refining process was 3.5 Pa, and the steel tapping time after the refining was 10 min.
[0188] Annealing: The steel ingot with a diameter of 300 mm was annealed at 1160 °C for 8 h;
[0189] Forging: The annealed steel ingot is forged to obtain a forged material with a diameter of 80 mm, with an initial forging temperature of 1180°C and a final forging temperature of 900°C;
[0190] Solution heat treatment: The forgings are subjected to solution heat treatment at 850°C for 3h;
[0191] Aging treatment: The forged material after solution heat treatment is aged at 500°C for 2h to obtain ultra-high strength steel.
[0192] Table 13 Chemical composition of ultra-high strength steel in comparative example 3 (unit: wt%)
[0193] C Ni Co Mo Ti O N S P La Fe 0.0030 17.8 11.2 5.06 0.094 0.0010 0.0006 0.0010 0.0014 0.066 margin
[0194] Table 14 shows the main inclusion distribution of the ultra-high strength steel prepared in this comparative example, from which it can be seen that the composition of the inclusions in the comparative steel is mainly TiN, RE2S3 and RE2O3, and the proportions of the three inclusions are 3%, 15% and 84% respectively. The proportion of fine inclusions with a size in the range of 1 to 5 μm is 98.2%, and only 1.8% of the inclusions are 5 to 10 μm in size, and there are no larger inclusions larger than 10 μm.
[0195] Figure 1 g shows the morphology of the solid solution state original austenite in this comparative example. The intercept method is used to evaluate the original austenite grain grade as level 9, and the calculated drawing forging ratio Y=14.1≥10.
[0196] After aging treatment, the matrix is a refined multi-level martensite structure. Figure 2 g shows that the average size of the martensite lath bundle is 2.5 μm, and the X-ray diffraction experiment determines that the steel contains 3.5% reversed austenite. The properties of the ultra-high strength steel of this comparative example are shown in Table 15.
[0197] Table 14 Types and number / proportion of inclusions in comparative example 2
[0198]
[0199] Table 15 shows the mechanical properties of the examples and comparative examples after solution treatment and aging treatment. First, compared with the impact toughness (A KV =20~31J), since no rare earth La is added in Comparative Example 1, the inclusions are mainly quadrilateral TiN, and the proportion of inclusions with a size of more than 5 μm is relatively high, which makes the impact toughness insufficient (A KV =12J); In contrast, in Comparative Example 3, 0.066% of rare earth La is added, which is not within the required range of rare earth addition. Although the inclusions are modified and refined, Figure 6 It can be seen that the excessive addition leads to the formation of large-sized undissolved elemental rare earth La particles in the matrix, which in turn destroys the homogeneity and continuity of the matrix, causing embrittlement, obvious attenuation of tensile plasticity, and difficulty in testing A KV Specific values; Different from the above two comparative examples, although comparative example 2 adds 0.006% rare earth La, which meets the rare earth addition range requirements and achieves the effect of modification and refinement of inclusions, due to the small forging deformation (which can be seen from the forging elongation ratio), the original austenite grain grade after forging is low, resulting in a large size of martensite lath bundles, and it is difficult to further improve the toughness. The impact toughness of comparative example 2 is poor (AKV =16J).
[0200] Table 15 Mechanical properties results of Examples 1 to 4 and Comparative Examples 1 to 3
[0201]
[0202]
[0203] The above embodiments and comparative examples show that the present invention can obtain an ultra-pure steel matrix, modified or refined inclusions and a multi-level complex phase structure through rare earth alloying and organizational regulation. Under the premise of ensuring the strengthening of the nano-precipitate phase, this multiple toughening effect can make the V-notch impact energy of 2.2GPa ultra-high strength steel reach 20 to 25J and above, and the maximum can reach 31J. Compared with steel without rare earth alloying or insufficient multi-level complex phase structure refinement, its impact toughness can be increased by 2 to 3 times.
[0204] It is easy for those skilled in the art to understand that, without conflict, the advantageous technical features of the above-mentioned methods can be freely combined and superimposed.
[0205] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention shall be included in the protection scope of the present invention. The above description is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present invention. These improvements and variations should also be regarded as the protection scope of the present invention.
Claims
1. An ultra-high strength steel, characterized in that: The content of rare earth RE in the ultra-high strength steel satisfies the following formula: -80<{[RE]-(a·T[O] s +b·T[S] m )} / (c·T[N] m )<200; Wherein, [RE] is the content of rare earth RE in ultra-high strength steel; T[O] s is the dissolved oxygen content in ultra-high strength steel; T[S] m is the total sulfur content in ultra-high strength steel; T[N] m is the total nitrogen content in ultra-high strength steel; [RE], T[O] s , T[S] m , T[N] m All are measured in mass percentage; a, b, and c are correction coefficient one, correction coefficient two, and correction coefficient three, respectively, and their values are 2 to 5, 1.5 to 2.5, and 0.5 to 1.
