Hydroxyl phosphorous acid aminoguanidine nonlinear optical crystal as well as preparation method and application thereof

By growing aminoguanidine hydroxyphosphite [CN4H7]HPO2(OH) nonlinear optical crystals, the shortcomings of existing short-wavelength nonlinear optical crystals in birefringence and growth size are solved, and large size, stability and low cost are achieved The preparation of nonlinear optical crystals is suitable for the application of laser devices.

CN118996633AActive Publication Date: 2024-11-22XINJIANG TECH INST OF PHYSICS & CHEM CHINESE ACAD OF SCI

Patent Information

Application Number
CN202410921095.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-22
Estimated Expiration
2044-07-10

AI Technical Summary

Technical Problem

Existing short-wavelength nonlinear optical crystals such as KBe2BO3F2, BaB2O4 and LiB3O5 have shortcomings in applications such as small birefringence and difficulty in growing large-sized crystals, which limits their application value.

Method used

Using aminoguanidine hydroxyphosphite [CN4H7]HPO2(OH) nonlinear optical crystals, crystals are grown by evaporation, hydrothermal or room temperature solution method, and a large second-order nonlinear coefficient, wide light transmission range, moderate double Crystals with refractive index.

Benefits of technology

It has achieved nonlinear optical crystals with large size, high transparency, fast growth speed and low cost. It is suitable for the production of laser devices, and has the advantages of stable physical and chemical properties and easy processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996633A_ABST
    Figure CN118996633A_ABST
Patent Text Reader

Abstract

The invention provides a hydroxyl phosphorous acid aminoguanidine nonlinear optical crystal and a preparation method and application thereof.The chemical formula of a compound of the crystal is [CN4H7] HPO4 (OH), the molecular weight is 156.09, the crystal belongs to an orthorhombic system, the space group is Pna21, the cell parameters are as follows: a = 14.9947 (10), b = 6.5890 (4), c = 6.6691 (4), alpha = 90 degrees, beta = 90 degrees, gamma = 90 degrees, the unit cell volume is 658.91 (7) 3, the frequency-doubled effect of the crystal is about 0.5 times that of KH2PO4 (KDP), the ultraviolet cut-off edge is about 196 nm, an evaporation method is adopted, and the nonlinear optical crystal is obtained. The crystal is grown by a hydrothermal method or a room-temperature solution method, and the crystal is good in chemical stability and can be applied to an all-solid-state laser as a short-wavelength ultraviolet nonlinear optical crystal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a hydroxyphosphite aminoguanidine [CN4H7]HPO2(OH) nonlinear optical crystal, a preparation method and application thereof. Background Art

[0002] Short-wavelength nonlinear optical crystals can use their frequency conversion properties to convert near-infrared, visible and other band lasers into short-wavelength lasers, and have important application value in the fields of medical treatment, communication, scientific research, etc. As we all know, the current short-wavelength nonlinear optical crystals are Chinese brand crystals KBe2BO3F2 (KBBF), BaB2O4 (BBO) and LiB3O5 (LBO), but these crystals have shortcomings such as low birefringence and difficulty in growing large-sized crystals, which limit their application to a certain extent. Therefore, the preparation and synthesis of new short-wavelength nonlinear optical crystal materials with excellent comprehensive performance is of great significance and practical value.

[0003] When designing and developing new short-wavelength nonlinear optical crystals, people hope to obtain crystals with large second-order nonlinear coefficients, wide light transmission range, short cutoff edges, and moderate birefringence. Summary of the invention

[0004] The present invention aims to provide a nonlinear optical crystal of aminoguanidine hydroxyphosphite, the chemical formula of the crystal is [CN4H7]HPO2(OH), the molecular weight is 156.09, it belongs to the orthorhombic system, the space group is Pna21, and the unit cell parameters are α=90°,β=90°,γ=90°, the unit cell volume is

[0005] Another object of the present invention is to provide a method for preparing hydroxyaminoguanidine phosphite nonlinear optical crystals, using an evaporation method, a hydrothermal method or a room temperature solution method to grow the crystals.

[0006] Another object of the present invention is to provide the use of hydroxyphosphite aminoguanidine [CN4H7]HPO2(OH) nonlinear optical crystal.

