Preparation method and application of graphene surface modified nano metal oxide composite electrode material

The growth of nanometal oxides on the graphene sheet through flame-assisted heat conduction technology solves the problem of easy stacking of graphene anode materials and low lithium storage rates in lithium-ion capacitors, and achieves the improvement of high capacity, excellent cycling performance and rate performance , suitable for lithium-ion capacitor negative electrode.

CN119008265APending Publication Date: 2024-11-22LANZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410936667.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The graphene anode material in existing lithium-ion capacitors has problems such as easy stacking, low Coulomb efficiency for the first time and insufficient SEI film thickness. The structure of metal oxides deteriorates during the cycle, resulting in a low lithium storage rate.

Method used

Using a flame-based high-temperature thermal conduction heating method, nanometal oxides are uniformly grown on the graphene sheet layer. Through the combination of metal element precursor and graphene oxide, the in-situ nucleation growth of metal oxides is achieved using flame-assisted heat conduction effect. , inhibit the dense accumulation of graphene and form a porous structure to improve electrochemical performance.

Benefits of technology

It realizes high coupling between graphene and nanometal oxide, promotes charge transfer and ion diffusion, improves the capacity characteristics and cycling performance of lithium-ion capacitors, and has the characteristics of green, efficient and energy-saving, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008265A_ABST
    Figure CN119008265A_ABST
Patent Text Reader

Abstract

The invention relates to the field of electrochemical new energy, in particular to a preparation method and application of a graphene surface modified nano metal oxide composite electrode material. A preparation method of a graphene surface modified nano metal oxide composite electrode material comprises the following steps: fully dissolving a metal element precursor in a solvent, adding a graphene oxide suspension, stirring to obtain a mixed suspension, and freeze-drying to obtain suspension powder; and carrying out transient treatment on the suspension powder by an outer flame at a certain sweeping speed, washing, and carrying out secondary drying treatment to obtain the graphene surface modified nano metal oxide composite electrode material. According to the graphene surface modified nano metal oxide composite electrode material obtained by the preparation method, the coupling property of the graphene surface modified nano metal oxide composite electrode material and the graphene surface modified nano metal oxide composite electrode material is extremely high, and metal oxide particles all grow on a graphene sheet layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of electrochemical new energy, and in particular to a preparation method and application of a graphene surface modified nano metal oxide composite electrode material. Background Art

[0002] Compared with lithium-ion batteries, the use of capacitor active materials in lithium-ion capacitors will reduce the specific energy density of the system on the one hand, but on the other hand, it enables lithium-ion capacitors to achieve rapid charging and discharging, and thus has a higher specific power density. Compared with supercapacitors, the Faraday redox reaction between lithium ions and the bulk phase of battery materials in lithium-ion capacitors is slower, which will slightly reduce its power density, but at the same time provide a higher storage capacity. It caters to the social development needs for fast charging, high power, long-lasting endurance, safety and stability of energy storage devices, and is expected to be widely used in new energy vehicles, solar energy, wind energy and other fields.

[0003] The energy storage mechanisms of the two poles of lithium-ion capacitors are different, and there are differences in energy storage rates. The ion storage mechanism is often regulated by the type of electrode materials and structural design to promote charge transfer, ion diffusion and increase the lithium storage rate of the negative electrode. Graphene has high conductivity, high stability and controllable structure, but porous graphene negative electrode materials have shortcomings such as easy stacking, low initial Coulomb efficiency and thick SEI film. Graphene can be composited with metal compounds to meet the requirements for electrochemical performance. Metal oxides (such as Fe2O3, Fe3O4, NiO, MnO, MoO2, RuO2, Nb2O5) have high theoretical capacity, low cost and wide sources, but they also have disadvantages such as poor conductivity and structural degradation during the cycle. The method of preparing composite materials by structural design, grain size refinement and modification of metal oxides on the graphene surface is expected to achieve complementary advantages and synergistically improve the lithium storage rate of the two. Summary of the invention

[0004] The purpose of the present invention is to address the above technical deficiencies and, based on the excellent thermal conductivity of graphene, propose a flame-based high-temperature heat conduction heating method to instantaneously complete the uniform in-situ growth of metal oxides on graphene sheets. Graphene oxide is reduced in this process, leaving a porous structure on the sheet. The reduced graphene tends to stack under the action of π-π stacking, which plays a spatial confinement role on the metal oxide.

