Additive material for negative electrode of lithium ion battery as well as preparation method and application of additive material

By using heterogeneous isomers constructed by Li3AlF6 and AlPO4 in the negative electrode material of lithium-ion battery and coating Li3PO4, an ion-electron hybrid conductor is formed, which solves the problem of safety hazards and insufficient desolvation ability of lithium-ion batteries at high magnifications. Significantly improves battery rate performance and safety.

CN119008951APending Publication Date: 2024-11-22LIONGO (CHANGZHOU) NEW ENERGY CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411112509.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing lithium-ion battery negative electrode materials have safety hazards under high charging rate, resulting in lithium dendrites generation and thermal runaway. The existing coating methods cannot effectively improve the desolvation ability of lithium ions and battery magnification performance.

Method used

Using heterogeneous isomers constructed from Li3AlF6 and AlPO4 as the core, combined with Li3PO4 cladding layer, a new ion-electron hybrid conductor is formed. Li3PO4 is coated through microwave heterogeneous precipitation to improve the desolvation of lithium ions and Transmission capability.

Benefits of technology

Significantly reduce polarization, improve battery rate performance, enhance battery safety and stability, inhibit lithium dendrites generation, and improve battery circulation performance and first-term effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004992742890000221
    Figure BDA0004992742890000221
  • Figure BDA0004992742890000231
    Figure BDA0004992742890000231
  • Figure HDA0004992742990000011
    Figure HDA0004992742990000011
Patent Text Reader

Abstract

The invention provides an additive material for a negative electrode of a lithium ion battery, which is characterized by comprising an inner core and a coating layer, the inner core is a heterogeneous isomorphic body constructed by Li3AlF6 and AlPO4, and the coating layer is Li3PO4. According to the invention, two electronic insulating materials of Li3AlF6 and AlPO4 are combined to prepare a heterogeneous isomorphic material, the material generates electron conductivity, so that a new ion-electron mixed conductor is obtained, and a layer of Li3PO4 is coated on the surface of the mixed conductor by using a microwave heterogeneous precipitation method, so that the composite material is obtained. When the mixed conductor material is applied to negative electrode coating, the migration kinetics of the lithium ions on the surface of a negative electrode can be accelerated, the polarization can be remarkably reduced, the rate capability of a battery can be improved, the generation of lithium dendrites can be inhibited, and the safety and the stability of the battery can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to an additive material for a negative electrode of a lithium ion battery, a preparation method thereof and an application thereof. Background Art

[0002] Lithium-ion batteries have many advantages such as high energy density, good cycle performance, long service life, and low self-discharge. They occupy a large application market in the fields of 3C electronics, power batteries, and energy storage, and have broad application prospects. As an important component of lithium-ion batteries, negative electrode materials are one of the main shortcomings that limit battery energy density, rate, and other performance. As one of the most commonly used negative electrode materials for lithium batteries, graphite has some safety issues. For example, when the battery is in a high charging rate working state, due to the slow lithium ion transfer on the graphite surface, the battery polarization increases, reaching the lithium ion deposition overpotential, and lithium ions are precipitated on the surface of graphite particles in the form of lithium dendrites, resulting in a reduction in active lithium. Lithium dendrites continue to grow, puncture the diaphragm, induce battery short circuit, generate a lot of heat, and cause thermal runaway, which deteriorates the safety performance of the battery. Effectively solving the safety hazards on the negative electrode side and avoiding the phenomenon of thermal runaway of the battery have become problems that need to be solved in the industry.

[0003] At present, existing technical solutions usually improve the rate performance of graphite through methods such as material modification and negative electrode coating. The method of modifying the morphology and structure of graphite is likely to cause damage to the graphite structure and increase the specific surface area in contact with the electrolyte. The formation of a solid electrolyte interface film will consume more active lithium, reduce the battery capacity and initial efficiency, and the desolvation ability of lithium ions has not been improved.

[0004] Therefore, coating the negative electrode material by coating can effectively improve the rate performance of graphite. However, coating with electronically conductive materials cannot improve the transport capacity of lithium ions, easily causes polarization, and cannot improve the desolvation capacity of lithium ions; and by coating with double coating layers of electronically conductive materials and ion conductive materials, due to the stratification of the coating layers, it is actually difficult to form a continuous electron and ion transmission channel, and it is also impossible to improve the desolvation capacity of lithium ions.

[0005] Therefore, it becomes a problem to be solved to provide a negative electrode additive material which has both ionic conductivity and electronic conductivity and can promote the desolvation of lithium ions, thereby improving the material performance of the negative electrode after coating. Summary of the invention

[0006] In view of this, the technical problem to be solved by the present invention is to provide an additive material for lithium ion battery negative electrode and a preparation method and application thereof. The additive material for lithium ion battery negative electrode provided by the present invention has both ionic conductivity characteristics and electronic conductivity characteristics, and can promote the desolvation of lithium ions, thereby improving the material performance of the negative electrode after coating.

[0007] The invention provides an additive material for a negative electrode of a lithium ion battery, comprising a core and a coating layer, wherein the core is a heterogeneous isomorph constructed of Li3AlF6 and AlPO4, and the coating layer is Li3PO4.

[0008] Preferably, the preparation method of the heterogeneous isomorph constructed by Li3AlF6 and AlPO4 comprises the following steps:

[0009] Under protective atmosphere conditions, Li3AlF6 and AlPO4 are mixed, subjected to high-energy ball milling, and then dried and calcined to obtain a heterogeneous isomorph constructed of Li3AlF6 and AlPO4.

[0010] Preferably, the molar ratio of Li3AlF6 to AlPO4 is 1:(2-3);

[0011] The protective atmosphere condition is argon;

[0012] During the high-energy ball milling, the mass ratio of the amount of the grinding balls added to the total amount of Li3AlF6 and AlPO4 is (5-10):1, the mass ratio of the mass of the grinding solvent to the total amount of Li3AlF6 and AlPO4 is (3-4):1, and the grinding solvent is selected from stearic acid;

[0013] The temperature of the high-energy ball mill is 25-35°C, and the high-energy ball mill is stopped after 60 minutes, and cooled for 10 minutes. The high-energy ball milling time is 30-40 hours, and the speed of the high-energy ball mill is 1600-1800 rpm;

[0014] The drying temperature is 100-200°C;

[0015] The calcination atmosphere is argon atmosphere, the calcination temperature is 400-500° C., and the calcination time is 4-6 hours.

[0016] Preferably, the particle size of the heterogeneous isomorph constructed of Li3AlF6 and AlPO4 is 100±20 nm, and the thickness of the coating layer is 5 to 10 nm.

[0017] The present invention also provides a method for preparing the above-mentioned additive material for lithium ion battery negative electrode, comprising the following steps:

[0018] A) mixing a heterogeneous isomeric compound composed of Li3AlF6 and AlPO4, water and a dispersant in a mass ratio of 10:(500-1000):(0.1-0.3) to obtain a suspension;

[0019] B) mixing a lithium compound, a phosphoric acid compound and a suspension to react, and after the reaction is completed, standing and separating the solid and the liquid to obtain an additive material for a negative electrode of a lithium ion battery.

[0020] Preferably, in step A), the dispersant is selected from one of polyethylene glycol, polyacrylamide, methylpentanol and triethylhexyl phosphoric acid.

[0021] Preferably, in step B), the lithium compound is selected from one or more of LiOH, Li2CO3, and CH3COOLi;

[0022] The phosphoric acid compound is selected from one or more of H3PO4, NH4H2PO4, (NH4)2HPO4;

[0023] The mass ratio of the heterogeneous isomorph constructed by Li3AlF6 and AlPO4, the lithium compound and the phosphoric acid compound is 10: (0.124-0.512): (0.169-0.253);

[0024] The reaction is a microwave heating reaction, the microwave power is 800-1000W, the reaction temperature is 60-80°C, and the reaction time is 10-20min.