[0007] The present invention discloses a nonlinear optical crystal of aminoguanidine hydroxyphosphite, the chemical formula of which is [CN4H7]HPO2(OH), the molecular weight is 156.09, it belongs to the orthorhombic system, the space group is Pna21, and the unit cell parameters are α=90°,β=90°,γ=90°, the unit cell volume is It is made by evaporation method, hydrothermal method and room temperature solution method.

[0008] The method for preparing the hydroxyphosphite aminoguanidine nonlinear optical crystal adopts an evaporation method, a hydrothermal method or a room temperature solution method to grow the crystal.

[0009] The evaporation method for growing aminoguanidine hydroxyphosphite crystals is specifically performed in the following steps:

[0010] a. Mix the compound containing [CN4H7] and the compound containing P in a molar ratio of [CN4H7]:P=1:1, add 0-80 ml of deionized water to mix, obtain a mixed solution, and then treat it with ultrasound to fully mix and dissolve it to obtain a clear solution; the compound containing [CN4H7] is CN4H7Cl, CN4H8CO3, CN4H7NO3 or CN4H8SO4; the compound containing P is H3PO3 and K2HPO3;

[0011] b. placing the clarified solution in step a in a resistance furnace, heating it to 50-85° C. at a rate of 10-20° C. / h, and keeping it at a constant temperature for 6-15 days to evaporate the solvent, and when crystal growth is completed, a hydroxyphosphite aminoguanidine nonlinear optical crystal is obtained;

[0012] The hydrothermal method for growing aminoguanidine hydroxyphosphite crystals is specifically performed in the following steps:

[0013] a. Mix the compound containing [CN4H7] and the compound containing P uniformly in a molar ratio of [CN4H7]:P=1:1, add 0-40 ml of deionized water to fully mix and dissolve them to obtain a mixed solution, wherein the compound containing [CN4H7] is CN4H7Cl, CN4H8CO3, CN4H7NO3 or CN4H8SO4; the compound containing P is H3PO3 and K2HPO3;

[0014] b. Transfer the mixed solution in step a into a polytetrafluoroethylene liner of a hydrothermal reactor with a volume of 23-100 ml, and tighten and seal the reactor; then heat it to 180-200° C. at a rate of 10-20° C. / h, keep it at a constant temperature for 2-5 days, and then cool it to room temperature at a rate of 1-2° C. / h to obtain a hydroxyphosphite aminoguanidine nonlinear optical crystal;

[0015] The room temperature solution method for growing aminoguanidine hydroxyphosphite crystals is specifically performed in the following steps:

[0016] a. Mix the compound containing [CN4H7] and the compound containing P uniformly in a molar ratio of [CN4H7]:P=1:1, add 50-150 ml of deionized water to fully mix and dissolve them to obtain a mixed solution, wherein the compound containing [CN4H7] is CN4H7Cl, CN4H8CO3, CN4H7NO3 or CN4H8SO4; the compound containing P is H3PO3 and K2HPO3;

[0017] b. Ultrasonicate the mixed solution in step a to fully dissolve it to obtain a clear solution, tightly seal the container with a polyvinyl chloride film, place it in a static environment without shaking, pollution, or air convection, and pierce a number of small holes in the sealing film. Let it stand at room temperature for 10-20 days, then crystals will precipitate out of the solution and gradually grow, thereby obtaining hydroxyphosphite aminoguanidine nonlinear optical crystals.

[0018] The hydroxyphosphite aminoguanidine nonlinear optical crystal is used in preparing harmonic light output of 1064nm fundamental frequency light output by Nd:YAG laser for double, triple, quadruple and quintuple frequency doubling.

[0019] The invention discloses a use of the hydroxyphosphite aminoguanidine nonlinear optical crystal in preparing ultraviolet frequency-doubled light output lower than 213nm.

[0020] The hydroxyphosphite aminoguanidine nonlinear optical crystal is used in preparing a frequency doubling generator, an up or down frequency converter or an optical parametric oscillator.

[0021] The invention discloses a method for preparing a nonlinear optical crystal of aminoguanidine hydroxyphosphite. The container used in the preparation process is a polytetrafluoroethylene beaker, a polytetrafluoroethylene liner, and a hydrothermal kettle with a stainless steel liner equipped with a platinum sleeve. Before use, the container must be cleaned with acid, then rinsed with deionized water, and dried; the resistance furnace used in the preparation process is a muffle furnace or a drying box.

