High-nickel positive electrode material and preparation method thereof, positive electrode plate, lithium ion battery and electric equipment

By using alkaline oxidant solution to wash and iron phosphate coated calcining on the nickel-rich NCM ternary layered positive electrode material, the residual alkali problem on the surface of nickel-rich NCM ternary layered positive electrode material is solved, and the stability and electrochemistry of the material are improved Performance, achieving high capacity and high rate performance.

CN119008883APending Publication Date: 2024-11-22JIANGXI JIANA ENERGY TECH CO LTD +3
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202411081752.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The presence of residual alkali compounds on the surface of nickel-rich NCM ternary layered cathode material leads to microcracks, Li+/Ni2+ mixed displacement, interface side reactions and lattice structure phase change during circulation, affecting the stability and electrochemical properties of the material.

Method used

An integrated treatment process is used to wash nickel-cobalt manganese oxide lithium and coat with iron phosphate to calcinate residual lithium and form a fast electronic conductive layer to inhibit interface side reactions and structural degradation.

Benefits of technology

The residual alkali content on the surface of the nickel-cobalt-manganese lithium cobalt-manganese oxide positive electrode material is significantly reduced, the structural stability and electrochemical performance of the material are improved, capacity and rate performance are enhanced, and the structural degradation and interface side reactions on the surface of the material are slowed down.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008883A_ABST
    Figure CN119008883A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion batteries, in particular to a high-nickel positive electrode material, a preparation method of the high-nickel positive electrode material, a positive electrode plate, a lithium ion battery and electric equipment. The high-nickel positive electrode material comprises a nickel cobalt lithium manganate positive electrode material and an iron phosphate coating layer coating the surface of the nickel cobalt lithium manganate positive electrode material; the molar weight of the nickel element in the nickel cobalt lithium manganate positive electrode material accounts for more than or equal to 80% of the total molar weight of other metal elements except lithium; the mass fraction of lithium carbonate in the nickel cobalt lithium manganate positive electrode material is 1t; 0.19 wt.%, and the mass fraction of lithium hydroxide is 1t; and 0.13 wt.%. The surface residual alkali content of the high-nickel positive electrode material is low, and the problems of overhigh surface alkalinity of the positive electrode material and side reaction with electrolyte are solved; moreover, the iron phosphate coating layer, as a protective layer, can stabilize the layered crystal structure of the nickel cobalt lithium manganate positive electrode material, effectively alleviates the surface structure degradation and interface side reaction of the material, and can form a rapid electron conducting layer to promote electron transfer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium-ion batteries, and in particular to a high-nickel positive electrode material and a preparation method thereof, a positive electrode sheet, a lithium-ion battery and electrical equipment. Background Art

[0002] Compared with many new energy materials such as LiFePO 4 、LiCoO 2 、LiNiO 2 、LiMnO 2 In comparison, LiNi x Mn y Co 1-x-y O 2 It has the advantages of high discharge capacity (>200mA·h / g), high energy density, low toxicity and low cost, making it a very potential positive electrode material for lithium-ion batteries.

[0003] In recent years, nickel-rich NCM ternary layered cathode materials have been highly sought after by researchers, and the method of increasing the nickel content is often used to obtain excellent reversible capacity, which has a very broad development prospect. With the increase of nickel content, the cobalt and manganese content will be reduced accordingly, which will greatly reduce the material cost and significantly improve the material specific capacity and energy density.

[0004] However, the surface of materials with nickel content above 80% is prone to generate residual alkali compounds LiOH / Li 2 CO 3 The surface side reactions induce a sharp increase in RLCs, which makes the nickel-rich NCM ternary layered cathode materials face the problems of microcracks, Li + / Ni 2+ There are problems such as interfacial side reactions and lattice structure phase change (degradation) during mixing, cycling, etc. Therefore, removing RLCs on the surface of nickel-rich NCM ternary layered cathode materials while taking into account their high specific capacity and high cycle stability has become one of the hot topics in this research field.

[0005] In addition, there are currently two strategies for removing RLCs on the surface of Ni-rich NCM ternary layered cathode materials: (1) surface coating, adding metal fluorides / oxides / phosphates that react with residual alkali compounds to isolate H in the air. 2 O and CO 2 On the other hand, surface coating modification can effectively inhibit the side reaction of interface, reduce the mixing of lithium and nickel, inhibit the phase change, and inhibit Li +However, single surface coating cannot completely remove the residual alkali insulating layer on the surface, reduce the surface impedance, and improve the electrochemical performance and increase the Li + The ability to embed / eject is limited. (2) Solution washing, directly removing soluble residual alkali compounds by solution washing, including deionized water washing, anhydrous ethanol washing, and solution washing. The solution washing process is simple, low-cost, and pollution-free. It can effectively wash and remove soluble RLCs on the surface of nickel-rich ternary positive electrode materials, significantly improving the cycle performance and crystal structure stability of electrode materials. However, the washing process is very likely to cause microcracks to expand, leading to aggravated cation mixing, structural instability, and erosion of interface side reactions during charging and discharging.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] The first purpose of the present invention is to provide a high-nickel positive electrode material, which has a low residual alkali content on the surface of the high-nickel positive electrode material, thereby solving the problems of excessive alkalinity on the surface of the positive electrode material and side reactions with the electrolyte; and the iron phosphate coating layer as a protective layer can stabilize the layered crystal structure of the nickel cobalt manganese oxide lithium positive electrode material, effectively slowing down the degradation of the material surface structure and interface side reactions, and at the same time can form a fast electronic conductive layer to promote electron transfer.

