Light-emitting diode chip with double electron blocking layers and preparation method of light-emitting diode chip
By providing the first and second electron barrier layers on both sides of the active layer of the light emitting diode chip, a potential barrier is formed, and the electron escape problem is solved and the recombination efficiency of the light emitting diode chip is improved.
Patent Information
- Application Number
- CN202411142141.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-22
AI Technical Summary
During the light emission process of the light emitting diode chip, some electrons may escape before entering the active layer or after leaving the active layer, resulting in a reduced recombination efficiency.
Using a dual electron barrier layer structure, a first electron barrier layer and a second electron barrier layer are respectively provided on both sides of the active layer to form a potential barrier to prevent electrons from escaping and improve the recombination efficiency of electrons and holes.
It effectively increases the probability of recombination of electrons and holes in the active layer, improves the internal quantum efficiency of the light-emitting diode chip, prevents electrons from escaping, and thus improves the recombination efficiency.
Smart Images

Figure CN119008798A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of semiconductor technology, and in particular relates to a light emitting diode chip with a double electron blocking layer and a preparation method thereof. Background Art
[0002] A light emitting diode (LED) is a semiconductor diode that can convert electrical energy into light energy.
[0003] In the related art, the LED chip is the main component of the LED, which mainly includes an epitaxial layer. The epitaxial layer includes an N-type semiconductor layer, an active layer and a P-type semiconductor layer. Electrons are injected from the N-type semiconductor layer into the active layer and recombine with holes injected from the P-type semiconductor layer to emit light.
[0004] However, in the process of light emitting diode chip emitting light, some electrons may escape before entering the active layer or after leaving the active layer, resulting in reduced recombination efficiency. Summary of the invention
[0005] The embodiment of the present disclosure provides a light-emitting diode chip with a double electron blocking layer and a preparation method thereof, which can effectively increase the recombination probability of electrons and holes in the active layer and improve the internal quantum efficiency of the light-emitting diode chip. The technical solution is as follows:
[0006] On the one hand, an embodiment of the present disclosure provides a light-emitting diode chip, comprising a first semiconductor layer, a first electron blocking layer, an active layer, a second electron blocking layer, and a second semiconductor layer stacked in sequence;
[0007] The first semiconductor layer is of a first conductivity type, and the second semiconductor layer is of a second conductivity type, and the second conductivity type is different from the first conductivity type;
[0008] The first electron blocking layer and the second electron blocking layer are both Al x In 1-x P layer, 0.5≤x≤1.
[0009] In one implementation of the present disclosure, the thickness of the first electron blocking layer is 10 to 15 nm;
[0010] The thickness of the second electron blocking layer is 10-15 nm.
[0011] In another implementation of the present disclosure, the light-emitting diode chip further includes a first waveguide layer and a second waveguide layer;
[0012] The first waveguide layer is located between the first electron blocking layer and the active layer;
[0013] The second waveguide layer is located between the second electron blocking layer and the active layer.
[0014] In yet another implementation of the present disclosure, the thickness of the first waveguide layer is 100-200 nm;
[0015] The thickness of the second waveguide layer is 100-200 nm.
[0016] In another implementation of the present disclosure, the light-emitting diode chip further includes a first ohmic contact layer, an electrode fixing layer, and a first current spreading layer stacked in sequence;
[0017] The first ohmic contact layer is an N-type GaAs layer, the electrode fixing layer is an N-type GaInP layer, and the first current spreading layer is an N-type (Al x Ga 1-x ) 0.5 In 0.5 P layer, 0.3≤x≤1;
[0018] The first current spreading layer is located on a side of the first semiconductor layer facing away from the first electron blocking layer.
[0019] In another implementation of the present disclosure, the thickness of the first ohmic contact layer is 50-80 nm;
[0020] The thickness of the electrode firming layer is 10 to 20 nm;
[0021] The thickness of the first current spreading layer is 3-4 μm.