[0022] The hydroxyphosphite aminoguanidine nonlinear optical crystal obtained by the method of the present invention is a centimeter-sized [CN4H7]HPO2(OH) nonlinear optical crystal. By using a large-sized container and extending the growth period of the crystal, a corresponding large-sized nonlinear optical crystal [CN4H7]HPO2(OH) can be obtained. During the growth of the [CN4H7]HPO2(OH) nonlinear optical crystal, the crystal is easy to grow, transparent and without wrapping, and has the advantages of fast growth speed, low cost, and easy acquisition of large-sized crystals.

[0023] The hydroxyaminoguanidine phosphite nonlinear optical crystal obtained by the method of the present invention can be used as a nonlinear optical device by orienting the crystal blank according to the crystallographic data of the crystal, cutting the crystal according to the required angle, thickness and cross-sectional size, and polishing the light-transmitting surface of the crystal. The [CN4H7]HPO2(OH) nonlinear optical crystal has the advantages of a wide light transmission band, stable physical and chemical properties, and easy processing and storage. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The powder XRD spectrum of the compound [CN4H7]HPO2(OH) of the present invention;

[0025] Figure 2 It is the structure diagram of the [CN4H7]HPO2(OH) crystal of the present invention;

[0026] Figure 3 This is a working principle diagram of the nonlinear optical device made of [CN4H7]HPO2(OH) crystal of the present invention, wherein 1 is a laser, 2 is an emitted light beam, 3 is a [CN4H7]HPO2(OH) crystal, 4 is an output light beam, and 5 is a filter. DETAILED DESCRIPTION

[0027] The present invention is further described below in conjunction with the examples. It should be noted that the following examples cannot be used to limit the scope of protection of the present invention, and any improvements made on the basis of the present invention do not violate the spirit of the present invention. The raw materials or equipment used in the present invention, unless otherwise specified, are all commercially available.

[0028] Example 1

[0029] According to the reaction formula: CN4H7Cl+H3PO3→[CN4H7]HPO2(OH)+HCl, the [CN4H7]HPO2(OH) nonlinear optical crystal is grown by evaporation method:

[0030] a. Mix CN4H7Cl and H3PO3 in a molar ratio of 1:1, put them into a 100ml polytetrafluoroethylene beaker, add 80ml deionized water, stir evenly to obtain a mixed solution; then treat with ultrasound to fully mix and dissolve them to obtain a clear solution;

[0031] b. Place the clarified solution in step a in a resistance furnace, raise the temperature to 85°C at a rate of 20°C / h, and keep it at a constant temperature for 8 days to evaporate the solvent. When the crystal growth is completed, a hydroxyaminoguanidine phosphite nonlinear optical crystal with a size of Φ4mm×3mm×1.6mm is obtained.

[0032] Example 2

[0033] According to the reaction formula: CN4H8CO3+H3PO3→[CN4H7]HPO2(OH)+CO2+H2O, the [CN4H7]HPO2(OH) nonlinear optical crystal is grown by evaporation method:

[0034] a. Mix CN4H8CO3 and H3PO3 in a molar ratio of 1:1, put them into a 200ml polytetrafluoroethylene beaker, add 60ml deionized water, stir evenly to obtain a mixed solution, and then treat it with ultrasound to fully mix and dissolve it to obtain a clear solution;

[0035] b. Place the clarified solution in step a in a resistance furnace, raise the temperature to 75°C at a rate of 15°C / h, and keep it at a constant temperature for 10 days to evaporate the solvent. When the crystal growth is completed, a hydroxyaminoguanidine phosphite nonlinear optical crystal with a size of Φ5mm×2mm×1.1mm is obtained.

[0036] Example 3

[0037] According to the reaction formula: CN4H7NO3+H3PO3→[CN4H7]HPO2(OH)+NO2+H2O, the [CN4H7]HPO2(OH) nonlinear optical crystal is grown by evaporation method:

[0038] a. Mix CN4H7NO3 and H3PO3 in a molar ratio of 1:1, put them into a 300ml polytetrafluoroethylene beaker, add 50ml deionized water, stir evenly to obtain a mixed solution, and then treat it with ultrasound to fully mix and dissolve it to obtain a clear solution;

[0039] b. Place the mixed solution in step a in a resistance furnace, heat it to 50°C at a rate of 10°C / h, keep it at a constant temperature for 15 days to evaporate the solvent, and wait until the crystal growth is completed to obtain a hydroxyphosphite aminoguanidine nonlinear optical crystal with a size of Φ3mm×1.3mm×0.6mm.