[0008] The second purpose of the present invention is to provide a method for preparing a high-nickel positive electrode material, which uses an integrated treatment process of washing, coating and calcining nickel cobalt manganese oxide with an alkaline oxidant solution. The process can solve the problems of incomplete removal of residual lithium in a single coating or single water washing process, aggravated cation mixing during the water washing process, and erosion of interface side reactions during charging and discharging, and form a fast electronic conductive layer to promote electron transfer.

[0009] The third object of the present invention is to provide a positive electrode plate, which has high capacity, good rate performance and excellent cycle performance.

[0010] A fourth object of the present invention is to provide a lithium ion battery having high capacity, good cycle performance and high rate performance.

[0011] A fifth object of the present invention is to provide an electrical device.

[0012] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0013] The present invention first provides a high-nickel positive electrode material, including a nickel-cobalt-manganese-oxide lithium positive electrode material and an iron phosphate coating layer coated on the surface of the nickel-cobalt-manganese-oxide lithium positive electrode material;

[0014] In the nickel-cobalt-manganese-oxide lithium positive electrode material, the molar amount of nickel element accounts for ≥80% of the total molar amount of other metal elements except lithium;

[0015] In the nickel-cobalt-manganese-oxide lithium positive electrode material, the mass fraction of lithium carbonate is less than 0.19 wt.%, and the mass fraction of lithium hydroxide is less than 0.13 wt.%.

[0016] Preferably, the chemical formula of the lithium nickel cobalt manganese oxide positive electrode material is LiNi x Co y Mn 1-x-y O 2 , where 0.8≤x≤0.96, 0.03≤y≤0.12, 1-xy>0.

[0017] Preferably, the mass of the iron phosphate coating layer accounts for 0.2-1.0 wt % of the mass of the lithium nickel cobalt manganese oxide positive electrode material.

[0018] The present invention further provides a method for preparing the high-nickel positive electrode material, comprising the following steps:

[0019] The lithium nickel cobalt manganese oxide is mixed with an alkaline oxidant solution, washed and then dried to obtain a washed material;

[0020] The washed material is mixed with iron phosphate and calcined to obtain the high-nickel positive electrode material;

[0021] Wherein, the percentage of the molar amount of nickel element in the lithium nickel cobalt manganese oxide to the total molar amount of other metal elements except lithium is ≥80%;

[0022] The oxidant in the alkaline oxidant solution includes H 2 O 2 NH 4 ) 2 S 2 O 8 、Na 2 S 2 O 8 , K 2 S 2 O 8 , NaClO and KMnO 4 At least one of .

[0023] Preferably, the pH of the alkaline oxidant solution is 7-12.

[0024] Preferably, the molar concentration of the oxidant in the alkaline oxidant solution is 0.1-2 mol / L.

[0025] Preferably, the alkaline compound in the alkaline oxidant solution includes at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate and sodium phosphate.

[0026] Preferably, the washing temperature is 20-40° C., and the washing time is 5-60 min.

[0027] Preferably, stirring is continued during the washing process.

[0028] Preferably, the drying method comprises vacuum drying.

[0029] Preferably, the mass of the iron phosphate accounts for 0.2-1.0 wt % of the mass of the washed material.

[0030] Preferably, the calcination temperature is 600-800° C., and the calcination holding time is 8-24 hours.

[0031] Preferably, the calcination is performed under an oxygen-containing atmosphere.

[0032] Preferably, the method of mixing the washed material with ferric phosphate comprises mixing and grinding.

[0033] Preferably, the method for preparing the nickel cobalt manganese oxide comprises: mixing a nickel cobalt manganese hydroxide precursor with a lithium source and then sintering the mixture.

[0034] Preferably, the nickel-cobalt-manganese hydroxide precursor is washed with water and dried.

[0035] Preferably, the median particle size of the nickel-cobalt-manganese hydroxide precursor is 8 to 13 μm.

[0036] Preferably, the molar ratio of the nickel-cobalt-manganese hydroxide precursor to the lithium element in the lithium source is 1:1.01-1.2.

[0037] Preferably, the sintering is performed in an oxygen-containing atmosphere.

[0038] Preferably, the sintering comprises: firstly keeping the temperature at 400-500° C. for 4-8 hours, and then keeping the temperature at 700-800° C. for 18-24 hours.

[0039] The present invention further provides a positive electrode plate, comprising the high-nickel positive electrode material, or the high-nickel positive electrode material prepared by the method for preparing the high-nickel positive electrode material.