[0005] A method for preparing a graphene surface modified nano-metal oxide composite electrode material comprises the following steps:

[0006] After the metal element precursor is fully dissolved in the solvent, the graphene oxide suspension is added and stirred to obtain a mixed suspension, and the suspension powder is obtained after freeze-drying; the suspension powder is subjected to an external flame transient treatment at a certain scanning speed, washed, and subjected to a secondary drying treatment to obtain a graphene surface modified nano-metal oxide composite electrode material.

[0007] Furthermore, the metal element in the metal element precursor is any one or more of vanadium, iron, cobalt, nickel and niobium.

[0008] Furthermore, in terms of mass ratio, the metal element precursor: graphene oxide = 0.2-10:1, the graphene oxide suspension is prepared by a modified Hummer method, the solid content of the graphene oxide suspension is 1-20 mg / ml, the stirring time is 6-24 h, and the temperature is 25-100°C.

[0009] Furthermore, the freeze-drying treatment of the mixed suspension adopts a liquid nitrogen quenching method.

[0010] Furthermore, the temperature of the outer flame is 600-2000° C., and the relative scanning speed between the outer flame and the suspension powder is 0.1-1 m / s.

[0011] Furthermore, the secondary drying process is freeze-drying or drying.

[0012] The graphene surface modified nano metal oxide composite electrode material obtained by the above preparation method.

[0013] The above graphene surface modified nano metal oxide composite electrode material is used as a negative electrode material for lithium ion capacitors.

[0014] The present invention has the following beneficial effects:

[0015] (1) The composite electrode material obtained by the preparation method of the present invention has extremely high coupling between graphene and nano-metal oxide, and the metal oxide particles are all grown on the graphene sheets, which inhibits the dense accumulation of multi-layer graphene after the reduction of single-layer graphene oxide and increases its interlayer spacing. The successful construction of the graphene conductive network and the nano-sized metal oxide on the sheet promote charge transfer and ion diffusion. Based on the flame-assisted heat conduction effect, the reduction of graphene oxide and the in-situ nucleation and growth of the metal oxide anchored on its sheet can be completed instantaneously. For bimetallic elements or multi-metal elements, the flame-assisted heat conduction effect is expected to form bimetallic oxides or high-entropy metal oxides. This heat treatment preparation process is short in time and can continuously complete the heat treatment of electrode materials. It has the characteristics of being green, efficient, and energy-saving, and is suitable for large-scale industrial production.

[0016] (2) The graphene surface modified nano-metal oxide composite electrode material obtained by the preparation method of the present invention can be used for the negative electrode of lithium ion capacitors. When the graphene surface modified nano-metal oxide composite electrode material is applied to the negative electrode of lithium ion capacitors, it exhibits excellent capacity characteristics, cycle performance and ultra-high rate performance, and can reach a high specific capacity of 1000 to 2000 mAh / g. The energy density of the constructed button-type lithium ion capacitor can reach 218.6Wh / kg, and the energy density of the constructed multi-layer soft-pack lithium ion capacitor can reach 151.3Wh / kg. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 ab are respectively the SEM and TEM images of the graphene surface modified nano-metal oxide composite electrode material of Example 1 of the present invention;

[0018] Figure 1 cd are respectively the SEM image and TEM image of the graphene surface modified nano-metal oxide composite electrode material of Example 14 of the present invention;

[0019] Figure 2 ab are the XRD spectra of the graphene surface modified nano-metal oxide composite electrode materials of Example 1 and Example 14 of the present invention, respectively;

[0020] Figure 3 ab are GCD curves of graphene surface modified nano-metal oxide composite electrode materials of Example 1 and Example 14 of the present invention, respectively; the current density along the arrow direction is 0.1A / g, 0.2A / g, 0.5A / g, 1A / g, 2A / g and 4A / g, respectively;

[0021] Figure 4 The Ragone diagram of the negative electrode obtained in Example 1 of the present invention and the lithium ion capacitor assembled in Comparative Example 1;

[0022] Figure 5 This is an energy density diagram of a multilayer soft-package lithium ion capacitor constructed with the negative electrode obtained in Example 1 of the present invention and activated carbon as the positive electrode. DETAILED DESCRIPTION

[0023] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.