[0040] Example 4

[0041] According to the reaction formula: CN4H7NO3+KH2PO3→[CN4H7]HPO2(OH)+KNO3, the [CN4H7]HPO2(OH) nonlinear optical crystal is grown by evaporation method:

[0042] a. Mix CN4H7NO3 and KH2PO3 in a molar ratio of 1:1, put into a 50ml polytetrafluoroethylene beaker, add 40ml deionized water and mix evenly, then treat with ultrasound to fully mix and dissolve to obtain a clear solution;

[0043] b. placing the mixed solution in step a in a resistance furnace, heating it to 55° C. at a rate of 12° C. / h, and keeping it at a constant temperature for 8 days to evaporate the solvent, and when the crystal growth is completed, a hydroxyphosphite aminoguanidine nonlinear optical crystal with a size of Φ6 mm×4.3 mm×2.1 mm is obtained;

[0044] Example 5

[0045] According to the reaction formula: CN4H8SO4+KH2PO3→[CN4H7]HPO2(OH)+KHSO4, the [CN4H7]HPO2(OH) nonlinear optical crystal is grown by evaporation method:

[0046] a. Put CN4H8SO4 and KH2PO3 in a 150ml polytetrafluoroethylene beaker in a molar ratio of 1:1 and mix them evenly. Add 70ml of deionized water and stir evenly to obtain a mixed solution. Then, treat it with ultrasound to fully mix and dissolve it to obtain a clear solution.

[0047] b. Place the clarified solution in step a in a resistance furnace, raise the temperature to 75°C at a rate of 20°C / h, and keep it at a constant temperature for 15 days to evaporate the solvent. Crystals precipitate and gradually grow. When the crystal growth is completed, a [CN4H7]HPO2(OH) nonlinear optical crystal with a size of Φ5mm×3.1mm×1.3mm is obtained.

[0048] Example 6

[0049] According to the reaction formula: CN4H7NO3+H3PO3→[CN4H7]HPO2(OH)+NO2+H2O, the [CN4H7]HPO2(OH) nonlinear optical crystal is grown by hydrothermal method:

[0050] a. Mix CN4H7NO3 and H3PO3 in a molar ratio of 1:1, put them into the polytetrafluoroethylene liner of a hydrothermal reactor with a volume of 100 ml, add 40 ml of deionized water, stir evenly to obtain a mixed solution;

[0051] b. Place the reactor in step a in a constant temperature box, heat it to 180°C at a rate of 15°C / h, keep it at this temperature for 2 days, then cool it down to room temperature at a rate of 1°C / h, open the high-pressure reactor, and obtain a [CN4H7]HPO2(OH) nonlinear optical crystal with a size of 2mm×1.3mm×0.5mm.

[0052] Example 7

[0053] According to the reaction formula: CN4H7Cl+H3PO3→[CN4H7]HPO2(OH)+HCl, the [CN4H7]HPO2(OH) nonlinear optical crystal is grown by hydrothermal method:

[0054] a. Mix CN4H7Cl and H3PO3 in a molar ratio of 1:1, add 15 ml of deionized water, stir evenly to obtain a mixed solution;

[0055] b. Transfer the mixed solution in step a into the polytetrafluoroethylene liner of a hydrothermal reactor with a volume of 23 ml, and tighten and seal the reactor; place the reactor in a constant temperature box, heat it to 190°C at a rate of 15°C / h, keep it at a constant temperature for 2 days, then cool it to room temperature at a rate of 1°C / h, open the high-pressure reactor, and obtain a [CN4H7]HPO2(OH) nonlinear optical crystal with a size of 1.3mm×0.6mm×0.3mm.