[0040] The present invention further provides a lithium-ion battery, comprising the positive electrode plate.

[0041] The present invention also provides an electrical device, comprising the lithium-ion battery.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] (1) The high-nickel positive electrode material provided by the present invention has low residual alkali content, low degree of lithium-nickel mixing, high capacity and rate performance, stable structure, and can inhibit phase change and electrolyte interface side reactions; and the iron phosphate coating layer can serve as a protective layer to stabilize the layered crystal structure of the nickel-cobalt-manganese-oxide lithium positive electrode material, effectively slowing down the material surface structure degradation and interface side reactions, and at the same time can form a fast electronic conductive layer to promote electron transfer.

[0044] (2) The preparation method of the high-nickel positive electrode material provided by the present invention adopts an integrated treatment process of washing the nickel cobalt manganese oxide with an alkaline oxidant solution and coating and calcining the lithium nickel manganese oxide to modify and optimize the surface of the positive electrode material, thereby improving the structural stability and electrochemical performance of the material. The positive electrode material has the advantages of low degree of lithium-nickel mixing, high capacity and rate performance, stable material structure, inhibition of phase change and electrolyte interface side reactions, etc., and the iron phosphate coating layer can form a fast electronic conductive layer to promote electron transfer.

[0045] (3) The preparation method of the high nickel positive electrode material provided by the present invention can effectively remove the residual lithium on the surface of the nickel cobalt manganese oxide positive electrode material and inhibit the Li + and H in water + Make an exchange. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0047] Figure 1 This is a SEM image of the high-nickel ternary positive electrode material obtained in step (1) of Example 2 provided by the present invention;

[0048] Figure 2 This is a SEM image of the washed material obtained in step (2) of Example 2 provided by the present invention. DETAILED DESCRIPTION

[0049] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0050] If there is no special explanation, in the present invention, "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "the first", "the second", "the third", "the fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0051] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0052] If there is no special explanation, in the present invention, "one or more" or "at least one" refers to any one, any two or more of the listed items. Among them, "several" refers to any two or more of the listed items.

[0053] In a first aspect, the present invention provides a high-nickel positive electrode material, comprising a nickel-cobalt-manganese-oxide lithium positive electrode material and an iron phosphate coating layer coated on the surface of the nickel-cobalt-manganese-oxide lithium positive electrode material.

[0054] In the nickel cobalt manganese oxide positive electrode material, the percentage of the molar amount of nickel element to the total molar amount of other metal elements except lithium is ≥80%, including but not limited to any point value of 80%, 83%, 85%, 88%, 90%, 92%, 93%, 95%, 96% or any range value between two of them. That is, the nickel cobalt manganese oxide positive electrode material is a high nickel material.

[0055] In the nickel-cobalt-manganese-oxide lithium positive electrode material, the mass fraction of lithium carbonate is less than 0.19wt.%, including but not limited to any point value of 0.187wt.%, 0.18wt.%, 0.17wt.%, 0.16wt.%, 0.15wt.%, 0.13wt.%, 0.12wt.%, 0.11wt.%, 0.1wt.% or any range value between two of them; the mass fraction of lithium hydroxide is less than 0.13wt.%, including but not limited to any point value of 0.12wt.%, 0.11wt.%, 0.10wt.%, 0.09wt.%, 0.08wt.%, 0.06wt.% or any range value between two of them. The residual alkali content in the nickel-cobalt-manganese-oxide lithium positive electrode material is low.

[0056] The high-nickel positive electrode material has low residual alkali content, low degree of lithium-nickel mixing, high capacity and rate performance, stable structure, and can inhibit phase change and electrolyte interface side reactions, solving the problems of particle cracks in high-nickel ternary positive electrode materials, interface side reactions between the positive electrode and the electrolyte, and poor cycle performance and rate performance.

[0057] Among them, the iron phosphate coating layer as a protective layer can stabilize the layered crystal structure of the lithium nickel cobalt manganese oxide positive electrode material, effectively slow down the surface structure degradation and interface side reactions of the material, and at the same time form a fast electronic conductive layer to promote electron transfer.

[0058] In some specific embodiments, the chemical formula of the lithium nickel cobalt manganese oxide positive electrode material is LiNi x Co y Mn 1-x-y O 2 , where 0.8≤x≤0.96, 0.03≤y≤0.12, 1-xy>0.

[0059] Wherein, x includes but is not limited to any point value of 0.8, 0.83, 0.85, 0.88, 0.9, 0.92, 0.94, 0.95, 0.96 or any range value between two thereof. y includes but is not limited to any point value of 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12 or any range value between two thereof.

[0060] In some specific embodiments, the mass of the iron phosphate coating layer accounts for 0.2-1.0wt% of the mass of the nickel cobalt manganese oxide lithium positive electrode material, including but not limited to any one of 0.2wt.%, 0.3wt.%, 0.4wt.%, 0.5wt.%, 0.6wt.%, 0.7wt.%, 0.8wt.%, 0.9wt.%, 1.0wt.% or a range between any two of them.