[0025] The present invention also provides a negative electrode material, comprising a negative electrode active material and an additive material coated on the surface of the negative electrode active material, wherein the additive material is selected from the above-mentioned additive material for the negative electrode of a lithium ion battery.

[0026] Preferably, the negative electrode active material is selected from one or more of graphite, silicon-carbon material, and silicon-oxygen material;

[0027] The mass ratio of the negative electrode active material to the additive material is 49-99.

[0028] The present invention also provides a method for preparing the above-mentioned negative electrode material, comprising the following steps:

[0029] preparing a composite slurry of negative electrode active material and additive material;

[0030] The composite slurry is spray-dried to obtain a negative electrode active material coated with the additive material.

[0031] The present invention also provides a lithium ion battery comprising the above negative electrode material.

[0032] Compared with the prior art, the present invention provides an additive material for the negative electrode of a lithium ion battery, characterized in that it includes a core and a coating layer, wherein the core is a heterogeneous isomorph constructed of Li3AlF6 and AlPO4, and the coating layer is Li3PO4. The present invention prepares a heterogeneous isomorph material by combining two electronic insulating materials, Li3AlF6 and AlPO4, so that the material produces electronic conductivity, thereby obtaining a new ion-electron mixed conductor, and a layer of Li3PO4 is coated on the surface of the mixed conductor using a microwave heterogeneous precipitation method to obtain a composite material that can quickly desolvate lithium ions and quickly transport lithium ions. The mixed conductor material is applied to the negative electrode coating, which can accelerate the lithium ion migration kinetics on the negative electrode surface, significantly reduce polarization, improve the battery rate performance, inhibit the generation of lithium dendrites, and increase the safety and stability of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The X-ray photoelectron spectra of Example 1, Comparative Example 2 and Comparative Example 6 are shown;

[0034] Figure 2 The X-ray photoelectron spectra of Example 1, Comparative Example 3 and Comparative Example 6 are shown;

[0035] Figure 3 TEM image of Li3PO4@Li3AlF6&AlPO4 prepared in Example 1;

[0036] Figure 4 This is the energy spectrum scanning diagram of Li3PO4@Li3AlF6&AlPO4 prepared in Example 1. DETAILED DESCRIPTION

[0037] The invention provides an additive material for a negative electrode of a lithium ion battery, comprising a core and a coating layer, wherein the core is a heterogeneous isomorph constructed of Li3AlF6 and AlPO4, and the coating layer is Li3PO4.

[0038] The additive material for lithium ion battery negative electrode provided by the present invention comprises a core, wherein the core is a heterogeneous isomorph constructed by Li3AlF6 and AlPO4, wherein the preparation method of the heterogeneous isomorph constructed by Li3AlF6 and AlPO4 comprises the following steps:

[0039] Under protective atmosphere conditions, Li3AlF6 and AlPO4 are mixed, subjected to high-energy ball milling, and then dried and calcined to obtain a heterogeneous isomorph constructed of Li3AlF6 and AlPO4.

[0040] Wherein, the protective atmosphere condition is argon.

[0041] The present invention first mixes Li3AlF6 and AlPO4. Wherein, Li3AlF6 is preferably prepared according to the following preparation method:

[0042] The lithium compound, the aluminum source compound and the fluorine source compound are mixed and calcined to obtain Li3AlF6 powder material.

[0043] Wherein, the lithium compound is selected from one or more of lithium nitrate, lithium acetate, lithium oxalate, lithium carbonate, lithium hydroxide, and lithium fluoride;

[0044] The aluminum source compound is selected from one or more of aluminum oxide, aluminum hydroxide, and aluminum nitrate;

[0045] The fluorine source compound is selected from one or more of ammonium fluoride and lithium fluoride;

[0046] The molar ratio of the lithium compound, the aluminum source compound and the fluorine source compound is (1.5-3): (0.5-1): (3-6), which can be 1.5:0.5:3, 2:0.5:3, 3:0.5:3, 1.5:1:3, 1.5:1:4, 1.5:1:5, 1.5:1:6, 2:1:3, 2:1:4, 2:1:5, 2:1:6, 3:1:3, 3:1:4, 3:1:5, 3:1:6, or any value between (1.5-3): (0.5-1): (3-6).

[0047] In the present invention, the mixing is performed by one or more of planetary ball milling, stirring milling and sand milling. Specifically, the raw materials (lithium compound, aluminum source compound and fluorine source compound) are mixed with a grinding solvent and grinding balls for grinding.

[0048] The mass ratio of the grinding balls to the raw materials is 5 to 20, and can be 5, 10, 15, 20, or any value between 5 and 20. The grinding balls are made of zirconia balls, alumina balls or agate balls, preferably zirconia balls. The diameter of the grinding balls is 3 to 5 mm, preferably 3 mm in diameter.

[0049] The mass ratio of the grinding solvent to the raw material is 2 to 5, and can be 2, 3, 4, 5, or any value between 2 and 5. The grinding solvent is selected from one or more of deionized water, anhydrous ethanol, isopropanol, and N-methylpyrrolidone, preferably deionized water.

[0050] The grinding time is 3 to 6 hours, and can be 3, 4, 5, 6, or any value between 3 and 6 hours.

[0051] After grinding, the slurry is dried at a temperature of 80-100° C. After drying, a powder agglomerated into a block is obtained, and the powder is ground in a mortar and passed through a 200-400 mesh screen.

[0052] The powder after grinding and screening is placed in an alumina crucible, heated to 500-600°C at 2-5°C / min, kept warm for 6-12h, and then cooled naturally to obtain Li3AlF6 powder material. The heating rate can be 2, 3, 4, 5, or any value between 2-5°C / min. The calcination temperature can be 500, 520, 540, 550, 560, 580, 600, or any value between 500-600°C, and the insulation time can be 6, 7, 8, 9, 10, 11, 12, or any value between 6-12h.

[0053] After obtaining Li3AlF6, Li3AlF6 and AlPO4 are mixed to obtain a mixed powder. The molar ratio of Li3AlF6 to AlPO4 is 1:(2-3), which can be 1:2, 1:2.1, 1:2.2, 1:2.3, 1:2.4, 1:2.5, 1:2.6, 1:2.7, 1:2.8, 1:2.9, 1:3, or any value between 1:(2-3).

[0054] Then, the mixed powder is subjected to high-energy ball milling, drying and calcination to obtain the heterogeneous isomorph Li3AlF6&AlPO4 constructed of Li3AlF6 and AlPO4.

[0055] During the high-energy ball milling, the mass ratio of the amount of the grinding balls added to the total amount of Li3AlF6 and AlPO4 is (5-10):1, which can be 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, or any value between (5-10):1; the mass ratio of the mass of the grinding solvent to the total amount of Li3AlF6 and AlPO4 is (3-4):1, which can be 3:1, 3.1:1, 3.2:1, 3.3:1, 3.4:1, 3.5:1, 3.6:1, 3.7:1, 3.8:1, 3.9:1, 4:1, or any value between (3-4):1; the grinding solvent is preferably stearic acid;

[0056] The temperature of the high energy ball mill is 25-35° C., which can be 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, or any value between 25 and 35° C. The high energy ball mill is stopped after 60 minutes and cooled for 10 minutes. The high energy ball milling time is 30-40 hours, which can be 30, 32, 34, 35, 36, 38, 40, or any value between 30 and 40 hours. The rotation speed of the high energy ball mill is 1600-1800 rpm, which can be 1600, 1700, 1800, or any value between 1600 and 1800 rpm.

[0057] The drying temperature is 100-200°C, and can be 100, 120, 150, 160, 180, 200, or any value between 100-200°C;

[0058] The calcination atmosphere is an argon atmosphere, the calcination temperature is 400-500°C, which can be 400, 420, 440, 450, 460, 480, 500, or any value between 400 and 500°C, and the calcination time is 4-6h, which can be 4, 5, 6, or any value between 4 and 6h.