[0024] It should be noted that the experimental methods described in the following embodiments are conventional methods unless otherwise specified, and the reagents and materials can be obtained from commercial channels unless otherwise specified.

[0025] The present invention provides a graphene surface modified nano-metal oxide composite electrode material, comprising the following steps:

[0026] Step S1, dissolving a metal element-containing precursor in a solvent and stirring to dissolve, adding a specific proportion of graphene oxide suspension and stirring for a certain period of time so that the metal cations are electrostatically adsorbed on the graphene oxide sheet; wherein the metal element in the metal element precursor is any one or more of vanadium, iron, cobalt, nickel, and niobium, and the solvent is any one or more of water, anhydrous ethanol, ethylene glycol, propylene glycol, and glycerol. In terms of mass ratio, the metal element precursor: graphene oxide = 0.2-10:1, specifically 0.2:1, 0.4:1, 1:1, 4:1, 5:1, 7:1, 10:1, the graphene oxide suspension is prepared by a modified Hummer method, the solid content of the graphene oxide suspension is 1-20 mg / ml, specifically 1 mg / ml, 4 mg / ml, 8 mg / ml, 12 mg / ml, 14 mg / ml, 16 mg / ml, 18 mg / ml, 20 mg / ml, the stirring time condition is 0.1-24h, specifically 0.1h, 1h, 6h, 10h, 14h, 18h, 22h, 24h, and the temperature condition is 0-100°C, specifically 0°C, 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C.

[0027] Step S2, freeze-drying the mixed suspension obtained in step S1 by liquid nitrogen quenching at a temperature of about -196°C to obtain a suspension powder.

[0028] Step S3, passing the suspension powder of step S2 through an outer flame at a certain sweep rate to transiently complete the reduction of graphene oxide and the in-situ nucleation growth of metal oxides on its sheets; wherein the temperature of the outer flame is 600-2500°C, specifically 600°C, 700°C, 800°C, 900°C, 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, 1500°C, 1600°C, 1700°C, etc. ℃, 1800℃, 1900℃, 2000℃, 2100℃, 2200℃, 2300℃, 2500℃, 2500℃, the relative scanning speed of the outer flame and the suspension powder is 0.1-1m / s, specifically 0.1m / s, 0.2m / s, 0.3m / s, 0.4m / s, 0.5m / s, 0.6m / s, 0.7m / s, 0.8m / s, 0.9m / s, 1m / s.

[0029] Step S4, washing and drying the sample obtained in step S3 to obtain a graphene surface modified nano-metal oxide composite electrode material. The washing method can be performed by centrifugation, suction filtration, standing, etc., the solvent added during washing includes any one or more of water, anhydrous ethanol, ethylene glycol, propylene glycol and glycerol, and the drying treatment is freeze-drying or drying.

[0030] In the present invention, the metal element precursor is dissolved in a solvent, and then a specific proportion of graphene oxide suspension is added and stirred evenly. The metal element ions are electrostatically adsorbed on the electronegative graphene oxide sheets in the solution, and then the liquid nitrogen quenching is performed to realize the rapid and uniform freezing of the liquid phase to the solid phase, avoiding the change of the solubility product constant during the slow freezing process and causing uneven segregation. Based on the excellent thermal conductivity of graphene itself, the high-temperature heat conduction heating of the auxiliary flame is used to transiently complete the uniform in-situ growth of nano-scale metal oxides on the graphene sheets. Graphene oxide is reduced in this process, leaving a porous structure on the sheet, and the reduced graphene tends to stack under the π-π stacking effect, which plays a spatial confinement role on the metal oxide. The nano-scale metal oxide anchored on the graphene sheet acts as an interlayer barrier to inhibit the self-stacking of reduced graphene oxide. When the flame is heated, the graphene oxide will be reduced and etched to produce micro-mesopores, and the addition of the metal element precursor plays the role of an antioxidant and a pore regulator.

[0031] Example 1

[0032] 240 mg of ferric chloride hexahydrate was dissolved in 10 ml of deionized water, and then 10 ml of graphene oxide suspension with a solid content of 8 mg / ml was added and stirred for 6 hours until uniformly dispersed. The obtained mixed suspension was injected into a liquid nitrogen bath, frozen and transferred to a freeze dryer for freeze drying. The freeze-dried suspension powder was flame-assisted treated at 1300°C with an external flame at a scanning speed of 0.1 m / s. Finally, it was washed with water and dried to obtain a graphene surface-modified nano-iron oxide composite electrode material.