[0061] In a second aspect, the present invention provides a method for preparing the high-nickel positive electrode material, comprising the following steps:

[0062] The lithium nickel cobalt manganese oxide is mixed with an alkaline oxidant solution, washed and then dried to obtain a washed material; the washed material is mixed with iron phosphate and calcined, and the high-nickel positive electrode material is obtained after cooling.

[0063] Wherein, the percentage of the molar amount of nickel element in the lithium nickel cobalt manganese oxide to the total molar amount of other metal elements except lithium is ≥80%, including but not limited to any point value of 80%, 83%, 85%, 88%, 90%, 92%, 93%, 95%, 96% or the range value between any two of them.

[0064] The oxidant in the alkaline oxidant solution includes H 2 O 2 NH 4 ) 2 S 2 O 8 、Na 2 S 2 O 8 , K 2 S 2 O 8 , NaClO and KMnO 4 When lithium nickel cobalt manganese oxide is washed with water, a substitution reaction of Li and H will occur, resulting in the dissolution of Li inside the material and reduced electrochemical performance. In order to solve this problem, the present invention uses an alkaline oxidant solution for washing. During the washing process, the alkaline environment will inhibit the substitution reaction of Li and H, reduce the dissolution of Li, and the oxidant can increase Ni 3+ The number of them increases, thereby improving the electrochemical performance.

[0065] The preparation method of the high-nickel positive electrode material provided by the present invention adopts an integrated treatment process of washing the nickel cobalt manganese oxide with an alkaline oxidant solution and coating and calcining, and the surface of the positive electrode material is modified and optimized, thereby improving the structural stability and electrochemical performance of the material. The positive electrode material has the advantages of low lithium-nickel mixing degree, high capacity and rate performance, stable material structure, inhibition of phase change and electrolyte interface side reaction, etc., and solves the problems of incomplete removal of residual lithium in a single coating or single water washing process, aggravation of cation mixing in the water washing process, and erosion of interface side reactions during charge and discharge.

[0066] In addition, the iron phosphate coating layer as a protective layer can stabilize the layered crystal structure of the lithium nickel cobalt manganese oxide positive electrode material, effectively slow down the surface structure degradation and interface side reactions of the material, and at the same time form a fast electronic conductive layer to promote electron transfer.

[0067] In addition, the alkaline oxidant solution used in the present invention can effectively remove residual lithium on the surface of the nickel cobalt manganese oxide positive electrode material and inhibit the Li + and H in water + Exchange is carried out to reduce Li dissolution and solve the problems of excessive alkalinity on the surface of the positive electrode material and side reactions with the electrolyte.

[0068] In some specific embodiments, the pH of the alkaline oxidant solution is 7-12, including but not limited to any one of 7, 8, 9, 10, 11, and 12, or a range between any two of them.

[0069] In some specific embodiments, the molar concentration of the oxidant in the alkaline oxidant solution is 0.1-2 mol / L; including but not limited to any point value of 0.1 mol / L, 0.3 mol / L, 0.5 mol / L, 0.8 mol / L, 1 mol / L, 1.3 mol / L, 1.5 mol / L, 1.8 mol / L, 2 mol / L or any range value between two of them. If the molar concentration of the oxidant is too large, it will change the morphological characteristics of the positive electrode material, increase the mixing of the Li-Ni material, and reduce the electrochemical performance. The present invention controls the molar concentration of the oxidant within the above range to ensure the electrochemical performance of the high nickel positive electrode material.

[0070] In some specific embodiments, the alkaline compound in the alkaline oxidant solution includes at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate and sodium phosphate. It is understood that the solution of the alkaline compound dissolved in water is alkaline.

[0071] In some specific embodiments, the washing temperature is 20-40°C, including but not limited to any point value of 20°C, 23°C, 25°C, 28°C, 30°C, 32°C, 35°C, 38°C, 40°C or any range value between two thereof; the washing time is 5-60min, including but not limited to any point value of 5min, 10min, 20min, 30min, 40min, 50min, 60min or any range value between two thereof. The lattice lithium dissolution of the material increases with the increase of the water washing temperature, and excessively high washing temperature will lead to a decrease in the discharge specific capacity of the material. The present invention can ensure the capacity of the high nickel positive electrode material and reduce energy consumption by controlling the washing temperature within the above range.

[0072] In some specific embodiments, stirring is continued during the washing process.

[0073] In some specific embodiments, during the washing process, the lithium nickel cobalt manganese oxide is immersed in an alkaline oxidant solution.

[0074] In some specific embodiments, the drying method comprises vacuum drying.

[0075] In some specific embodiments, the mass of the iron phosphate accounts for a percentage of the mass of the washed material of 0.2-1.0 wt%, including but not limited to any point value of 0.2 wt.%, 0.3 wt.%, 0.4 wt.%, 0.5 wt.%, 0.6 wt.%, 0.7 wt.%, 0.8 wt.%, 0.9 wt.%, 1.0 wt.%, or a range value between any two of them.