[0059] The additive material for lithium ion battery negative electrode provided by the present invention also includes a coating layer, and the coating layer is Li3PO4. In the present invention, the coating layer is prepared by microwave heterogeneous precipitation method.

[0060] The particle size of the heterogeneous isomorph constructed by Li3AlF6 and AlPO4 is 100±20nm, and the thickness of the coating layer is 5-10nm, which can be 5, 6, 7, 8, 9, 10, or any value between 5 and 10nm.

[0061] The present invention also provides a method for preparing the above-mentioned additive material for lithium ion battery negative electrode, comprising the following steps:

[0062] A) mixing a heterogeneous isomeric structure composed of Li3AlF6 and AlPO4, water and a dispersant to obtain a suspension;

[0063] B) mixing a lithium compound, a phosphoric acid compound and a suspension to react, allowing the mixture to stand after the reaction is completed, and performing solid-liquid separation to obtain a Li3PO4@Li3AlF6&AlPO4 lithium ion battery negative electrode additive material.

[0064] Specifically, the present invention first mixes a heterogeneous isomorph constructed by Li3AlF6 and AlPO4, water and a dispersant to obtain a suspension.

[0065] Wherein, the dispersant is selected from one of polyethylene glycol, polyacrylamide, methylpentanol and triethylhexyl phosphoric acid.

[0066] The mass ratio of the isomer, water and dispersant is 10:(500-1000):(0.1-0.3), which can be 10:500:0.1, 10:1000:0.1, 10:500:0.3, 10:1000:0.3, 10:750:0.2, or any value between 10:(500-1000):(0.1-0.3).

[0067] In the present invention, the mixing is preferably ultrasonic mixing.

[0068] Next, a lithium compound, a phosphoric acid compound and a suspension are mixed to react. The lithium compound is selected from one or more of LiOH, Li2CO3, and CH3COOLi;

[0069] The phosphoric acid compound is selected from one or more of H3PO4, NH4H2PO4, (NH4)2HPO4;

[0070] The mass ratio of the heterogeneous isomorph constructed by Li3AlF6 and AlPO4, the lithium compound and the phosphoric acid compound is 10:(0.124-0.512):(0.169-0.253), which can be 10:0.124:0.169, 10:0.2:0.18, 10:0.3:0.2, 10:0.5:0.25, 10:0.512:0.253, or any value between 10:(0.124-0.512):(0.169-0.253).

[0071] The reaction is a microwave heating reaction, the microwave power is 800-1000 W, and can be 800, 850, 900, 950, 1000, or any value between 800 and 1000 W. The reaction temperature is 60-80° C., and can be 60, 65, 70, 75, 80, or any value between 60 and 80° C. The reaction time is 10-20 min, and can be 10, 15, 20, or any value between 10 and 20 min.

[0072] After the reaction is completed, the obtained reaction solution is allowed to stand, and after solid-liquid separation, the obtained precipitate is washed with water and centrifuged, and dried in an oven at 50-80°C to obtain Li3PO4@Li3AlF6&AlPO4 lithium ion battery negative electrode additive material.

[0073] The present invention adopts a microwave heterogeneous precipitation method to prepare a Li3PO4 coating layer on the surface of Li3AlF6&AlPO4, which can realize a coating layer with a nanometer size and uniform thickness.

[0074] The present invention also provides a negative electrode material, comprising a negative electrode active material and an additive material coated on the surface of the negative electrode active material, wherein the additive material is selected from the above-mentioned additive material for the negative electrode of a lithium ion battery.

[0075] Specifically, the negative electrode material provided by the present invention includes a negative electrode active material, and the negative electrode active material is selected from one or more of graphite, silicon-carbon material, and silicon-oxygen material.

[0076] The mass ratio of the negative electrode active material to the additive material is 49-99, and can be 49, 50, 55, 60, 65, 70, 75, 80, 85, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or any value between 49 and 99.

[0077] The present invention also provides a method for preparing the above-mentioned negative electrode material, comprising the following steps:

[0078] preparing a composite slurry of negative electrode active material and additive material;

[0079] The composite slurry is spray-dried to obtain a negative electrode active material coated with the additive material.

[0080] The present invention first prepares the negative electrode active material and the additive material into a composite slurry, wherein the solvent in the composite slurry is selected from one or more of deionized water, anhydrous ethanol and isopropanol.

[0081] Then, the composite slurry is spray-dried to obtain a negative electrode active material coated with the additive material.

[0082] The present invention also provides a lithium ion battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the negative electrode comprises a current collector and a negative electrode film composited on the surface of the current collector, and the negative electrode film is prepared from a negative electrode material, a conductive agent, a binder and a thickener.

[0083] Among them, the negative electrode material is selected from the negative electrode active material coated with the additive material mentioned above, that is, (Li3PO4@Li3AlF6&AlPO4)@negative electrode active material, the conductive agent is selected from acetylene black, graphene, carbon black, carbon nanotubes; the binder is selected from styrene-butadiene rubber (SBR), polyacrylic acid (PAA), polyvinyl alcohol (PVA), and the thickener is selected from sodium carboxymethyl cellulose (CMC), methyl cellulose (MC), ethyl cellulose (EC), and hydroxyethyl cellulose (HEC).

[0084] The positive electrode comprises a current collector and a positive electrode film compounded on the surface of the current collector, and the positive electrode film is prepared from a positive electrode active material, a conductive agent and a binder.

[0085] The present invention has no particular restrictions on the specific types of the positive electrode active material, the conductive agent and the binder, and any material known to those skilled in the art for preparing the positive electrode can be used. In the present invention, the positive electrode active material is preferably a lithium iron phosphate material, the conductive agent is preferably acetylene black, and the binder is preferably PVDF.

[0086] The present invention has no particular limitation on the specific types of the separator and the electrolyte, and any separator and electrolyte known to those skilled in the art may be used.

[0087] In the present invention, the additive material for the negative electrode of the lithium-ion battery is represented by "Li3PO4@Li3AlF6&AlPO4", that is, Li3PO4 is used as a coating layer to coat the heterogeneous isomorph constructed by Li3AlF6 and AlPO4.

[0088] In the present invention, the negative electrode material is represented by "(Li3PO4@Li3AlF6&AlPO4)@negative electrode active material", that is, the negative electrode active material is coated with the additive material Li3PO4@Li3AlF6&AlPO4 as a coating layer.

[0089] The present invention combines two electronic insulating materials, Li3AlF6 and AlPO4, to prepare a heterogeneous isomorphic material, so that the material produces electronic conductivity, thereby obtaining a new ionic electron mixed conductor, and uses a microwave heterogeneous precipitation method to coat a layer of Li3PO4 on the surface of the mixed conductor to obtain a composite material that can quickly desolvate lithium ions and quickly transmit lithium ions. The mixed conductor material is applied to negative electrode coating, which can accelerate the lithium ion migration kinetics on the negative electrode surface, significantly reduce polarization, improve battery rate performance, inhibit the generation of lithium dendrites, and increase battery safety and stability.

[0090] In order to further understand the present invention, the additive material for lithium ion battery negative electrode provided by the present invention and its preparation method and application are described below in conjunction with embodiments. The protection scope of the present invention is not limited by the following embodiments.

[0091] Example 1

[0092] 1. Preparation of Li3AlF6 materials

[0093] Weigh 86.25g of lithium nitrate, 21.25g of aluminum oxide and 92.57g of ammonium fluoride, disperse the above powders in a solvent by planetary ball milling, add 400g of isopropanol, and grind for 6h, wherein the ball-to-material mass ratio is 5, the mass of the grinding ball is 1000g, the material of the grinding ball is zirconia ball, and the diameter of the grinding ball is 5mm.

[0094] After grinding, the slurry was dried at 80° C. After drying, a powder agglomerated into a block was obtained, and the powder was ground with a mortar and passed through a 200-mesh sieve.

[0095] The ground and sieved powder was placed in an alumina crucible, heated to 500°C at 2°C / min, kept warm for 6 hours, and then cooled naturally to obtain Li3AlF6 powder material.