[0033] Example 2

[0034] 80 mg of ferric chloride hexahydrate was dissolved in 10 ml of deionized water, and then 10 ml of graphene oxide suspension with a solid content of 8 mg / ml was added and stirred for 6 hours until uniformly dispersed. The obtained mixed suspension was injected into a liquid nitrogen bath, frozen and transferred to a freeze dryer for freeze drying. The freeze-dried suspension powder was flame-assisted treated at an external flame of 1300°C and a scanning speed of 0.1 m / s. Finally, it was washed with water and dried to obtain a graphene surface-modified nano-iron oxide composite electrode material.

[0035] Example 3

[0036] 160 mg of ferric chloride hexahydrate was dissolved in 10 ml of deionized water, and then 10 ml of graphene oxide suspension with a solid content of 8 mg / ml was added and stirred for 6 hours until uniformly dispersed. The obtained mixed suspension was injected into a liquid nitrogen bath, frozen and transferred to a freeze dryer for freeze drying. The freeze-dried suspension powder was flame-assisted treated with an external flame at 1300°C and a scanning speed of 0.1 m / s. Finally, it was washed with anhydrous ethanol and dried to obtain a graphene surface-modified nano-iron oxide composite electrode material.

[0037] Example 4

[0038] 240 mg of ferric chloride hexahydrate was dissolved in 10 ml of deionized water, and then 150 ml of graphene oxide suspension with a solid content of 8 mg / ml was added and stirred for 6 hours until uniformly dispersed. The obtained mixed suspension was injected into a liquid nitrogen bath, frozen and transferred to a freeze dryer for freeze drying. The freeze-dried suspension powder was flame-assisted treated at 1300°C with an external flame at a scanning speed of 0.1 m / s. Finally, it was washed with ethylene glycol and dried to obtain a graphene surface modified nano-iron oxide composite electrode material.

[0039] Example 5

[0040] 240 mg of ferric chloride hexahydrate was dissolved in 10 ml of deionized water, and then 3 ml of graphene oxide suspension with a solid content of 8 mg / ml was added and stirred for 6 hours until uniformly dispersed. The obtained mixed suspension was injected into a liquid nitrogen bath, frozen and transferred to a freeze dryer for freeze drying. The freeze-dried suspension powder was flame-assisted treated with an external flame at 1300°C and a scanning speed of 0.1 m / s. Finally, it was washed with ethylene glycol and dried to obtain a graphene surface modified nano-iron oxide composite electrode material.

[0041] Example 6

[0042] 240 mg of ferric chloride hexahydrate was dissolved in 10 ml of deionized water, and then 10 ml of graphene oxide suspension with a solid content of 8 mg / ml was added and stirred for 6 hours until uniformly dispersed. The obtained mixed suspension was injected into a liquid nitrogen bath, frozen and transferred to a freeze dryer for freeze drying. The freeze-dried suspension powder was flame-assisted treated at 1300°C with an external flame at a scanning speed of 0.1 m / s. Finally, it was washed with ethylene glycol and dried to obtain a graphene surface modified nano-iron oxide composite electrode material.

[0043] Example 7

[0044] 240 mg of ferric chloride hexahydrate was dissolved in 10 ml of deionized water, and then 10 ml of graphene oxide suspension with a solid content of 8 mg / ml was added and stirred for 6 hours until uniformly dispersed. The obtained mixed suspension was injected into a liquid nitrogen bath, frozen and transferred to a freeze dryer for freeze drying. The freeze-dried suspension powder was flame-assisted treated at 1300°C with an external flame at a scanning speed of 1 m / s. Finally, it was washed with ethylene glycol and dried to obtain a graphene surface modified nano-iron oxide composite electrode material.