[0076] In some specific embodiments, the calcination temperature is 600-800°C, including but not limited to any one of 600°C, 650°C, 700°C, 750°C, and 800°C, or a range between any two of them; the calcination holding time is 8-24h, including but not limited to any one of 8h, 10h, 12h, 15h, 18h, 20h, 22h, and 24h, or a range between any two of them.

[0077] In some specific embodiments, the heating rate of calcination is 1 to 10°C / min, including but not limited to any one of 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 8°C / min, and 10°C / min, or a range between any two of them.

[0078] In some specific embodiments, the calcination is performed under an oxygen-containing atmosphere.

[0079] In some specific embodiments, the oxygen-containing atmosphere includes an oxygen atmosphere and / or an air atmosphere.

[0080] In some specific embodiments, the method of mixing the washed material with ferric phosphate comprises mixing and grinding.

[0081] In some specific embodiments, the method for preparing the nickel cobalt manganese oxide includes: mixing a nickel cobalt manganese hydroxide precursor with a lithium source and then sintering the mixture.

[0082] In some specific embodiments, the nickel-cobalt-manganese hydroxide precursor is washed with water and dried.

[0083] In some specific embodiments, the median particle size of the nickel cobalt manganese hydroxide precursor is 8 to 13 μm, including but not limited to any point value of 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, or a range value between any two of them.

[0084] In some specific embodiments, the molar ratio of the nickel-cobalt-manganese hydroxide precursor to the lithium element in the lithium source is 1:1.01-1.2, including but not limited to any point value of 1:1.01, 1:1.03, 1:1.05, 1:1.08, 1:1, 1:1.5, 1:1.2 or any range value between two of them. Excessive lithium element can ensure that it is fully integrated into the crystal and avoid lithium loss during the sintering process leading to insufficient lithium element usage.

[0085] In some specific embodiments, the sintering is performed in an oxygen atmosphere and / or an air atmosphere.

[0086] In some specific embodiments, the sintering includes: first keeping warm at 400-500°C (including but not limited to any point value of 400°C, 420°C, 430°C, 450°C, 460°C, 480°C, 500°C or any range value between two of them) for 4-8h (including but not limited to any point value of 4h, 5h, 6h, 7h, 8h or any range value between two of them), and then keeping warm at 700-800°C (including but not limited to any point value of 700°C, 730°C, 750°C, 780°C, 800°C or any range value between two of them) for 18-24h (including but not limited to any point value of 18h, 19h, 20h, 21h, 22h, 24h or any range value between two of them).

[0087] In some specific embodiments, the sintering heating rate is 1 to 10°C / min, including but not limited to any one of 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 8°C / min, and 10°C / min, or a range between any two of them.

[0088] In some specific embodiments, the lithium source includes lithium hydroxide.

[0089] In a third aspect, the present invention provides a positive electrode plate, comprising the high-nickel positive electrode material, or the high-nickel positive electrode material prepared by the method for preparing the high-nickel positive electrode material.

[0090] The positive electrode plate has high capacity, good rate performance and excellent cycle performance.

[0091] In some specific embodiments, the positive electrode plate includes a positive electrode active layer disposed on a current collector, and the positive electrode active layer includes the above-mentioned high-nickel positive electrode material.

[0092] Optionally, the positive electrode plate further includes a conductive agent and / or a binder, which is not limited in the present invention.

[0093] In a fourth aspect, the present invention provides a lithium-ion battery, comprising the positive electrode plate.

[0094] The lithium-ion battery has high capacity, good cycle performance and high rate performance.

[0095] Optionally, the lithium-ion battery further includes a negative electrode plate, a separator and an electrolyte, which is not limited in the present invention.

[0096] In a fifth aspect, the present invention provides an electrical device comprising the lithium-ion battery.

[0097] It is understandable that the electrical equipment includes any equipment or device including the above-mentioned lithium-ion battery, such as electric vehicles, electric motorcycles, electric bicycles, electric tools, starting power supplies, energy storage devices, electronic products, office equipment, etc., and the present invention is not limited to this.

[0098] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0099] Example 1

[0100] The method for preparing the high nickel positive electrode material provided in this embodiment comprises the following steps:

[0101] (1) The high nickel ternary precursor Ni with a median particle size of 10 μm 0.80 Co 0.10 Mn 0.10 (OH) 2 After washing and drying, the mixture was mixed evenly with lithium hydroxide at a molar ratio of 1:1.04, and then heated to 450°C at a rate of 2°C / min in an oxygen atmosphere, sintered for 4 hours, and then heated to 750°C at a rate of 2°C / min, sintered for 18 hours, and the furnace temperature was naturally cooled to take a sample out of the furnace, and passed through a 300-mesh sieve to obtain a high-nickel ternary positive electrode material (i.e., a nickel-cobalt-manganese-oxide lithium positive electrode material, whose chemical formula is LiNi 0.80 Co 0.10 Mn 0.10 O 2 ).