[0096] 2. Use 107.49g of commercial AlPO4 and 92.51g of the prepared Li3AlF6 to mix, put into a high-energy ball mill after mixing evenly, control the temperature in the cavity at 25°C, and perform ball milling under argon protective atmosphere. Stop and cool for 10 minutes every 60 minutes. The grinding time is 30 hours, the rotation speed is 1600rpm, the grinding ball mass is 1000g, and the stearic acid is 600g.

[0097] The slurry was dried at 100°C and kept at 400°C for 6 h in an argon atmosphere to obtain Li3AlF6&AlPO4 heterogeneous isomorphs.

[0098] 3. Preparation of Li3PO4@Li3AlF6&AlPO4 composite powder by microwave heterogeneous precipitation method

[0099] 10g Li3AlF6&AlPO4 powder, 800g deionized water and 0.1g polyethylene glycol dispersant were mixed and ultrasonically dispersed to obtain Li3AlF6&AlPO4 suspension; 0.124g LiOH was added to a double-mouth round-bottom flask, and 50g deionized water was added, and the mixture was placed in a laboratory microwave oven and stirred to obtain a LiOH solution; the Li3AlF6&AlPO4 suspension was added to the LiOH solution, and 0.169g H3PO4 was added at the same time, the microwave power was 800W, the reaction temperature was controlled to be 60°C, the mixture was reacted for 10min under stirring, and the mixture was allowed to stand for solid-liquid separation. The obtained powder precipitate was washed and centrifuged, and dried in an oven at 50°C to obtain Li3PO4@Li3AlF6&AlPO4 composite powder;

[0100] The Li3PO4@Li3AlF6&AlPO4 composite powder includes: a Li3AlF6&AlPO4 inner core with a particle size of 100±20nm; and a Li3PO4 coating layer composited on the outer surface of the Li3AlF6&AlPO4 inner core with a thickness of 5nm.

[0101] 4. Test ionic conductivity

[0102] Take 0.5g of the powder prepared above. Use a mold with a diameter of 10mm, apply a pressure of 5MPa in a desktop powder tablet press, maintain the pressure for 15min, and then demold to obtain a thin sheet of mixed ion conductor. Place the above-mentioned thin sheet in a sintering furnace, heat it to 900℃ at 2℃ / min, and keep it warm for 20h. You can get a ceramic sheet of mixed ion conductor. Use 1000-grit sandpaper moistened with alcohol to gently polish the surface of the above-mentioned ceramic sheet according to the cross-cross method to remove surface impurities and ensure that the thickness of the electrolyte is uniform at all positions. Use a vernier caliper to measure the thickness L of the ceramic sheet, use an ion sputtering instrument to evaporate the gold blocking electrode, and use AC impedance to test the ionic conductivity of the mixed ion conductor, recorded as σ1.

[0103] 5. Test electronic conductivity

[0104] Based on the principle of testing the electronic conductivity of powder by the four-probe method, the electronic conductivity of the mixed ion conductor was tested. 5g of the above mixed ion conductor material Li3PO4@Li3AlF6&AlPO4 was added to the powder resistance tester for testing. The electronic conductivity of the sample was tested under a pressure of 100MPa, which was recorded as ρ1.

[0105] 6. Coated graphite negative electrode

[0106] Commercial graphite and Li3PO4@Li3AlF6&AlPO4 powder were prepared into a composite slurry in a mass ratio of 98:2, and the slurry was dried into (Li3PO4@Li3AlF6&AlPO4)@graphite material by spray drying.

[0107] 7. Preparation of button cells

[0108] The (Li3PO4@Li3AlF6&AlPO4)@graphite (active material), acetylene black (conductive agent), sodium carboxymethyl cellulose (CMC as thickener) and styrene-butadiene rubber (SBR as binder) prepared in this embodiment were added with an appropriate amount of deionized water in a mass ratio of 96.5:0.5:1.2:1.8 and stirred for 10 hours to form a slurry. The slurry was applied on the cut copper foil and kept at 80°C for 10 hours to obtain the negative electrode foil. The dried electrode foil was punched into a pole piece with a diameter of 10 mm using a cutting machine.

[0109] The positive electrode sheet is made of lithium iron phosphate material. The preparation method of the lithium iron phosphate positive electrode sheet is as follows: lithium iron phosphate is used as the active material, acetylene black is used as the conductive agent, and PVDF is used as the binder. After mixing in a mass ratio of 8:1:1, an appropriate amount of NMP is added as the solvent, and the positive electrode slurry is obtained after stirring for 10 hours. The mixed slurry is coated on aluminum foil and vacuum dried at 100°C for 12 hours. After taking it out, it is cut into 10mm pole pieces. In the glove box, the (Li3PO4@Li3AlF6&AlPO4)@graphite pole piece is placed in the electrode shell, the diaphragm is placed in and the electrolyte is dripped. Then the lithium sheet, gasket, shrapnel, and battery shell are placed in order and the battery is pressed.

[0110] The assembled button cell was subjected to constant current charge and discharge test on the battery test system, with a voltage range of 0.01 to 1.0 V and a rate of 0.05C.

[0111] 9. Electrochemical performance test

[0112] The battery test was carried out at a constant temperature of 25°C. For the cycle performance test, the battery was first activated by charging and discharging at a low current of 0.1C three times, and then charged and discharged at a constant current of 0.5C for 100 times. For the rate performance test, the battery was charged and discharged at a constant current of 1C, 2C, 3C, and 5C for five times in the voltage range of 2.5 to 3.65V.

[0113] The electronic state of Li3AlF6 before and after the combination with AlPO4 was analyzed by XPS. Compared with Li3AlF6 in Comparative Example 3 and AlPO4 in Comparative Example 2, and Li3AlF6-AlPO4 prepared by simple mixing in Comparative Example 6, the F1s peak of Li3AlF6&AlPO4 shifted to a lower binding energy by about 0.5 eV, while the O1s peak shifted to a higher binding energy by about 0.5 eV. These chemical shifts indicate that electron transfer occurred in the middle layer, that is, an electron was transferred from O in AlPO4 to F in Li3AlF6. This shows that Li3AlF6 and AlPO4 are tightly combined and form a heterogeneous isomorph, which produces electrons that can move, thus giving the material electronic conductivity. See Figure 1 and Figure 2 As shown, Figure 1 The X-ray photoelectron spectra of Example 1, Comparative Example 2 and Comparative Example 6 are shown in FIG. Figure 2 The X-ray photoelectron spectra of Example 1, Comparative Example 3 and Comparative Example 6 are shown.

[0114] Figure 3 This is a TEM image of a thin layer of Li3PO4 coated on Li3AlF6&AlPO4 by microwave heterogeneous precipitation. It can be seen from the figure that the coating is uniform and continuous. Figure 4 The energy spectrum scanning diagram shows that the coating layer contains phosphorus but does not contain aluminum and F, which further confirms that the coating layer is Li3PO4.

[0115] Example 2

[0116] 1. Preparation of Li3AlF6 materials

[0117] Weigh 57.81g of lithium carbonate, 26.56g of aluminum oxide and 115.63g of ammonium fluoride, disperse the above powders in a solvent by planetary ball milling, add 600g of deionized water, and grind for 3h, wherein the ball-to-material mass ratio is 10, the mass of the grinding ball is 2000g, the material of the grinding ball is aluminum oxide ball, and the diameter of the grinding ball is 3mm.

[0118] After grinding, the slurry was dried at 90° C. After drying, a powder agglomerated into a block was obtained, and the powder was ground with a mortar and passed through a 300-mesh sieve.

[0119] The ground and sieved powder was placed in an alumina crucible, heated to 550°C at 3°C / min, kept warm for 8 hours, and then cooled naturally to obtain Li3AlF6 powder material.