[0056] Example 8

[0057] According to the reaction formula: CN4H8SO4+KH2PO3→[CN4H7]HPO2(OH)+KHSO4, the [CN4H7]HPO2(OH) nonlinear optical crystal is grown by hydrothermal method:

[0058] a. Mix CN4H8SO4 and K2HPO3 in a molar ratio of 1:1, add 30 ml of deionized water, stir evenly to obtain a mixed solution;

[0059] b. Transfer the mixed solution in step a into the polytetrafluoroethylene liner of a hydrothermal reactor with a volume of 100 ml, and tighten and seal the reactor. Place the reactor in a constant temperature box, heat it to 200°C at a rate of 20°C / h, keep it at a constant temperature for 5 days, and then cool it to room temperature at a rate of 1°C / h. Open the high-pressure reactor to obtain a [CN4H7]HPO2(OH) nonlinear optical crystal with a size of 2.4mm×1.3mm×0.6mm.

[0060] Example 9

[0061] According to the reaction formula: CN4H8CO3+H3PO3→[CN4H7]HPO2(OH)+CO2+H2O, the [CN4H7]HPO2(OH) nonlinear optical crystal is grown by hydrothermal method:

[0062] a. Mix CN4H8CO3 and H3PO3 in a molar ratio of 1:1, add 12 ml of deionized water, stir evenly to obtain a mixed solution;

[0063] b. Transfer the mixed solution in step a into the polytetrafluoroethylene liner of a hydrothermal reactor with a volume of 23 ml, and tighten and seal the reactor; place the reactor in a constant temperature box, heat it to 180°C at a rate of 15°C / h, keep it at a constant temperature for 2 days, then cool it to room temperature at a rate of 2°C / h, open the high-pressure reactor, and you can get a [CN4H7]HPO2(OH) nonlinear optical crystal with a size of 1.8mm×0.8mm×0.4mm.

[0064] Example 10

[0065] According to the reaction formula: CN4H7NO3+KH2PO3→[CN4H7]HPO2(OH)+KNO3, the [CN4H7]HPO2(OH) nonlinear optical crystal is grown by hydrothermal method:

[0066] a. Mix CN4H7NO3 and KH2PO3 in a molar ratio of 1:1, add 40 ml of deionized water, stir evenly to obtain a mixed solution;

[0067] b. Transfer the mixed solution in step a into the polytetrafluoroethylene liner of a hydrothermal reactor with a volume of 100 ml, and tighten and seal the reactor; place the reactor in a constant temperature box, heat it to 200°C at a rate of 20°C / h, keep the temperature constant for 5 days, then cool it to room temperature at a rate of 2°C / h, open the high-pressure reactor, and you can get a [CN4H7]HPO2(OH) nonlinear optical crystal with a size of 4.3mm×1.5mm×0.6mm.

[0068] Embodiment 11

[0069] According to the reaction formula: CN4H8CO3+H3PO3→[CN4H7]HPO2(OH)+CO2+H2O, [CN4H7]HPO2(OH) is grown by room temperature solution method:

[0070] a. Mix CN4H8CO3 and H3PO3 in a molar ratio of 1:1, add 120 ml of deionized water, stir evenly to obtain a mixed solution;

[0071] b. Ultrasonicate the mixed solution in step a to mix and dissolve it fully to obtain a clear solution, then seal it with a polyvinyl chloride film, place it in a static environment without shaking, pollution, and air convection, pierce a number of small holes in the seal to adjust the volatilization rate of the solvent in the solution, and let it stand at room temperature for 10 days. Then crystals gradually precipitate from the solution. After the reaction is completed, a [CN4H7]HPO2(OH) nonlinear optical crystal with a size of 9.3 mm×4.8 mm×2 mm can be obtained.

[0072] Example 12

[0073] According to the reaction formula: CN4H7NO3+KH2PO3→[CN4H7]HPO2(OH)+KNO3, the [CN4H7]HPO2(OH) nonlinear optical crystal was grown by room temperature solution method:

[0074] a. Mix CN4H7NO3 and KH2PO3 in a molar ratio of 1:1, add 50 ml of deionized water, stir evenly to obtain a mixed solution;

[0075] b. Ultrasonicate the mixed solution in step a to mix and dissolve it fully to obtain a clear solution, then seal it with a polyvinyl chloride film and place it in a static environment without shaking, pollution and air convection. Punch a number of small holes in the seal to adjust the volatilization rate of the solvent in the solution. Let it stand at room temperature for 12 days, then crystals will gradually precipitate from the solution. After the reaction is completed, a [CN4H7]HPO2(OH) nonlinear optical crystal with a size of 5.2 mm×2 mm×1.4 mm can be obtained.