[0102] (2) At 25°C, add 30 g of the high-nickel ternary positive electrode material obtained in step (1) to 150 ml of an alkaline oxidant solution, and stir at 400 rpm for 5 min. The alkaline oxidant solution is a mixture of sodium carbonate and H 2 O 2Mixed solution (solvent is water), pH = 9, where H 2 O 2 The molar concentration is 2 mol / l. The wet material is then filtered and dried under vacuum at 120°C for 5 h to obtain a washed material.

[0103] (3) The washed material was mixed with FePO4 (0.2 wt% of the washed material) 4 The mixture was mixed and ground to make it evenly dispersed, and then the temperature was raised to 700°C at a rate of 2°C / min in an oxygen atmosphere for calcination. After keeping the temperature for 8 hours, a high-nickel positive electrode material modified by coating with iron phosphate was obtained.

[0104] Example 2

[0105] The method for preparing the high nickel positive electrode material provided in this embodiment comprises the following steps:

[0106] (1) The high nickel ternary precursor Ni with a median particle size of 8 μm 0.83 Co 0.11 Mn 0.06 (OH) 2 After washing and drying, the mixture was mixed evenly with lithium hydroxide at a molar ratio of 1:1.08, and then heated to 450°C at a rate of 2°C / min in an oxygen atmosphere, sintered for 4 hours, and then heated to 750°C at a rate of 2°C / min, sintered for 18 hours, and the furnace temperature was cooled naturally to take a sample out of the furnace, and passed through a 300-mesh sieve to obtain a high-nickel ternary positive electrode material (chemical formula LiNi 0.83 Co 0.11 Mn 0.06 O 2 ).

[0107] (2) At 25°C, add 30 g of the high-nickel ternary positive electrode material obtained in step (1) to the alkaline oxidant solution, and stir at a speed of 300 rpm for 30 min. The alkaline oxidant solution is a mixture of sodium hydroxide and H 2 O 2 Mixed solution (solvent is water), pH = 11, where H 2 O 2 The molar concentration is 2 mol / l. The wet material is then filtered and dried under vacuum at 120°C for 5 h to obtain a washed material.

[0108] (3) The washed material was mixed with FePO4 (0.8 wt %) 4 The mixture was mixed and ground to make it evenly dispersed, and then the temperature was raised to 650°C at a rate of 2°C / min in an oxygen atmosphere for calcination. After keeping the temperature for 8 hours, a high-nickel positive electrode material modified by coating with iron phosphate was obtained.

[0109] Example 3

[0110] The method for preparing the high nickel positive electrode material provided in this embodiment comprises the following steps:

[0111] (1) The high nickel ternary precursor Ni with a median particle size of 13 μm 0.9 Co 0.05 Mn 0.05 (OH) 2 After washing and drying, the mixture was mixed evenly with lithium hydroxide at a molar ratio of 1:1.05, and then heated to 450°C at a rate of 2°C / min in an oxygen atmosphere, sintered for 8 hours, and then heated to 750°C at a rate of 2°C / min, sintered for 24 hours, and the furnace temperature was cooled naturally to take a sample out of the furnace, and passed through a 300-mesh sieve to obtain a high-nickel ternary positive electrode material (chemical formula LiNi 0.9 Co 0.05 Mn 0.05 O 2 ).

[0112] (2) Add 30 g of the high-nickel ternary positive electrode material obtained in step (1) to 150 ml of an alkaline oxidant solution, and continue stirring at 300 rpm for 5 min, wherein the washing temperature is 40° C. The alkaline oxidant solution is a mixture of sodium phosphate and H 2 O 2 Mixed solution (solvent is water), pH = 10, where H 2 O 2 The molar concentration is 2 mol / l. The wet material is then filtered and dried under vacuum at 120°C for 5 h to obtain a washed material.

[0113] (3) The washed material was mixed with FePO4 (0.4 wt%) 4 The mixture was mixed and ground to make it evenly dispersed, and then the temperature was raised to 750°C at a rate of 2°C / min in an oxygen atmosphere for calcination. After keeping the temperature for 8 hours, a high-nickel positive electrode material modified by coating with iron phosphate was obtained.

[0114] Example 4

[0115] The preparation method of the high nickel positive electrode material provided in this embodiment is basically the same as that in embodiment 1, except that in step (2), the alkaline oxidant solution is replaced by sodium hydroxide and (NH 4 ) 2 S 2 O 8 The mixed solution, pH = 10, where (NH 4 ) 2 S 2 O 8 The molar concentration is 1 mol / l.

[0116] Example 5

[0117] The preparation method of the high nickel positive electrode material provided in this embodiment is basically the same as that in embodiment 1, except that in step (2), the alkaline oxidant solution is replaced by a mixed solution of sodium hydroxide and NaClO, pH = 10, wherein the molar concentration of NaClO is 1.5 mol / l.

[0118] Example 6

[0119] The preparation method of the high nickel positive electrode material provided in this embodiment is basically the same as that in embodiment 1, except that in step (2), the alkaline oxidant solution is replaced by sodium hydroxide and KMnO 4 Mixed solution, pH = 8.5, in which KMnO 4 The molar concentration is 0.5 mol / l.