[0045] Example 8

[0046] 240 mg of ferric chloride hexahydrate was dissolved in 10 ml of deionized water, and then 10 ml of graphene oxide suspension with a solid content of 8 mg / ml was added and stirred for 6 hours until uniformly dispersed. The obtained mixed suspension was injected into a liquid nitrogen bath, frozen and transferred to a freeze dryer for freeze drying. The freeze-dried suspension powder was flame-assisted treated with an external flame at 600°C and a scanning speed of 0.1 m / s. Finally, it was washed with ethylene glycol and dried to obtain a graphene surface modified nano-iron oxide composite electrode material.

[0047] Example 9

[0048] 240 mg of ferric chloride hexahydrate was dissolved in 10 ml of deionized water, and then 10 ml of graphene oxide suspension with a solid content of 8 mg / ml was added and stirred for 6 hours until uniformly dispersed. The obtained mixed suspension was injected into a liquid nitrogen bath, frozen and transferred to a freeze dryer for freeze drying. The freeze-dried suspension powder was flame-assisted treated with an external flame at 600°C and a scanning speed of 0.1 m / s. Finally, it was washed with ethylene glycol and dried to obtain a graphene surface modified nano-iron oxide composite electrode material.

[0049] Example 10

[0050] 240 mg of ferric chloride hexahydrate was dissolved in 10 ml of deionized water, and then 10 ml of graphene oxide suspension with a solid content of 8 mg / ml was added and stirred for 6 hours until uniformly dispersed. The obtained mixed suspension was injected into a liquid nitrogen bath, frozen and transferred to a freeze dryer for freeze drying. The freeze-dried suspension powder was flame-assisted treated with an external flame at 2000°C and a scanning speed of 0.1 m / s. Finally, it was washed with ethylene glycol and dried to obtain a graphene surface-modified nano-iron oxide composite electrode material.

[0051] Embodiment 11

[0052] 240 mg of ferric chloride hexahydrate was dissolved in 10 ml of deionized water, and then 80 ml of graphene oxide suspension with a solid content of 1 mg / ml was added and stirred for 6 hours until uniformly dispersed. The obtained mixed suspension was injected into a liquid nitrogen bath, frozen and transferred to a freeze dryer for freeze drying. The freeze-dried suspension powder was flame-assisted treated at 1300°C with an external flame at a scanning speed of 0.1 m / s. Finally, it was washed with ethylene glycol and dried to obtain a graphene surface modified nano-iron oxide composite electrode material.

[0053] Example 12

[0054] 240 mg of ferric chloride hexahydrate was dissolved in 10 ml of deionized water, and then 4 ml of graphene oxide suspension with a solid content of 20 mg / ml was added and stirred for 6 hours until uniformly dispersed. The obtained mixed suspension was injected into a liquid nitrogen bath, frozen and transferred to a freeze dryer for freeze drying. The freeze-dried suspension powder was flame-assisted treated with an external flame at 1300°C and a scanning speed of 0.1 m / s. Finally, it was washed with ethylene glycol and dried to obtain a graphene surface-modified nano-iron oxide composite electrode material.

[0055] Example 13

[0056] 240 mg of ferrous chloride tetrahydrate was dissolved in 10 ml of deionized water, and then 10 ml of graphene oxide suspension with a solid content of 8 mg / ml was added and stirred for 6 hours until uniformly dispersed. The obtained mixed suspension was injected into a liquid nitrogen bath, frozen and transferred to a freeze dryer for freeze drying. The freeze-dried suspension powder was flame-assisted treated at 1300°C with an external flame at a scanning speed of 0.1 m / s. Finally, it was washed with ethylene glycol and dried to obtain a graphene surface modified nano-iron oxide composite electrode material.

[0057] Embodiment 14

[0058] 160 mg of nickel chloride was dissolved in 10 ml of deionized water, and then 10 ml of graphene oxide suspension with a solid content of 8 mg / ml was added and stirred for 6 hours until uniformly dispersed. The obtained mixed suspension was injected into a liquid nitrogen bath, frozen and transferred to a freeze dryer for freeze drying. The freeze-dried suspension powder was flame-assisted treated with an external flame at 1300°C and a scanning speed of 0.1 m / s. Finally, it was washed with ethylene glycol and dried to obtain a graphene surface-modified nano-nickel oxide composite electrode material.