[0022] In another implementation of the present disclosure, the light-emitting diode chip further includes a second current spreading layer and a second ohmic contact layer stacked in sequence;
[0023] The second current spreading layer and the second ohmic contact layer are both P-type GaP layers;
[0024] The second current spreading layer is located on a side of the second semiconductor layer facing away from the second electron blocking layer.
[0025] In another implementation of the present disclosure, the thickness of the second current spreading layer is 1-2 μm;
[0026] The thickness of the second ohmic contact layer is 50-200 nm.
[0027] On the other hand, an embodiment of the present disclosure provides a method for preparing a light emitting diode chip, the method comprising:
[0028] preparing a first semiconductor layer, wherein the first semiconductor layer is of a first conductivity type;
[0029] A first electron blocking layer is prepared on one side of the first semiconductor layer. The first electron blocking layer is Al x In 1-x P layer, 0.5≤x≤1;
[0030] preparing an active layer on one side of the first electron blocking layer;
[0031] A second electron blocking layer is prepared on one side of the active layer, wherein the second electron blocking layer is Al x In 1-x P layer, 0.5≤x≤1;
[0032] A second semiconductor layer is prepared on one side of the second electron blocking layer. The second semiconductor layer is of a second conductivity type, and the second conductivity type is different from the first conductivity type.
[0033] In one implementation of the present disclosure, preparing the first electron blocking layer includes:
[0034] The growth temperature is set to 700-720°C, the growth rate is set to 0.35-0.45 nm / s, and the growth thickness is set to 10-15 nm;
[0035] The first semiconductor layer is grown.
[0036] The technical solution provided by the embodiments of the present disclosure has the following beneficial effects:
[0037] During the operation of the light-emitting diode chip, electrons are injected from one of the first semiconductor layer and the second semiconductor layer into the active layer, and recombine with holes injected from the other of the first semiconductor layer and the second semiconductor layer to emit light. Since the first electron blocking layer and the second electron blocking layer are respectively disposed on both sides of the active layer, the first electron blocking layer and the second electron blocking layer can optimize the injection and transmission characteristics of carriers, and utilize the potential barrier formed by the first electron blocking layer and the second electron blocking layer to improve the recombination efficiency of electrons and holes.
[0038] That is to say, the light-emitting diode chip provided in the embodiment of the present disclosure forms a potential barrier by respectively arranging a first electron blocking layer and a second electron blocking layer on both sides of the active layer, thereby preventing electrons from escaping and improving the recombination efficiency of electrons and holes. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the technical solutions in the embodiments of the present disclosure, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0040] Figure 1 is a structural schematic diagram of a light-emitting diode chip provided by an embodiment of the present disclosure;
[0041] Figure 2 is a flow chart of a method for preparing a light-emitting diode chip provided by an embodiment of the present disclosure;
[0042] Figure 3 It is a flow chart of another method for preparing a light emitting diode chip provided in an embodiment of the present disclosure.
[0043] The symbols in the figure mean the following:
[0044] 11. first semiconductor layer; 12. active layer; 13. second semiconductor layer;
[0045] 21. a first electron blocking layer; 22. a second electron blocking layer;
[0046] 31. first waveguide layer; 32. second waveguide layer;
[0047] 41. a first ohmic contact layer; 42. a second ohmic contact layer;
[0048] 5. Electrode firming layer;
[0049] 61. a first current spreading layer; 62. a second current spreading layer;
[0050] 7. Substrate;
[0051] 8. Buffer layer;
[0052] 9. Erosion cut-off layer.
[0053] The above drawings show clear embodiments of the present disclosure, which will be described in more detail below. These drawings and text descriptions are not intended to limit the scope of the present disclosure in any way, but to illustrate the concepts of the present disclosure to those skilled in the art by referring to specific embodiments. DETAILED DESCRIPTION
[0054] In order to make the objectives, technical solutions and advantages of the present disclosure more clear, the embodiments of the present disclosure will be further described in detail below with reference to the accompanying drawings.