[0120] Example 7

[0121] The preparation method of the high nickel positive electrode material provided in this embodiment is basically the same as that in embodiment 1, except that in step (1), the sintering process is replaced by: first heating to 500°C at a rate of 3°C / min, sintering for 6h, then heating to 800°C at a rate of 3°C / min, and sintering for 20h.

[0122] Comparative Example 1

[0123] The preparation method of the high-nickel positive electrode material provided in this comparative example is basically the same as that in Example 1, except that in step (2), the alkaline oxidant solution is replaced with an equal volume of water.

[0124] Comparative Example 2

[0125] The preparation method of the high-nickel positive electrode material provided in this comparative example is basically the same as that of Example 1, except that in step (2), the alkaline oxidant solution is replaced with an equal volume of sodium hydroxide solution with a pH of 9.

[0126] Comparative Example 3

[0127] The preparation method of the high nickel positive electrode material provided in this comparative example is basically the same as that in Example 1, except that in step (2), the alkaline oxidant solution is replaced by an equal volume of H 2 O 2 Solution.

[0128] Comparative Example 4

[0129] The preparation method of the high nickel positive electrode material provided in this comparative example is basically the same as that in Example 1, except that FePO is not added in step (3). 4 .

[0130] Among them, the lithium carbonate content (mass fraction), lithium hydroxide content (mass fraction) in the high nickel ternary positive electrode material obtained in step (1) (i.e. before washing) and the washed material obtained in step (2) (i.e. after washing), and the specific surface area of ​​the material are shown in Table 1.

[0131] Table 1 Specific surface area and residual lithium content of materials before and after washing

[0132]

[0133]

[0134] It can be seen from Table 1 that the sodium hydroxide content and sodium carbonate content of the high-nickel ternary positive electrode material of each embodiment are significantly reduced after washing with an alkaline oxidant solution, and the specific surface area is appropriately increased (after washing, impurities on the particle surface are reduced and the specific surface area is increased). Appropriately increasing the specific surface area is beneficial to subsequent calcination and improving the electrochemical performance of the high-nickel positive electrode material.

[0135] Further, the SEM image of the high nickel ternary positive electrode material obtained in step (1) of Example 2 is shown in Figure 1 The SEM image of the washed material obtained in step (2) of Example 2 is shown in Figure 2 ,pass Figure 1 and Figure 2 It can be seen that the surface of the washed material is clean, with no obvious residual alkali residue, and no obvious gaps appear in the primary particle accumulation.

[0136] Experimental example

[0137] The high nickel positive electrode materials prepared in the above embodiments and comparative examples were used as positive electrode active materials to make positive electrode sheets, which were assembled into button cells and subjected to electrochemical performance tests. The test results are shown in Table 2.

[0138] The steps of preparing the positive electrode sheet are as follows: dissolving high nickel positive electrode material, conductive carbon (Super P) and polyvinylidene fluoride (PVDF) in N-methylpyrrolidone (NMP) at a weight ratio of 8:1:1, stirring thoroughly to obtain positive electrode slurry; using a film applicator to evenly coat the positive electrode slurry on aluminum foil, vacuum drying at 120°C for 10 hours to obtain a positive electrode sheet, and using a punching machine to cut the positive electrode sheet into a 14mm circular sheet. The steps of assembling the button battery are as follows: assembling in a glove box, the argon content in the glove box is 99.999%, the actual oxygen content is <0.01ppm, and the moisture content is <0.01ppm; assembling the battery in the order of negative electrode shell, positive electrode sheet, diaphragm, electrolyte, negative electrode sheet, gasket, spring and positive electrode shell; wherein the electrolyte is prepared by lithium hexafluorophosphate and an organic solvent, the organic solvent is diethyl carbonate, and the negative electrode sheet is a metal lithium sheet.

[0139] The steps of the electrochemical performance test method are as follows: in a constant temperature test room at 25°C, place the button lithium-ion battery for 10 hours, then charge it to 4.3V at a constant current rate of 0.1C, discharge it to 3.0V at a constant current, and cycle it three times for activation. The first coulomb efficiency can be obtained through the first charge and discharge capacity; then perform a constant current charge and discharge test between 3.0V and 4.3V at a rate of 1C, and cycle it 100 times to obtain the capacity retention rate of the battery after 100 cycles, which is used to measure the battery's cycle stability.

[0140] Table 2 Electrochemical performance test results of the battery

[0141]

[0142] It can be seen from Table 2 that the high-nickel positive electrode materials prepared in various embodiments have high capacity and good cycle performance.

[0143] However, the capacities of Comparative Examples 1 to 4 are reduced or the cycle performance is degraded.