[0120] 2. Use 85.92g of commercial AlPO4 and 114.08g of the prepared Li3AlF6 to mix, put into a high-energy ball mill after mixing evenly, control the temperature in the cavity at 30°C, and perform ball milling under argon protective atmosphere. Stop and cool for 10 minutes every 60 minutes. The grinding time is 40 hours, the rotation speed is 1800rpm, the grinding ball mass is 2000g, and stearic acid is 800g.

[0121] The slurry was dried at 150°C and kept at 450°C for 5 h in an argon atmosphere to obtain Li3AlF6&AlPO4 heterogeneous isomorphs.

[0122] 3. Preparation of Li3PO4@Li3AlF6&AlPO4 composite powder by microwave heterogeneous precipitation method

[0123] 10g Li3AlF6&AlPO4 powder, 500g deionized water and 0.2g polyacrylamide dispersant were mixed and ultrasonically dispersed to obtain Li3AlF6&AlPO4 suspension; 0.191g Li2CO3 was added to a double-mouth round-bottom flask, and 75g deionized water was added, and the mixture was placed in a laboratory microwave oven and stirred to obtain a Li2CO3 solution; the Li3AlF6&AlPO4 suspension was added to the Li2CO3 solution, and 0.169g H3PO4 was added at the same time, the microwave power was 900W, the reaction temperature was controlled to 70°C, the mixture was reacted for 15min under stirring, and the mixture was allowed to stand for solid-liquid separation. The obtained powder precipitate was washed and centrifuged, and dried in an oven at 60°C to obtain Li3PO4@Li3AlF6&AlPO4 composite powder;

[0124] The Li3PO4@Li3AlF6&AlPO4 composite powder includes: a Li3AlF6&AlPO4 inner core with a particle size of 100±20nm; and a Li3PO4 coating layer composited on the outer surface of the Li3AlF6&AlPO4 inner core with a thickness of 7nm.

[0125] 4. Test ionic conductivity

[0126] Take 0.1g of the powder prepared above. Use a mold with a diameter of 10mm, apply a pressure of 10MPa in a desktop powder tablet press, maintain the pressure for 10min, and then demold to obtain a thin sheet of mixed ion conductor. Place the above-mentioned thin sheet in a sintering furnace, heat it to 1000℃ at 4℃ / min, and keep it warm for 15h. You can get a ceramic sheet of mixed ion conductor. Use 1000-mesh sandpaper moistened with alcohol to gently polish the surface of the above-mentioned ceramic sheet according to the cross-cross method to remove surface impurities and ensure that the thickness of the electrolyte is uniform at all positions. Use a vernier caliper to measure the thickness L of the ceramic sheet, use an ion sputtering instrument to evaporate the gold blocking electrode, and use AC impedance to test the ionic conductivity of the mixed ion conductor, recorded as σ2.

[0127] 5. Test electronic conductivity

[0128] Based on the principle of testing the electronic conductivity of powder by the four-probe method, the electronic conductivity of the mixed ion conductor is tested. 10g of the above mixed ion conductor material Li3PO4@Li3AlF6&AlPO4 is added to the powder resistance tester for testing. The electronic conductivity of the sample is tested under a pressure of 100MPa, which is recorded as ρ2.

[0129] 6. Coated graphite negative electrode

[0130] Commercial graphite and Li3PO4@Li3AlF6&AlPO4 powder were prepared into a composite slurry in a mass ratio of 99:1, and the slurry was dried into (Li3PO4@Li3AlF6&AlPO4)@graphite material by a spray drying method.

[0131] 7. The subsequent steps are consistent with Example 1.

[0132] Example 3

[0133] 1. Preparation of Li3AlF6 materials

[0134] Weigh 42.60g of lithium hydroxide, 26.04g of aluminum hydroxide and 131.36g of ammonium fluoride, disperse the above powders in a solvent by planetary ball milling, add 800g of anhydrous ethanol, and grind for 6h, wherein the ball-to-material mass ratio is 20, the mass of the grinding balls is 4000g, the material of the grinding balls is agate balls, and the diameter of the grinding balls is 4mm.

[0135] After grinding, the slurry was dried at 100° C. After drying, a powder agglomerated into a block was obtained, and the powder was ground with a mortar and passed through a 400-mesh sieve.

[0136] The ground and sieved powder was placed in an alumina crucible, heated to 550°C at 4°C / min, kept warm for 12 hours, and then cooled naturally to obtain Li3AlF6 powder material.

[0137] 2. Use 40.13g of commercial AlPO4 and 159.87g of the prepared Li3AlF6 to mix, put into a high-energy ball mill after mixing evenly, control the temperature in the cavity at 35°C, and perform ball milling under argon protective atmosphere. Stop and cool for 10 minutes every 60 minutes. The grinding time is 35 hours, the rotation speed is 1700rpm, the grinding ball mass is 1400g, and the stearic acid is 700g.

[0138] The slurry was dried at 200°C and kept at 500°C for 6 h in an argon atmosphere to obtain Li3AlF6&AlPO4 heterogeneous isomorphs.

[0139] 3. Preparation of Li3PO4@Li3AlF6&AlPO4 composite powder by microwave heterogeneous precipitation method

[0140] 10g Li3AlF6&AlPO4 powder, 1000g deionized water and 0.3g methyl pentanol dispersant were mixed and ultrasonically dispersed to obtain Li3AlF6&AlPO4 suspension; 0.512g CH3COOLi was added to a double-mouth round-bottom flask, and 100g deionized water was added, and the mixture was placed in a laboratory microwave oven and stirred to obtain a CH3COOLi solution; the Li3AlF6&AlPO4 suspension was added to the CH3COOLi solution, and 0.253g H3PO4 was added at the same time, the microwave power was 1000W, the reaction temperature was controlled to 80°C, the mixture was reacted for 20min under stirring, and the mixture was allowed to stand for solid-liquid separation. The obtained powder precipitate was washed and centrifuged, and dried in an oven at 80°C to obtain Li3PO4@Li3AlF6&AlPO4 composite powder;

[0141] The Li3PO4@Li3AlF6&AlPO4 composite powder includes: a Li3AlF6&AlPO4 inner core with a particle size of 100±20nm; and a Li3PO4 coating layer composited on the outer surface of the Li3AlF6&AlPO4 inner core with a thickness of 10nm.

[0142] 4. Test ionic conductivity

[0143] Take 5g of the powder prepared above. Use a mold with a diameter of 15mm, apply a pressure of 15MPa in a desktop powder tablet press, maintain the pressure for 20min, and then demold to obtain a thin sheet of mixed ion conductor. Place the above-mentioned thin sheet in a sintering furnace, heat it to 1300℃ at 5℃ / min, and keep it warm for 20h. You can get a ceramic sheet of mixed ion conductor. Use 1000-mesh sandpaper moistened with alcohol to gently polish the surface of the above-mentioned ceramic sheet according to the cross-cross method to remove surface impurities and ensure that the thickness of the electrolyte is uniform at all positions. Use a vernier caliper to measure the thickness L of the ceramic sheet, use an ion sputtering instrument to evaporate the gold blocking electrode, and use AC impedance to test the ionic conductivity of the mixed ion conductor, recorded as σ3.

[0144] 5. Test electronic conductivity

[0145] Based on the principle of testing the electronic conductivity of powder by the four-probe method, the electronic conductivity of the mixed ion conductor was tested. 10g of the above mixed ion conductor material Li3PO4@Li3AlF6&AlPO4 was added to the powder resistance tester for testing. The electronic conductivity of the sample was tested at a pressure of 300MPa, which was recorded as ρ3.

[0146] 6. Coated silicon-carbon negative electrode

[0147] Commercial silicon-carbon material and Li3PO4@Li3AlF6&AlPO4 powder were prepared into a composite slurry in a mass ratio of 98.5:1.5, and the slurry was dried into (Li3PO4@Li3AlF6&AlPO4)@silicon-carbon material by spray drying.

[0148] 7. The subsequent steps are consistent with Example 1.