[0055] The embodiment of the present disclosure provides a light emitting diode chip, Figure 1 is a schematic diagram of the structure of the light emitting diode chip, see Figure 1 In this embodiment, the light emitting diode chip includes a first semiconductor layer 11, a first electron blocking layer 21, an active layer 12, a second electron blocking layer 22 and a second semiconductor layer 13 which are stacked in sequence.
[0056] The first semiconductor layer 11 is of the first conductivity type, the second semiconductor layer 13 is of the second conductivity type, and the second conductivity type is different from the first conductivity type. The first electron blocking layer 21 and the second electron blocking layer 22 are both Al x In 1-x P layer, 0.5≤x≤1.
[0057] During the operation of the light-emitting diode chip, electrons are injected from one of the first semiconductor layer 11 and the second semiconductor layer 13 into the active layer 12, and are recombined with holes injected from the other of the first semiconductor layer 11 and the second semiconductor layer 13 to emit light. Since the first electron blocking layer 21 and the second electron blocking layer 22 are respectively disposed on both sides of the active layer 12, the first electron blocking layer 21 and the second electron blocking layer 22 can optimize the injection and transport characteristics of carriers, and utilize the potential barrier formed by the first electron blocking layer 21 and the second electron blocking layer 22 to improve the recombination efficiency of electrons and holes.
[0058] That is to say, the light-emitting diode chip provided in the embodiment of the present disclosure forms a potential barrier by respectively disposing a first electron blocking layer 21 and a second electron blocking layer 22 on both sides of the active layer 12, thereby preventing electrons from escaping and improving the recombination efficiency of electrons and holes.
[0059] In this embodiment, the thickness of the first electron blocking layer 21 is 10-15 nm, and the thickness of the second electron blocking layer 22 is 10-15 nm.
[0060] In the above implementation, the first electron blocking layer 21 and the second electron blocking layer 22 are set to the above thickness range, which can effectively ensure that the first electron blocking layer 21 and the second electron blocking layer 22 block the escaping electrons on the one hand, and can shorten the preparation time on the other hand, thereby improving the overall preparation efficiency of the light-emitting diode chip.
[0061] Exemplarily, the thickness of the first electron blocking layer 21 is 12 nm, and the thickness of the second electron blocking layer 22 is the same as the thickness of the first electron blocking layer 21, which is also 12 nm. Of course, the thickness of the first electron blocking layer 21 and the thickness of the second electron blocking layer 22 may also be different, and the present disclosure does not limit this.
[0062] Exemplarily, V / III of the first electron blocking layer 21 is 25-35, and V / III of the second electron blocking layer 22 is 25-35.
[0063] In this embodiment, the first semiconductor layer 11 is an N-type AlInP layer, the active layer 12 is a multi-quantum well layer, and the second semiconductor layer 13 is a P-type AlInP layer. The first electron blocking layer 21 is located on the side of the first semiconductor layer 11 facing the active layer 12, and the second electron blocking layer 22 is located on the side of the second semiconductor layer 13 facing the active layer 12.
[0064] In the above implementation, the first semiconductor layer 11 is an N-type layer, the second semiconductor layer 13 is a P-type layer, and energy transition occurs between the first semiconductor layer 11 and the second semiconductor layer 13, so that light can be emitted at the active layer 12. In addition, by providing the first electron blocking layer 21 and the second electron blocking layer 22 between the first semiconductor layer 11 and the second semiconductor layer 13, a potential barrier is formed to prevent electrons from escaping, thereby improving the recombination efficiency of electrons and holes.
[0065] In addition, since the first semiconductor layer 11 is an N-type AlInP layer and the second semiconductor layer 13 is a P-type AlInP layer, the light emitting diode chip is a red light chip.
[0066] Exemplarily, the first semiconductor layer 11 has a thickness of 200-300 nm, a V / III ratio of 25-35, and a carrier concentration of 1e18-2e18.
[0067] Exemplarily, the thickness of the second semiconductor layer 13 is 200-300 nm, V / III is 25-35, and the carrier concentration is 7e17-9e17.