[0076] Embodiment 13

[0077] Preparation of compounds:

[0078] According to the reaction formula: CN4H7Cl+H3PO3→[CN4H7]HPO2(OH)+HCl, the [CN4H7]HPO2(OH) nonlinear optical crystal was grown by room temperature solution method:

[0079] a. Mix CN4H7Cl and H3PO3 in a molar ratio of 1:1, add 70 ml of deionized water, stir evenly to obtain a mixed solution;

[0080] b. Ultrasonicate the mixed solution in step a to mix and dissolve it fully to obtain a clear solution, then seal it with a polyvinyl chloride film, place it in a static environment without shaking, pollution, and air convection, pierce a number of small holes in the seal to adjust the volatilization rate of the solvent in the solution, and let it stand at room temperature for 15 days. Then, crystals gradually precipitate from the solution. After the reaction is completed, a [CN4H7]HPO2(OH) nonlinear optical crystal with a size of 6.4 mm×4.2 mm×2 mm can be obtained.

[0081] Embodiment 14

[0082] According to the reaction formula: CN4H7NO3+H3PO3→[CN4H7]HPO2(OH)+NO2+H2O, the [CN4H7]HPO2(OH) nonlinear optical crystal was grown by room temperature solution method:

[0083] a. Mix CN4H7NO3 and +H3PO3 in a molar ratio of 1:1, add 50 ml of deionized water, stir evenly to obtain a mixed solution;

[0084] b. Ultrasonicate the mixed solution in step a to mix and dissolve it fully to obtain a clear solution, then seal it with a polyvinyl chloride film, place it in a static environment without shaking, pollution, and air convection, pierce a number of small holes in the seal to adjust the volatilization rate of the solvent in the solution, and let it stand at room temperature for 20 days. Then crystals gradually precipitate from the solution. After the reaction is completed, a [CN4H7]HPO2(OH) nonlinear optical crystal with a size of 2 mm×1.6 mm×0.4 mm can be obtained.

[0085] Embodiment 15

[0086] According to the reaction formula: CN4H8SO4+KH2PO3→[CN4H7]HPO2(OH)+KHSO4, the [CN4H7]HPO2(OH) nonlinear optical crystal was grown by room temperature solution method:

[0087] a. Mix CN4H8SO4 and KH2PO3 in a molar ratio of 1:1, add 100 ml of deionized water, stir evenly to obtain a mixed solution;

[0088] b. Ultrasonicate the mixed solution in step a to mix and dissolve it fully to obtain a clear solution, then seal it with a polyvinyl chloride film, place it in a static environment without shaking, pollution, and air convection, pierce a number of small holes in the seal to adjust the volatilization rate of the solvent in the solution, and let it stand at room temperature for 18 days. Then crystals gradually precipitate from the solution. After the reaction is completed, a [CN4H7]HPO2(OH) nonlinear optical crystal with a size of 1.2 mm×0.8 mm×0.4 mm can be obtained.

[0089] Example 16

[0090] Any [CN4H7]HPO2(OH) nonlinear optical crystal obtained in Examples 1-15 is processed in a matching direction, and the attached Figure 3 As shown, it is placed at position 3. At room temperature, a Q-switched Nd:YAG laser is used as the light source. The incident wavelength is 1064nm. The infrared light beam 2 with a wavelength of 1064nm emitted by the Q-switched Nd:YAG laser 1 is incident on the [CN4H7]HPO2(OH) single crystal 3, generating green frequency-doubled light with a wavelength of 532nm. The output intensity is about 0.5 times that of KDP under the same conditions. At the same time, under the same experimental setup, purple frequency-doubled light with a wavelength of 266nm is generated, and the output intensity is 0.1 times that of BBO under the same conditions.

Claims

1. A nonlinear optical crystal of aminoguanidine hydroxyphosphite, characterized in that: The chemical formula of the crystal is [CN4H7]HPO2(OH), the molecular weight is 156.09, it belongs to the orthorhombic system, and the space group is Pn 21, the unit cell parameters are a =14.9947(10) Å, b =6.5890(4) Å, c =6.6691(4) Å, α= 90°, β= 90°, γ= 90°, unit cell volume is 658.91(7)Å 3 It is made by evaporation method, hydrothermal method and room temperature solution method.