[0149] Example 4

[0150] 1. Preparation of Li3AlF6 materials

[0151] Weigh 45.35g of lithium fluoride, 25.58g of aluminum hydroxide and 129.07g of ammonium fluoride, disperse the above powders in a solvent by planetary ball milling, add 900g of N-methylpyrrolidone, and grind for 5h, wherein the ball-to-material mass ratio is 15, the mass of the grinding balls is 3000g, the material of the grinding balls is alumina balls, and the diameter of the grinding balls is 5mm.

[0152] After grinding, the slurry was dried at 90° C. After drying, a powder agglomerated into a block was obtained, and the powder was ground with a mortar and passed through a 350-mesh sieve.

[0153] The ground and sieved powder was placed in an alumina crucible, heated to 600°C at 2°C / min, kept warm for 9 hours, and then cooled naturally to obtain Li3AlF6 powder material.

[0154] 2. Use 120.20g of commercial AlPO4 and 79.80g of the prepared Li3AlF6 to mix, put into a high-energy ball mill after mixing evenly, control the temperature in the cavity at 30°C, and perform ball milling under argon protective atmosphere. Stop and cool for 10 minutes every 60 minutes. The grinding time is 40 hours, the rotation speed is 1800rpm, the grinding ball mass is 1800g, and the stearic acid is 750g.

[0155] The slurry was dried at 190°C and kept at 480°C for 5 h in an argon atmosphere to obtain Li3AlF6&AlPO4 heterogeneous isomorphs.

[0156] 3. Preparation of Li3PO4@Li3AlF6&AlPO4 composite powder by microwave heterogeneous precipitation method

[0157] 10g Li3AlF6&AlPO4 powder, 600g deionized water and 0.2g triethylhexyl phosphoric acid dispersant were mixed and ultrasonically dispersed to obtain Li3AlF6&AlPO4 suspension; 0.124g Li2CO3 was added to a double-mouth round-bottom flask, and 90g deionized water was added, and the mixture was placed in a laboratory microwave oven and stirred to obtain a Li2CO3 solution; the Li3AlF6&AlPO4 suspension was added to the Li2CO3 solution, and 0.198g NH4H2PO4 was added at the same time, the microwave power was 800W, the reaction temperature was controlled to 75°C, the mixture was reacted for 18min under stirring, and the mixture was allowed to stand for solid-liquid separation. The obtained powder precipitate was washed and centrifuged, and dried in an oven at 75°C to obtain Li3PO4@Li3AlF6&AlPO4 composite powder;

[0158] The Li3PO4@Li3AlF6&AlPO4 composite powder includes: a Li3AlF6&AlPO4 inner core with a particle size of 100±20nm; and a Li3PO4 coating layer composited on the outer surface of the Li3AlF6&AlPO4 inner core with a thickness of 6nm.

[0159] 4. Test ionic conductivity

[0160] Take 2g of the powder prepared above. Use a mold with a diameter of 10mm, apply a pressure of 10MPa in a desktop powder tablet press, maintain the pressure for 15min, and then demold to obtain a thin sheet of mixed ion conductor. Place the above-mentioned thin sheet in a sintering furnace, heat it to 1200℃ at 4℃ / min, and keep it warm for 14h. You can get a ceramic sheet of mixed ion conductor. Use 1000-grit sandpaper moistened with alcohol to gently polish the surface of the above-mentioned ceramic sheet according to the cross-cross method to remove surface impurities and ensure that the thickness of the electrolyte is uniform at all positions. Use a vernier caliper to measure the thickness L of the ceramic sheet, use an ion sputtering instrument to evaporate the gold blocking electrode, and use AC impedance to test the ionic conductivity of the mixed ion conductor, recorded as σ4.

[0161] 5. Test electronic conductivity

[0162] Based on the principle of testing the electronic conductivity of powder by the four-probe method, the electronic conductivity of the mixed ion conductor was tested. 10g of the above mixed ion conductor material Li3PO4@Li3AlF6&AlPO4 was added to the powder resistance tester for testing. The electronic conductivity of the sample was tested at a pressure of 300MPa, which was recorded as ρ4.

[0163] 6. Coated silicon oxide negative electrode

[0164] Commercial silicon oxide material and Li3PO4@Li3AlF6&AlPO4 powder were prepared into a composite slurry in a mass ratio of 98.7:1.3, and the slurry was dried into (Li3PO4@Li3AlF6&AlPO4)@silicon oxide material by spray drying.

[0165] 7. The subsequent steps are consistent with Example 1.

[0166] Example 5

[0167] 1. Preparation of Li3AlF6 materials

[0168] Weigh 49.81g of lithium acetate, 94.34g of aluminum nitrate and 55.85g of ammonium fluoride, disperse the above powders in a solvent by planetary ball milling, add 400ml of deionized water, and grind for 3h, wherein the ball-to-material mass ratio is 5, the mass of the grinding ball is 1000g, the material of the grinding ball is zirconia ball, and the diameter of the grinding ball is 3mm.

[0169] After grinding, the slurry was dried at 80° C. After drying, a powder agglomerated into a block was obtained, and the powder was ground with a mortar and passed through a 200-mesh sieve.

[0170] The ground and sieved powder was placed in an alumina crucible, heated to 500°C at 4°C / min, kept warm for 6 hours, and then cooled naturally to obtain Li3AlF6 powder material.

[0171] 2. Use 66.85g of commercial AlPO4 and 133.15g of the prepared Li3AlF6 to mix, put into a high-energy ball mill after mixing evenly, control the temperature in the cavity at 25°C, and perform ball milling under argon protective atmosphere. Stop and cool for 10 minutes every 60 minutes. The grinding time is 30 hours, the rotation speed is 1600rpm, the grinding ball mass is 1000g, and the stearic acid is 600g.

[0172] The slurry was dried at 100°C and kept at 400°C for 4 h in an argon atmosphere to obtain Li3AlF6&AlPO4 heterogeneous isomorphs.

[0173] 3. Preparation of Li3PO4@Li3AlF6&AlPO4 composite powder by microwave heterogeneous precipitation method

[0174] 10g Li3AlF6&AlPO4 powder, 500g deionized water and 0.1g polyethylene glycol dispersant were mixed and ultrasonically dispersed to obtain Li3AlF6&AlPO4 suspension; 0.191g Li2CO3 was added to a double-mouth round-bottom flask, and 50g deionized water was added, and the mixture was placed in a laboratory microwave oven and stirred to obtain a Li2CO3 solution; the Li3AlF6&AlPO4 suspension was added to the Li2CO3 solution, and 0.228g (NH4)2HPO4 was added at the same time, the microwave power was 800W, the reaction temperature was controlled to be 60°C, the mixture was reacted for 10min under stirring, and the mixture was allowed to stand for solid-liquid separation. The obtained powder precipitate was washed and centrifuged, and dried in an oven at 50°C to obtain Li3PO4@Li3AlF6&AlPO4 composite powder;

[0175] The Li3PO4@Li3AlF6&AlPO4 composite powder includes: a Li3AlF6&AlPO4 inner core with a particle size of 100±20nm; and a Li3PO4 coating layer composited on the outer surface of the Li3AlF6&AlPO4 inner core with a thickness of 5nm.

[0176] 4. Test ionic conductivity

[0177] Take 3g of the powder prepared above. Use a mold with a diameter of 10mm, apply a pressure of 5MPa in a desktop powder tablet press, maintain the pressure for 10min, and then demold to obtain a thin sheet of mixed ion conductor. Place the above thin sheet in a sintering furnace, heat it to 900℃ at 2℃ / min, and keep it warm for 12h. You can get a ceramic sheet of mixed ion conductor. Use 1000-grit sandpaper moistened with alcohol to gently polish the surface of the above ceramic sheet according to the cross-cross method to remove surface impurities and ensure that the thickness of the electrolyte is uniform at all positions. Use a vernier caliper to measure the thickness L of the ceramic sheet, use an ion sputtering instrument to evaporate the gold blocking electrode, and use AC impedance to test the ionic conductivity of the mixed ion conductor, recorded as σ5.