[0068] Exemplarily, the multi-quantum well layer includes quantum well layers and quantum barrier layers that are periodically and alternately stacked, wherein the thickness of the quantum well layer is 4-6 nm, the thickness of the quantum barrier layer is 8 nm-12 nm, the number of stacking periods is 5-10, and V / III is 25-35.
[0069] In this embodiment, the light emitting diode chip further includes a first waveguide layer 31 and a second waveguide layer 32 . The first waveguide layer 31 is located between the first electron blocking layer 21 and the active layer 12 , and the second waveguide layer 32 is located between the second electron blocking layer 22 and the active layer 12 .
[0070] In the above implementation, the first waveguide layer 31 is an N-type waveguide layer, and the second waveguide layer 32 is a P-type waveguide layer.
[0071] Exemplarily, the thickness of the first waveguide layer 31 is 100-200 nm, and V / III is 25-35. The thickness of the second waveguide layer 32 is 100-200 nm, and V / III is 25-35.
[0072] In this embodiment, the light emitting diode chip further includes a substrate 7 , and the substrate 7 is a GaAs substrate.
[0073] In the above implementation, the substrate 7 can provide a support basis for the growth of other sub-layers.
[0074] In this embodiment, the light emitting diode chip further includes a buffer layer 8, which is located on one side of the substrate 7. The buffer layer 8 is an N-type GaAs layer. The thickness of the buffer layer 8 is 250-350 nm, and V / III is 25-35.
[0075] In the above implementation, by providing the buffer layer 8, a good foundation can be provided for the preparation of other sub-layers, which is helpful to solve the problem of lattice mismatch. In addition, by designing the thickness of the buffer layer 8 to be within the above range, on the one hand, it can avoid reducing the quality of the subsequently grown crystals due to being too thin, and on the other hand, it can avoid increasing the absorption of light by the buffer layer 8 due to being too thick, thereby reducing the luminous efficiency of the light-emitting diode chip.
[0076] In this embodiment, the light emitting diode further includes a corrosion stop layer 9, which is located on the side of the buffer layer 8 facing away from the substrate. The corrosion stop layer 9 is an N-type GaInP layer, has a thickness of 250-350 nm, and V / III is 25-35.
[0077] In this embodiment, the light emitting diode chip further includes a first ohmic contact layer 41 , an electrode fixing layer 5 , and a first current spreading layer 61 which are stacked in sequence.
[0078] The first ohmic contact layer 41 is an N-type GaAs layer, the electrode fixing layer 5 is an N-type GaInP layer, and the first current spreading layer 61 is an N-type (Al x Ga 1-x ) 0.5 In 0.5 P layer, 0.3≤x≤1. The first current spreading layer 61 is located on a side of the first semiconductor layer 11 facing away from the first electron blocking layer 21 .
[0079] In the above implementation, the first ohmic contact layer 41, the electrode fixing layer 5, and the first current spreading layer 61 are sequentially stacked on the corrosion stop layer 9. The first ohmic contact layer 41 is an N-type ohmic contact layer for realizing ohmic contact, the electrode fixing layer 5 is used to improve the adhesion firmness of the electrode, and the first current spreading layer 61 is used to realize longitudinal and lateral current expansion, which is beneficial to improve the voltage of the light-emitting diode chip and improve the luminous efficiency of the light-emitting diode chip.
[0080] Exemplarily, the first ohmic contact layer 41 has a thickness of 50-80 nm, a V / III ratio of 25-35, and a carrier concentration of 3e18-5e18.
[0081] Exemplarily, the thickness of the electrode securing layer 5 is 10 nm to 20 nm, and V / III is 25 to 35.
[0082] Exemplarily, the first current spreading layer 61 has a thickness of 3-4 μm, a V / III ratio of 25-35, and a carrier concentration of 1e18-3e18.
[0083] In this embodiment, the light emitting diode chip further includes a second current spreading layer 62 and a second ohmic contact layer 42 which are stacked in sequence.