[0059] Embodiment 15

[0060] 240 mg of vanadium chloride was dissolved in 10 ml of deionized water, and then 10 ml of graphene oxide suspension with a solid content of 8 mg / ml was added and stirred for 6 hours until uniformly dispersed. The obtained mixed suspension was injected into a liquid nitrogen bath, frozen and transferred to a freeze dryer for freeze drying. The freeze-dried suspension powder was flame-assisted treated at an external flame of 1300°C and a scanning speed of 0.1 m / s. Finally, it was washed with ethylene glycol and dried to obtain a graphene surface-modified nano-iron oxide composite electrode material.

[0061] Example 16

[0062] 240 mg of cobalt chloride was dissolved in 10 ml of deionized water, and then 10 ml of graphene oxide suspension with a solid content of 8 mg / ml was added and stirred for 6 hours until uniformly dispersed. The obtained mixed suspension was injected into a liquid nitrogen bath, frozen and transferred to a freeze dryer for freeze drying. The freeze-dried suspension powder was flame-assisted treated with an external flame at 1300°C and a scanning speed of 0.1 m / s. Finally, it was washed with ethylene glycol and dried to obtain a graphene surface modified nano-iron oxide composite electrode material.

[0063] Embodiment 17

[0064] 240 mg of niobium chloride was dissolved in 10 ml of deionized water, and then 10 ml of graphene oxide suspension with a solid content of 8 mg / ml was added and stirred for 6 hours until uniformly dispersed. The obtained mixed suspension was injected into a liquid nitrogen bath, frozen and transferred to a freeze dryer for freeze drying. The freeze-dried suspension powder was flame-assisted treated with an external flame at 1300°C and a scanning speed of 0.1 m / s. Finally, it was washed with ethylene glycol and dried to obtain a graphene surface-modified nano-iron oxide composite electrode material.

[0065] Comparative Example 1

[0066] 10 ml of freeze-dried powder of graphene oxide suspension with a solid content of 8 mg / ml was treated by flame-assisted method at 1300° C. with an external flame at a scanning speed of 0.2 m / s to obtain reduced graphene oxide electrode material.

[0067] The performance of the graphene surface modified nano iron oxide composite electrode materials prepared in Examples 1-17 and Comparative Example 1 was tested, and the results are shown in Table 1-2:

[0068] Table 1 Performance of graphene surface modified nano-iron oxide composite electrode materials obtained in Examples 1-9

[0069]

[0070] Table 2 Performance of graphene surface modified nano-iron oxide composite electrode materials obtained in Examples 10-17 and Comparative Example 1

[0071]

[0072]

[0073] The preparation method of the present invention can achieve uniform growth of metal oxide particles on the graphene sheet, with uniform particle size and uniform distribution (such as Figure 1 ad), can effectively expand the graphene layer spacing and promote charge transfer and ion diffusion, so the rate capacity of the examples at 4A / g is greater than that of the comparative sample 1. It can be seen from Examples 1 to 5 that the amount of metal element precursor added is not the more the better. The more it is added, the higher the loading amount of the metal oxide will be and the lower the conductivity of the composite material will be, resulting in reduced rate performance. It can be seen from Examples 6 to 10 that changes in flame scanning speed and temperature have a significant effect on the structure and electrochemical properties of metal oxides grown on graphene sheets, which lies in the differences in grain size and structure grown under different thermodynamic conditions and the different oxidation etching degrees of graphene sheets. It can be seen from Examples 11 and 12 that changes in the solid content of the precursor graphene oxide suspension affect the uniformity of the composite material, so there are differences in rate performance. It can be seen from Example 13 that the valence state of the metal element has a significant effect on the electrochemical performance, Fe 2+ Fe 3+ The adsorption performance is poor, and more Fe3O4 is generated after thermal reduction, and its theoretical capacity is lower than that of Fe2O3. Therefore, its specific capacity at 0.1A / g and specific capacity at 4A / g are worse than those in Example 1. It can be seen from Examples 14 to 17 that this preparation method can modify other metal oxides such as nickel oxide on graphene sheets, has scalability, and the rate performance is improved relative to the rate performance of Comparative Example 1.

[0074] Figure 2 a is the XRD spectrum of the composite electrode material obtained in Example 1, Figure 2 It can be seen from a that for some single metal elements, two-step oxidation can be achieved. For example, Fe first forms Fe3O4 during the heat conduction process, and the Fe3O4 on the surface will be continuously oxidized to Fe2O3 during this process, forming a Fe3O4-Fe2O3 heterogeneous hybrid structure. Figure 2 b is the XRD spectrum of the composite electrode material obtained in Example 14. Figure 2 b It can be seen that the composite electrode material prepared in Example 14 successfully achieved the modification of nickel oxide on the graphene sheet, which has scalability.