[0178] 5. Test electronic conductivity

[0179] Based on the principle of testing the electronic conductivity of powder by the four-probe method, the electronic conductivity of the mixed ion conductor was tested. 10g of the above mixed ion conductor material Li3PO4@Li3AlF6&AlPO4 was added to the powder resistance tester for testing. The electronic conductivity of the sample was tested at a pressure of 300MPa, which was recorded as ρ5.

[0180] 6. Coated graphite negative electrode

[0181] Commercial graphite and Li3PO4@Li3AlF6&AlPO4 powder were prepared into a composite slurry in a mass ratio of 98.3:1.7, and the slurry was dried into (Li3PO4@Li3AlF6&AlPO4)@graphite material by a spray drying method.

[0182] 6. The subsequent steps are consistent with Example 1.

[0183] Comparative Example 1 (graphite control group)

[0184] Pure graphite was used as the active material to prepare button cells according to step 7 of Example 1 and then tested.

[0185] Comparative Example 2 (Li3AlF6@graphite control group)

[0186] 1. Preparation of Li3AlF6 materials

[0187] Weigh 86.25g of lithium nitrate, 21.25g of aluminum oxide and 92.57g of ammonium fluoride, disperse the above powders in a solvent by planetary ball milling, add 400g of isopropanol, and grind for 6h, wherein the ball-to-material mass ratio is 5, the mass of the grinding ball is 1000g, the material of the grinding ball is zirconia ball, and the diameter of the grinding ball is 5mm.

[0188] After grinding, the slurry was dried at 80° C. After drying, a powder agglomerated into a block was obtained, and the powder was ground with a mortar and passed through a 200-mesh sieve.

[0189] The ground and sieved powder was placed in an alumina crucible, heated to 500°C at 2°C / min, kept warm for 6 hours, and then cooled naturally to obtain Li3AlF6 powder material.

[0190] 2. Commercial graphite and Li3AlF6 powder were used in a mass ratio of 98:2 to prepare a composite slurry, and the slurry was dried into Li3AlF6@graphite material by spray drying.

[0191] 3. Li3AlF6@graphite was used as the active material to prepare button cells according to step 7 of Example 1 and then tested.

[0192] Comparative Example 3 (AlPO4@graphite control group)

[0193] 1. Commercial graphite and 2 wt.% of commercial AlPO4 powder were used to prepare a composite slurry, and the slurry was dried into AlPO4@graphite material by spray drying.

[0194] 2. AlPO4@graphite was used as the active material to prepare button cells according to step 7 of Example 1 and then tested.

[0195] Comparative Example 4 (Li3PO4@graphite control group)

[0196] 1. Commercial graphite and commercial Li3PO4 powder were used in a mass ratio of 98:2 to prepare a composite slurry, and the slurry was dried into Li3PO4@graphite material by a spray drying method.

[0197] 2. Li3PO4@graphite was used as the active material to prepare button cells according to step 7 of Example 1 and then tested.

[0198] Comparative Example 5 ((Li3AlF6&AlPO4)@graphite control group)

[0199] 1. Preparation of Li3AlF6 materials

[0200] Weigh 86.25g of lithium nitrate, 21.25g of aluminum oxide and 92.57g of ammonium fluoride, disperse the above powders in a solvent by planetary ball milling, add 400g of isopropanol, and grind for 6h, wherein the ball-to-material mass ratio is 5, the mass of the grinding ball is 1000g, the material of the grinding ball is zirconia ball, and the diameter of the grinding ball is 5mm.

[0201] After grinding, the slurry was dried at 80° C. After drying, a powder agglomerated into a block was obtained, and the powder was ground with a mortar and passed through a 200-mesh sieve.

[0202] The ground and sieved powder was placed in an alumina crucible, heated to 500°C at 2°C / min, kept warm for 6 hours, and then cooled naturally to obtain Li3AlF6 powder material.

[0203] 2. Use 107.49g of commercial AlPO4 and 92.51g of the prepared Li3AlF6 to mix, put into a high-energy ball mill after mixing evenly, control the temperature in the cavity at 25°C, and perform ball milling under argon protective atmosphere. Stop and cool for 10 minutes every 60 minutes. The grinding time is 30 hours, the rotation speed is 1600rpm, the grinding ball mass is 1000g, and the stearic acid is 600g.

[0204] The slurry was dried at 100°C and kept at 400°C for 6 h in an argon atmosphere to obtain Li3AlF6&AlPO4 heterogeneous isomorphs.

[0205] 3. Commercial graphite and Li3AlF6&AlPO4 powder were used in a mass ratio of 98:2 to prepare a composite slurry, and the slurry was dried into (Li3AlF6&AlPO4)@graphite material by spray drying.

[0206] 4. (Li3AlF6&AlPO4)@graphite was used as the active material to prepare button cells according to step 7 of Example 1 and then tested.

[0207] Comparative Example 6 ((Li3AlF6-AlPO4)@graphite control group)

[0208] 1. Preparation of Li3AlF6 materials

[0209] Weigh 86.25g of lithium nitrate, 21.25g of aluminum oxide and 92.57g of ammonium fluoride, disperse the above powders in a solvent by planetary ball milling, add 400g of isopropanol, and grind for 6h, wherein the ball-to-material mass ratio is 5, the mass of the grinding ball is 1000g, the material of the grinding ball is zirconia ball, and the diameter of the grinding ball is 5mm.

[0210] After grinding, the slurry was dried at 80° C. After drying, a powder agglomerated into a block was obtained, and the powder was ground with a mortar and passed through a 200-mesh sieve.

[0211] The ground and sieved powder was placed in an alumina crucible, heated to 500°C at 2°C / min, kept warm for 6 hours, and then cooled naturally to obtain Li3AlF6 powder material.

[0212] 2. Use 107.49 g of commercial AlPO4 and 92.51 g of the prepared Li3AlF6 by planetary milling at 300 rpm for 10 min to obtain Li3AlF6-AlPO4 mixed powder.

[0213] 3. Use commercial graphite and Li3AlF6-AlPO4 mixed powder in a mass ratio of 98:2 to prepare a composite slurry, and dry the above slurry into (Li3AlF6-AlPO4)@graphite material by spray drying.

[0214] 4. (Li3AlF6-AlPO4)@graphite was used as the active material to prepare button cells according to step 7 of Example 1 and then tested.

[0215] Comparative Example 7 ((Li3PO4@Li3AlF6)@graphite control group)

[0216] 1. Preparation of Li3AlF6 materials

[0217] Weigh 86.25g of lithium nitrate, 21.25g of aluminum oxide and 92.57g of ammonium fluoride, disperse the above powders in a solvent by planetary ball milling, add 400g of isopropanol, and grind for 6h, wherein the ball-to-material mass ratio is 5, the mass of the grinding ball is 1000g, the material of the grinding ball is zirconia ball, and the diameter of the grinding ball is 5mm.

[0218] After grinding, the slurry was dried at 80° C. After drying, a powder agglomerated into a block was obtained, and the powder was ground with a mortar and passed through a 200-mesh sieve.

[0219] The ground and sieved powder was placed in an alumina crucible, heated to 500°C at 2°C / min, kept warm for 6 hours, and then cooled naturally to obtain Li3AlF6 powder material.

[0220] 2. Preparation of Li3PO4@Li3AlF6 powder by microwave heterogeneous precipitation method

[0221] 10g Li3AlF6 powder, 800g deionized water and 0.1g polyethylene glycol dispersant were mixed and ultrasonically dispersed to obtain Li3AlF6 suspension; 0.124g LiOH was added to a double-necked round-bottom flask, and 50g deionized water was added, and the mixture was placed in a laboratory microwave oven and stirred to obtain LiOH solution; the Li3AlF6 suspension was added to the LiOH solution, and 0.169g H3PO4 was added at the same time, the microwave power was 800W, the reaction temperature was controlled to be 60°C, the mixture was reacted for 10min under stirring, and the mixture was allowed to stand for solid-liquid separation. The obtained powder precipitate was washed with water and centrifuged, and dried in an oven at 50°C to obtain Li3PO4@Li3AlF6 composite powder.