2. The method for preparing the nonlinear optical crystal of aminoguanidine hydroxyphosphite according to claim 1, characterized in that Growing crystals by evaporation, hydrothermal or room temperature solution methods; The evaporation method for growing aminoguanidine hydroxyphosphite crystals is specifically performed in the following steps: a. Mix the compound containing [CN4H7] and the compound containing P uniformly in a molar ratio of [CN4H7]:P=1:1, add 0-80 ml of deionized water to mix, obtain a mixed solution, and then treat it with ultrasound to fully mix and dissolve it to obtain a clear solution; The [CN4H7]-containing compound is CN4H7Cl, CN4H8CO3, CN4H7NO3, or CN4H8SO4; the P-containing compound is H3PO3 and K2HPO3; b. placing the clarified solution in step a in a resistance furnace, heating it to 50-85° C. at a rate of 10-20° C. / h, and keeping it at a constant temperature for 6-15 days to evaporate the solvent, and when crystal growth is completed, a hydroxyphosphite aminoguanidine nonlinear optical crystal is obtained; The hydrothermal method for growing aminoguanidine hydroxyphosphite crystals is specifically performed in the following steps: a. Mix the compound containing [CN4H7] and the compound containing P uniformly in a molar ratio of [CN4H7]:P=1:1, add 0-40 ml of deionized water to fully mix and dissolve them to obtain a mixed solution, wherein the compound containing [CN4H7] is CN4H7Cl, CN4H8CO3, CN4H7NO3, or CN4H8SO4; the compound containing P is H3PO3 and K2HPO3; b. Transfer the mixed solution in step a into a polytetrafluoroethylene liner of a hydrothermal reactor with a volume of 23-100 ml, and tighten and seal the reactor; then heat it to 180-200° C. at a rate of 10-20° C. / h, keep it at a constant temperature for 2-5 days, and then cool it to room temperature at a rate of 1-2° C. / h to obtain a hydroxyphosphite aminoguanidine nonlinear optical crystal; The room temperature solution method for growing aminoguanidine hydroxyphosphite crystals is specifically performed in the following steps: a. Mix the compound containing [CN4H7] and the compound containing P uniformly at a molar ratio of [CN4H7]:P=1:1, add 50-150 ml of deionized water to fully mix and dissolve them to obtain a mixed solution, wherein the compound containing [CN4H7] is CN4H7Cl, CN4H8CO3, CN4H7NO3, or CN4H8SO4; the compound containing P is H3PO3 and K2HPO3; b. Ultrasonicate the mixed solution in step a to fully dissolve it to obtain a clear solution, tightly seal the container with a polyvinyl chloride film, place it in a static environment without shaking, pollution, or air convection, and pierce a number of small holes in the sealing film. Let it stand at room temperature for 10-20 days, then crystals will precipitate out of the solution and gradually grow, thereby obtaining hydroxyphosphite aminoguanidine nonlinear optical crystals.

3. Use of the hydroxyphosphite aminoguanidine nonlinear optical crystal as claimed in claim 1 in preparing harmonic light output of 1064nm fundamental frequency light output by Nd:YAG laser for double, triple, quadruple and quintuple frequency multiplication.

4. Use of the hydroxyphosphite aminoguanidine nonlinear optical crystal as claimed in claim 1 in the preparation of ultraviolet doubled frequency light output below 213 nm.

5. Use of the aminoguanidine hydroxyphosphite nonlinear optical crystal as claimed in claim 1 in the preparation of a frequency doubling generator, an up or down frequency converter or an optical parametric oscillator.

Citation Information

Patent Citations

  • Nonlinear optical crystal monoflurophospate

    CN109208077A

  • Guanidine tetrafluoroborate nonlinear optical crystal and preparation method and application thereof

    CN112760717A

  • Guanidine phosphate ultraviolet frequency doubling crystal material, and preparation method and application thereof

    CN113322518A

Cited By

  • Application of biguanide carbonate or biguanide nitrate as nonlinear optical crystal

    CN119356009A

  • Aminoguanidine oxalate second-order nonlinear optical crystal material as well as preparation and application thereof

    CN119753848A

  • An aminoguanidine oxalate second-order nonlinear optical crystal material and its preparation and application

    CN119753848B

  • Dihydroguanidino urea phosphite nonlinear optical crystal as well as preparation method and application thereof

    CN120099648A

  • Guanidine nitrate nonlinear optical crystal as well as preparation method and application thereof