[0144] Among them, although the washing methods of Comparative Examples 1 to 3 can reduce the amount of residual alkali on the surface of the material to a certain extent, the capacity or cycle performance is significantly reduced. This shows that the use of alkaline oxidant solution for washing in the present invention can inhibit the replacement reaction of Li and H, reduce the dissolution of Li, and increase Ni 3+ The number of increases, thereby improving the electrochemical performance of the high-nickel positive electrode material. In summary, the present invention provides a new surface modification treatment method for high-nickel ternary positive electrode materials, which adopts the method of washing with alkaline oxidant solution to significantly reduce the alkalinity of the surface of the high-nickel positive electrode material, and inhibits the decomposition of the electrolyte on the surface of the high-nickel ternary positive electrode material and the structural degradation of the material surface through the coating modification of the surface iron phosphate, thereby improving the reversible capacity of the high-nickel ternary positive electrode material and significantly improving its cycle stability.

[0145] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A high nickel positive electrode material, characterized in that: It includes a nickel cobalt lithium manganese oxide positive electrode material and an iron phosphate coating layer coated on the surface of the nickel cobalt lithium manganese oxide positive electrode material; In the nickel-cobalt-manganese-oxide lithium positive electrode material, the percentage of the molar amount of nickel element to the total molar amount of other metal elements except lithium is ≥80%; In the nickel-cobalt-manganese-oxide lithium positive electrode material, the mass fraction of lithium carbonate is less than 0.19 wt.%, and the mass fraction of lithium hydroxide is less than 0.13 wt.%.

2. The high nickel positive electrode material according to claim 1, characterized in that: The chemical formula of the lithium nickel cobalt manganese oxide positive electrode material is LiNi x Co y Mn 1-x-y O2, where 0.8≤x≤0.96, 0.03≤y≤0.12, 1-xy>0.

3. The high nickel positive electrode material according to claim 1, characterized in that: The mass of the iron phosphate coating layer accounts for 0.2-1.0 wt % of the mass of the nickel cobalt manganese oxide lithium positive electrode material.

4. The method for preparing a high-nickel positive electrode material according to any one of claims 1 to 3, characterized in that: The steps include: The lithium nickel cobalt manganese oxide is mixed with an alkaline oxidant solution, washed and then dried to obtain a washed material; The washed material is mixed with iron phosphate and calcined to obtain the high-nickel positive electrode material; Wherein, the percentage of the molar amount of nickel element in the lithium nickel cobalt manganese oxide to the total molar amount of other metal elements except lithium is ≥80%; The oxidant in the alkaline oxidant solution includes at least one of H2O2, (NH4)2S2O8, Na2S2O8, K2S2O8, NaClO and KMnO4.

5. The method for preparing a high-nickel positive electrode material according to claim 4, characterized in that: At least one of the following conditions is met: (1) The pH of the alkaline oxidant solution is 7 to 12; (2) the molar concentration of the oxidant in the alkaline oxidant solution is 0.1 to 2 mol / L; (3) the alkaline compound in the alkaline oxidant solution includes at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate and sodium phosphate; (4) The washing temperature is 20 to 40° C. and the washing time is 5 to 60 minutes; (5) stirring continuously during the washing process; (6) The drying method includes vacuum drying.

6. The method for preparing a high-nickel positive electrode material according to claim 4, characterized in that: At least one of the following conditions is met: (1) The mass of the iron phosphate accounts for 0.2-1.0 wt% of the mass of the washed material; (2) The calcination temperature is 600 to 800° C., and the calcination holding time is 8 to 24 hours; (3) the calcination is carried out in an oxygen-containing atmosphere; (4) The method of mixing the washed material with iron phosphate includes mixing and grinding.

7. The method for preparing a high-nickel positive electrode material according to claim 4, characterized in that: The preparation method of the nickel cobalt manganese oxide comprises: mixing a nickel cobalt manganese hydroxide precursor with a lithium source and then sintering the mixture; Preferably, the nickel-cobalt-manganese hydroxide precursor is washed and dried; Preferably, the median particle size of the nickel-cobalt-manganese hydroxide precursor is 8 to 13 μm; Preferably, the molar ratio of the nickel-cobalt-manganese hydroxide precursor to the lithium element in the lithium source is 1:1.01-1.2; Preferably, the sintering is carried out in an oxygen-containing atmosphere; Preferably, the sintering comprises: firstly keeping the temperature at 400-500° C. for 4-8 hours, and then keeping the temperature at 700-800° C. for 18-24 hours.

8. A positive electrode sheet, characterized in that: It comprises the high-nickel positive electrode material as claimed in any one of claims 1 to 3, or the high-nickel positive electrode material prepared by the preparation method of the high-nickel positive electrode material as claimed in any one of claims 4 to 7.

9. A lithium ion battery, characterized in that: Comprising the positive electrode plate as claimed in claim 8.

10. An electrical device, characterized in that: Comprising the lithium ion battery as claimed in claim 9.

Citation Information

Cited By

  • Nickel-rich layered oxide positive electrode coated with mixed coating and application of nickel-rich layered oxide positive electrode

    CN119400846A

  • A mixed coating coated nickel-rich layered oxide positive electrode and its application

    CN119400846B

  • Positive electrode material and surface coating method thereof

    CN120581554A

  • A positive electrode material and a surface coating method thereof

    CN120581554B

  • High-energy-density rate type solid-liquid mixed lithium ion battery and preparation method thereof