[0075] Figure 3 a is the GCD curve of the composite electrode material obtained in Example 1, Figure 3a It can be seen that the rate capacity retention rate of the composite electrode material prepared in Example 1 can reach 49.4% (0.1-4 A / g); Figure 3 b is the GCD curve of the composite electrode material obtained in Example 14. Figure 3 b It can be seen that the rate capacity retention rate of the composite electrode material prepared in Example 14 can reach 38.4% (0.1-4 A / g), while that of Comparative Example 1 is only 12.9% (0.1-4 A / g).

[0076] The present invention provides a graphene surface modified nano-metal oxide composite electrode material, which is prepared according to the preparation method of the graphene surface modified nano-metal oxide composite electrode material described above. Since the graphene surface modified nano-metal oxide composite electrode material adopts all the technical solutions of all the above embodiments, it at least has the beneficial effects brought by the technical solutions of the above embodiments, which will not be repeated here one by one.

[0077] The present invention also provides a negative electrode for a lithium ion capacitor, wherein the graphene surface modified nano-metal oxide composite electrode material described above is used as the negative electrode of the lithium ion capacitor electrode.

[0078] It should be noted that when the composite electrode material obtained by the preparation method of the present invention is used as the negative electrode of a lithium ion capacitor, a capacity of 1000 to 2000 mAh / g can be achieved at a current density of 0.1 A / g. The composite electrode material obtained in Example 1 of the present invention is used as the negative electrode, and the composite electrode material obtained in Comparative Example 1 is used as the positive electrode to assemble a button-type lithium ion capacitor to achieve an energy density of 218.6 Wh / kg (432 W / kg) and a power density of 43.2 kW / kg (90.1 Wh / kg) (e.g. Figure 4 shown).

[0079] The energy density of the multilayer soft-pack lithium ion capacitor constructed by using the composite electrode material obtained in Example 1 of the present invention as the negative electrode and activated carbon as the positive electrode can reach 151.3Wh / kg (such as Figure 5 shown).

[0080] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the embodiments shown and described herein.

Claims

1. A method for preparing a graphene surface modified nano-metal oxide composite electrode material, characterized in that: The following steps are involved: After the metal element precursor is fully dissolved in the solvent, the graphene oxide suspension is added and stirred to obtain a mixed suspension, and the suspension powder is obtained after freeze-drying; the suspension powder is subjected to an external flame transient treatment at a certain scanning speed, washed, and subjected to a secondary drying treatment to obtain a graphene surface modified nano-metal oxide composite electrode material.

2. The method for preparing a graphene surface modified nano-metal oxide composite electrode material according to claim 1, characterized in that: The metal element in the metal element precursor is any one or more of vanadium, iron, cobalt, nickel and niobium.

3. The method for preparing a graphene surface modified nano-metal oxide composite electrode material according to claim 1, characterized in that: In terms of mass ratio, the metal element precursor: graphene oxide = 0.2-10:1, the graphene oxide suspension is prepared by a modified Hummer method, the solid content of the graphene oxide suspension is 1-20 mg / ml, the stirring time condition is 6-24 hours, and the temperature condition is 25-100°C.

4. The method for preparing a graphene surface modified nano-metal oxide composite electrode material according to claim 1, characterized in that: The freeze-drying treatment of the mixed suspension was carried out by liquid nitrogen quenching method.

5. The method for preparing a graphene surface modified nano-metal oxide composite electrode material according to claim 1, characterized in that: The temperature of the outer flame is 600-2000°C, and the relative scanning speed between the outer flame and the suspension powder is 0.1-1 m / s.

6. The method for preparing a graphene surface modified nano-metal oxide composite electrode material according to claim 1, characterized in that: The secondary drying process is freeze-drying or drying.

7. A graphene surface modified nano-metal oxide composite electrode material obtained according to the preparation method according to any one of claims 1 to 6.

8. Use of the graphene surface modified nano-metal oxide composite electrode material as claimed in claim 7 as a negative electrode material for lithium ion capacitors.