[0084] The second current spreading layer 62 and the second ohmic contact layer 42 are both P-type GaP layers. The second current spreading layer 62 is located on a side of the second semiconductor layer 13 facing away from the second electron blocking layer 22 .
[0085] In the above implementation, the second ohmic contact layer 42 is a P-type ohmic contact layer for achieving ohmic contact, and the second current spreading layer 62 is used to achieve longitudinal and lateral current spreading, which is beneficial to improving the voltage of the LED chip and improving the luminous efficiency of the LED chip.
[0086] Exemplarily, the second current spreading layer 62 has a thickness of 1-2 μm, a V / III ratio of 25-35, and a carrier concentration of 1e19-6e19.
[0087] Exemplarily, the thickness of the second ohmic contact layer 42 is 50 nm to 200 nm.
[0088] Figure 2 A method for preparing a light emitting diode chip provided in an embodiment of the present disclosure, combined with Figure 2 In this embodiment, the preparation method comprises:
[0089] Step 201: Prepare a first semiconductor layer 11, where the first semiconductor layer 11 is of a first conductivity type.
[0090] Step 202: Prepare a first electron blocking layer 21 on one side of the first semiconductor layer 11. The first electron blocking layer 21 is Al x In 1-x P layer, 0.5≤x≤1.
[0091] Step 203 : preparing an active layer 12 on one side of the first electron blocking layer 21 .
[0092] Step 204: Prepare a second electron blocking layer 22 on one side of the active layer 12. The second electron blocking layer 22 is Al x In 1-x P layer, 0.5≤x≤1.
[0093] Step 205: Prepare a second semiconductor layer 13 on one side of the second electron blocking layer 22, wherein the second semiconductor layer 13 is of a second conductivity type, and the second conductivity type is different from the first conductivity type.
[0094] In the light-emitting diode chip prepared by the above preparation method, during operation, electrons are injected from one of the first semiconductor layer 11 and the second semiconductor layer 13 into the active layer 12, and are recombined with holes injected from the other of the first semiconductor layer 11 and the second semiconductor layer 13 to emit light. Since the first electron blocking layer 21 and the second electron blocking layer 22 are respectively provided on both sides of the active layer 12, the first electron blocking layer 21 and the second electron blocking layer 22 can optimize the injection and transport characteristics of carriers, and utilize the potential barrier formed by the first electron blocking layer 21 and the second electron blocking layer 22 to improve the recombination efficiency of electrons and holes.
[0095] That is, by respectively arranging the first electron blocking layer 21 and the second electron blocking layer 22 on both sides of the active layer 12 , a potential barrier is formed to prevent electrons from escaping, thereby improving the recombination efficiency of electrons and holes.
[0096] Figure 3 Another method for preparing a light emitting diode chip provided in the embodiment of the present disclosure is combined with Figure 3 In this embodiment, the preparation method comprises:
[0097] Step 301: Provide a substrate 7.
[0098] Exemplarily, the substrate is a GaAs substrate.
[0099] Step 302: Prepare a buffer layer 8.
[0100] Exemplarily, the buffer layer 8 is an N-type GaAs layer, the growth temperature is set to 680-700° C., the growth thickness is set to 250-350 nm, the growth rate is set to 1-1.5 nm / s, and the dopant is set to Si2H6.
[0101] Step 303: Prepare the corrosion stop layer 9.
[0102] Exemplarily, the corrosion stop layer 9 is an N-type GaInP layer, the growth temperature is set to 680-700° C., the growth thickness is set to 250-350 nm, the growth rate is set to 0.6-0.8 nm / s, and the dopant is set to Si2H6.
[0103] Step 304 : preparing a first ohmic contact layer 41 .
[0104] Exemplarily, the first ohmic contact layer 41 is an N-type GaAs layer, the growth temperature is set to 680-700° C., the growth thickness is set to 50-80 nm, the growth rate is set to 1-1.5 nm / s, and the dopant is set to Si2H6.
[0105] Step 305: Prepare the electrode fixing layer 5.