5.
2. The ultra-high strength steel according to claim 1, characterized in that: The chemical composition of the ultra-high strength steel includes, in terms of mass percentage, C≤0.01wt%, Ni: 17.0-18.5wt%, Co: 11.0-12.5wt%, Mo: 4.5-5.5wt%, Ti: 0.9-1.1wt%, S≤0.005wt%, P≤0.01wt%, O≤0.002wt%, N≤0.0015wt%, rare earth RE: 0.001-0.03wt%, and the balance is Fe; Preferably, the rare earth RE is one of lanthanum La, cerium Ce and yttrium Y.
3. The ultra-high strength steel according to claim 2, characterized in that: In the ultra-high strength steel: the mass percentage of O is ≤0.001wt%, the mass percentage of N is <0.001wt%, and the mass percentage of rare earth RE is 0.004-0.018wt%; Preferably, the mass percentage of rare earth RE is 0.0040-0.014wt%.
4. The ultra-high strength steel according to any one of claims 1 to 3, characterized in that: More than 50% of the total number of inclusions in the ultra-high strength steel has an average equivalent diameter D m The inclusions are spherical, nearly spherical or granular and dispersedly distributed with a size of 1 to 5 μm; the dispersedly distributed inclusions include rare earth sulfide RE2S3, rare earth oxide RE2O3, titanium nitride TiN, and rare earth oxysulfur-titanium nitride.
5. The ultra-high strength steel according to claim 1, characterized in that: The ultra-high strength steel has a complex phase structure and original austenite grains with a grain size greater than or equal to 8, the complex phase structure includes martensite, nano-precipitation phase and reversed austenite; the martensite includes martensite lath bundles; The average size of the martensitic lath bundles is less than or equal to 5 μm; The nano-precipitated phase includes a Ni3Ti phase and a molybdenum-rich phase, and the equivalent diameter of the nano-precipitated phase is 5 to 50 nm; In the multiphase structure, the volume percentage of the reversed austenite is 5 to 20 vol.%; Preferably, the volume percentage of the reversed austenite is 10-15 vol.%.
6. The ultra-high strength steel according to claim 1, characterized in that: The ultra-high strength steel according to claim 1 is characterized in that the properties of the ultra-high strength steel are as follows: yield strength ≥2.1 GPa, tensile strength ≥2.2 GPa, elongation after fracture ≥9%, cross-sectional shrinkage ≥50%, and V-notch impact energy ≥20-25 J.
7. A method for preparing the ultra-high strength steel according to any one of claims 1 to 6, characterized in that: The following steps are involved: Smelting: preparing materials according to the chemical composition of the ultra-high strength steel, performing smelting treatment, and obtaining steel ingots after casting; Annealing: annealing the steel ingot; the annealing time t h >(1.5D I ) / 100h, where D I is the cross-sectional size of the steel ingot obtained after casting, in mm; Forging: Forging the annealed steel ingot to obtain forged material; Solution heat treatment: The forging material is subjected to solution heat treatment; the time of the solution treatment is t s >(1.5~2.5)D b / 100h, where D b It is the cross-sectional dimension of the forging material obtained after forging, in mm; Aging treatment: The forged material after the solution heat treatment is subjected to aging treatment to obtain the ultra-high strength steel.
8. The method for preparing ultra-high strength steel according to claim 7, characterized in that: The drawing ratio Y in the forging process is ≥ 10, where Y = (D I / D b ) 2 .
9. The method for preparing ultra-high strength steel according to claim 7, characterized in that: In the smelting step: vacuum induction refining (VIM) or vacuum induction refining (VIM) + vacuum arc remelting (VAR) is used for smelting; Preferably, rare earth RE is added during VIM refining; the refining time t1 before adding rare earth RE is ≥ 60 min, and the refining time t2 after adding rare earth RE is ≥ 30 min; Preferably, the vacuum degree P during VIM refining is v ≤1~5Pa; Preferably, the steel tapping time after the smelting process is completed is t3≤30min.
10. The method for preparing ultra-high strength steel according to claim 7, characterized in that: The annealing temperature is 1000-1100°C; and / or The forging temperature is 800-1200° C.; and / or The temperature of the solution heat treatment is 800-900°C; and / or The temperature of the aging treatment is 460-540° C.; the time of the aging treatment is 1-16 hours.
Citation Information
Patent Citations
Nickel-saving type cobalt-free martensite aging ultrahigh strength steel
CN101100728A
Titanium reinforced high-cobalt martensitic aged anti-corrosion ultrahigh-strength steel and preparation method
CN103820729A
Ultra-clean rare earth steel and occluded foreign substance modification control method
CN110484811A
Multiphase reinforced ultrahigh-strength maraging stainless steel and preparation method thereof
CN113699463A
Maraging steel, preparation method of maraging steel and electronic equipment