[0106] Exemplarily, the electrode fixing layer 5 is an N-type GaInP layer, the growth temperature is set to 680-700° C., the growth thickness is set to 10-20 nm, the growth rate is set to 0.6-0.8 nm / s, and the dopant is set to Si2H6.
[0107] Step 306 : preparing a first current spreading layer 61 .
[0108] Exemplarily, the first current spreading layer 61 is N-type (Al x Ga 1-x ) 0.5 In 0.5 P layer, 0.3≤x≤1, the growth temperature is set to 680-700°C, the growth thickness is set to 3-4μm, the growth rate is set to 0.6-0.8nm / s, and the dopant is set to Si2H6.
[0109] Step 307 : preparing the first semiconductor layer 11 .
[0110] Exemplarily, the first semiconductor layer 11 is an N-type AlInP layer, the growth temperature is set to 700° C. to 720° C., the growth thickness is set to 200 to 300 nm, and the growth rate is set to 0.35 to 0.45 nm / s.
[0111] Step 308: preparing a first electron blocking layer 21 .
[0112] For example, the first electron blocking layer 21 is Al x In 1-x For the P layer, 0.5≤x≤1, the growth temperature is set to 700-720°C, the growth thickness is set to 10-15nm, and the growth rate is set to 0.35-0.45nm / s.
[0113] Step 309 : preparing the first waveguide layer 31 .
[0114] Exemplarily, the growth temperature is set to 680-700° C., the growth thickness is set to 100-200 nm, and the growth rate is set to 0.35-0.45 nm / s.
[0115] Step 310: Prepare the active layer 12.
[0116] Exemplarily, the active layer 12 is a multi-quantum well layer, and quantum well layers and quantum barrier layers are grown alternately periodically, wherein the growth temperature is set to 670°C to 700°C, the growth rate is set to 0.35 to 0.45 nm / s, the number of stacking periods is 5 to 10, the growth thickness of the quantum well layer is set to 4 to 6 nm, and the growth thickness of the quantum barrier layer is set to 8 to 12 nm.
[0117] Step 311: Prepare the second waveguide layer 32.
[0118] Exemplarily, the growth temperature is set to 680-700° C., the growth thickness is set to 100-200 nm, and the growth rate is set to 0.35-0.45 nm / s.
[0119] Step 312: preparing the second electron blocking layer 22.
[0120] For example, the second electron blocking layer 22 is Al x In 1-x For the P layer, 0.5≤x≤1, the growth temperature is set to 700-720°C, the growth thickness is set to 10-15nm, and the growth rate is set to 0.35-0.45nm / s.
[0121] Step 313: preparing a second semiconductor layer 13 .
[0122] Exemplarily, the second semiconductor layer 13 is a P-type AlInP layer, the growth temperature is set to 700° C. to 720° C., the growth thickness is set to 200 to 300 nm, and the growth rate is set to 0.35 to 0.45 nm / s.
[0123] Step 314 : preparing a second current spreading layer 62 .
[0124] Exemplarily, the second current spreading layer 62 is a P-type GaP layer, the growth temperature is set to 720-750° C., the growth thickness is set to 1-2 μm, and the growth rate is set to 3-3.5 nm / s.
[0125] Step 315: preparing a second ohmic contact layer 42 .
[0126] Exemplarily, the second ohmic contact layer 42 is a P-type GaP layer, the growth temperature is set to 640° C. to 660° C., the growth thickness is set to 50 nm to 200 nm, and the growth rate is set to 1 nm / s to 2 nm / s.
[0127] Unless otherwise defined, the technical terms or scientific terms used herein shall have the usual meanings understood by persons of ordinary skill in the field to which the present disclosure belongs. The words "first", "second", "third" and similar words used in the patent application specification and claims of the present disclosure do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, words such as "one" or "one" do not indicate a quantity limitation, but indicate the existence of at least one. Words such as "include" or "comprise" and similar words mean that the elements or objects appearing before "include" or "comprise" include the elements or objects listed after "include" or "comprise" and their equivalents, and do not exclude other elements or objects. Words such as "connect" or "connected" and similar words are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.
[0128] The above description is only an optional embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure shall be included in the protection scope of the present disclosure.
Claims
1. A light emitting diode chip, characterized in that: It comprises a first semiconductor layer (11), a first electron blocking layer (21), an active layer (12), a second electron blocking layer (22) and a second semiconductor layer (13) which are stacked in sequence; The first semiconductor layer (11) is of a first conductivity type, and the second semiconductor layer (13) is of a second conductivity type, and the second conductivity type is different from the first conductivity type; The first electron blocking layer (21) and the second electron blocking layer (22) are both Al x In 1-x P layer, 0.5≤x≤1.
2. The light emitting diode chip according to claim 1, characterized in that: The thickness of the first electron blocking layer (21) is 10 to 15 nm; The thickness of the second electron blocking layer (22) is 10-15 nm.
3. The light emitting diode chip according to claim 1, characterized in that: The light-emitting diode chip further comprises a first waveguide layer (31) and a second waveguide layer (32); The first waveguide layer (31) is located between the first electron blocking layer (21) and the active layer (12); The second waveguide layer (32) is located between the second electron blocking layer (22) and the active layer (12).
4. The light emitting diode chip according to claim 3, characterized in that: The thickness of the first waveguide layer (31) is 100-200 nm; The thickness of the second waveguide layer (32) is 100-200 nm.
5. The light emitting diode chip according to claim 1, characterized in that: The light-emitting diode chip further comprises a first ohmic contact layer (41), an electrode fixing layer (5), and a first current spreading layer (61) which are stacked in sequence; The first ohmic contact layer (41) is an N-type GaAs layer, the electrode fixing layer (5) is an N-type GaInP layer, and the first current spreading layer (61) is an N-type (Al x Ga 1-x ) 0.5 In 0.5 P layer, 0.3≤x≤1; The first current spreading layer (61) is located on a side of the first semiconductor layer (11) facing away from the first electron blocking layer (21).
6. The light emitting diode chip according to claim 5, characterized in that: The thickness of the first ohmic contact layer (41) is 50-80 nm; The thickness of the electrode fixing layer (5) is 10 to 20 nm; The thickness of the first current spreading layer (61) is 3-4 μm.
7. The light emitting diode chip according to claim 1, characterized in that: The light-emitting diode chip further comprises a second current spreading layer (62) and a second ohmic contact layer (42) stacked in sequence; The second current spreading layer (62) and the second ohmic contact layer (42) are both P-type GaP layers; The second current spreading layer (62) is located on a side of the second semiconductor layer (13) facing away from the second electron blocking layer (22).
8. The light emitting diode chip according to claim 7, characterized in that: The thickness of the second current spreading layer is 1-2 μm; The thickness of the second ohmic contact layer is 50-200 nm.
9. A method for preparing a light emitting diode chip, characterized in that: For preparing the light emitting diode chip according to claim 1, the preparation method comprises: Preparing a first semiconductor layer (11), wherein the first semiconductor layer (11) is of a first conductivity type; A first electron blocking layer (21) is prepared on one side of the first semiconductor layer (11), wherein the first electron blocking layer (21) is Al x In 1-x P layer, 0.5≤x≤1; Preparing an active layer (12) on one side of the first electron blocking layer (21); A second electron blocking layer (22) is prepared on one side of the active layer (12), wherein the second electron blocking layer (22) is Al x In 1-x P layer, 0.5≤x≤1; A second semiconductor layer (13) is prepared on one side of the second electron blocking layer (22), and the second semiconductor layer (13) is of a second conductivity type, and the second conductivity type is different from the first conductivity type.
10. The preparation method according to claim 9, characterized in that: The first electron blocking layer (21) is prepared, comprising: The growth temperature is set to 700-720°C, the growth rate is set to 0.35-0.45 nm / s, and the growth thickness is set to 10-15 nm; The first semiconductor layer (11) is grown.