[0222] 3. Commercial graphite and Li3PO4@Li3AlF6 powder were used in a ratio of 98:2 to prepare a composite slurry, and the slurry was dried into (Li3PO4@Li3AlF6)@graphite material by spray drying.

[0223] 4. (Li3PO4@Li3AlF6)@graphite was used as the active material to prepare button cells according to step 7 of Example 1 and then tested.

[0224] Comparative Example 8 Preparation of Li3PO4@AlPO4 powder by microwave heterogeneous precipitation method

[0225] 1. Mix 10g of commercial AlPO4 powder, 800g of deionized water and 0.1g of polyethylene glycol dispersant, and disperse them by ultrasonic dispersion to obtain AlPO4 suspension; add 0.124g of LiOH into a double-necked round-bottom flask, add 50g of deionized water, place it in a laboratory microwave oven, stir and mix to obtain LiOH solution; add the AlPO4 suspension to the LiOH solution, and add 0.169g of H3PO4 at the same time, the microwave power is 800W, the reaction temperature is controlled to 60°C, react for 10min under stirring, let it stand, after solid-liquid separation, the obtained powder precipitate is washed with water and centrifuged, and dried in an oven at 50°C to obtain Li3PO4@AlPO4 composite powder.

[0226] 2. Commercial graphite and 2 wt.% Li3PO4@AlPO4 powder were used to prepare a composite slurry, and the slurry was dried into (Li3PO4@AlPO4)@graphite material by spray drying.

[0227] 3. Using (Li3PO4@AlPO4)@graphite as the active material, button cells were prepared according to step 7 of Example 1 and then tested.

[0228] Comparative Example 9 ((Li3PO4@Li3AlF6-AlPO4)@graphite control group)

[0229] 1. Preparation of Li3AlF6 materials

[0230] Weigh 86.25g of lithium nitrate, 21.25g of aluminum oxide and 92.57g of ammonium fluoride, disperse the above powders in a solvent by planetary ball milling, add 400g of isopropanol, and grind for 6h, wherein the ball-to-material mass ratio is 5, the mass of the grinding ball is 1000g, the material of the grinding ball is zirconia ball, and the diameter of the grinding ball is 5mm.

[0231] After grinding, the slurry was dried at 80° C. After drying, a powder agglomerated into a block was obtained, and the powder was ground with a mortar and passed through a 200-mesh sieve.

[0232] The ground and sieved powder was placed in an alumina crucible, heated to 500°C at 2°C / min, kept warm for 6 hours, and then cooled naturally to obtain Li3AlF6 powder material.

[0233] 2. Use 107.49 g of commercial AlPO4 and 92.51 g of the prepared Li3AlF6 by planetary milling at 300 rpm for 10 min to obtain Li3AlF6-AlPO4 mixed powder.

[0234] 3. Preparation of Li3PO4@Li3AlF6-AlPO4 composite powder by microwave heterogeneous precipitation method

[0235] 10g Li3AlF6-AlPO4 powder, 800g deionized water and 0.1g polyethylene glycol dispersant were mixed and ultrasonically dispersed to obtain Li3AlF6-AlPO4 suspension; 0.124g LiOH was added to a double-necked round-bottom flask, and 50g deionized water was added, and the mixture was placed in a laboratory microwave oven and stirred to obtain a LiOH solution; the Li3AlF6-AlPO4 suspension was added to the LiOH solution, and 0.169g H3PO4 was added at the same time, the microwave power was 800W, the reaction temperature was controlled to be 60°C, the mixture was reacted for 10min under stirring, and the mixture was allowed to stand for solid-liquid separation. The obtained powder precipitate was washed with water and centrifuged, and dried in an oven at 50°C to obtain Li3PO4@Li3AlF6-AlPO4 composite powder.

[0236] 4. Commercial graphite and 2 wt.% of Li3PO4@Li3AlF6-AlPO4 powder were used to prepare a composite slurry, and the slurry was dried into (Li3PO4@Li3AlF6-AlPO4)@graphite material by spray drying.

[0237] 5. (Li3PO4@Li3AlF6-AlPO4)@graphite was used as the active material to prepare button cells according to step 7 of Example 1 and then tested.

[0238] Comparative Example 10 (Preparation of Li3PO4@Li3AlF6&AlPO4 by conventional heterogeneous precipitation method)

[0239] 1. Preparation of Li3AlF6 materials

[0240] Weigh 49.81g of lithium acetate, 94.34g of aluminum nitrate and 55.85g of ammonium fluoride, disperse the above powders in a solvent by planetary ball milling, add 400ml of deionized water, and grind for 3h, wherein the ball-to-material mass ratio is 5, the mass of the grinding ball is 1000g, the material of the grinding ball is zirconia ball, and the diameter of the grinding ball is 3mm.

[0241] After grinding, the slurry was dried at 80° C. After drying, a powder agglomerated into a block was obtained, and the powder was ground with a mortar and passed through a 200-mesh sieve.

[0242] The ground and sieved powder was placed in an alumina crucible, heated to 500°C at 4°C / min, kept warm for 6 hours, and then cooled naturally to obtain Li3AlF6 powder material.

[0243] 2. Use 66.85g of commercial AlPO4 and 133.15g of the prepared Li3AlF6 to mix, put into a high-energy ball mill after mixing evenly, control the temperature in the cavity at 25°C, and perform ball milling under argon protective atmosphere. Stop and cool for 10 minutes every 60 minutes. The grinding time is 30 hours, the rotation speed is 1600rpm, the grinding ball mass is 1000g, and the stearic acid is 600g.

[0244] The slurry was dried at 100°C and kept at 400°C for 4 h in an argon atmosphere to obtain Li3AlF6&AlPO4 heterogeneous isomorphs.

[0245] 3. Preparation of Li3PO4@Li3AlF6&AlPO4 composite powder by heterogeneous precipitation method

[0246] 10g Li3AlF6&AlPO4 powder, 500g deionized water and 0.1g polyethylene glycol dispersant were mixed and ultrasonically dispersed to obtain Li3AlF6&AlPO4 suspension; 0.191g Li2CO3 was added to a double-necked round-bottom flask, and 50g deionized water was added, and the mixture was placed in a laboratory water bath heater and stirred to obtain a Li2CO3 solution; the Li3AlF6&AlPO4 suspension was added to the Li2CO3 solution, and 0.228g (NH4)2HPO4 was added at the same time, the water bath temperature was controlled to 70°C, the mixture was reacted for 10min under stirring, and the mixture was allowed to stand for solid-liquid separation. The obtained powder precipitate was washed and centrifuged, and dried in an oven at 50°C to obtain a Li3PO4@Li3AlF6&AlPO4 composite powder;

[0247] The Li3PO4@Li3AlF6&AlPO4 composite powder includes: a Li3AlF6&AlPO4 core with a particle size of 100±20nm; and a Li3PO4 coating layer composited on the outer surface of the Li3AlF6&AlPO4 core with a thickness of about 5nm. At this time, the uniformity of the coating layer is poor.

[0248] 4. Test ionic conductivity

[0249] Take 3g of the powder prepared above. Use a mold with a diameter of 10mm, apply a pressure of 5MPa in a desktop powder tablet press, maintain the pressure for 10min, and then demold to obtain a thin sheet of mixed ion conductor. Place the above thin sheet in a sintering furnace, heat it to 900℃ at 2℃ / min, and keep it warm for 12h. You can get a ceramic sheet of mixed ion conductor. Use 1000-grit sandpaper moistened with alcohol to gently polish the surface of the above ceramic sheet according to the cross-cross method to remove surface impurities and ensure that the thickness of the electrolyte is uniform at all positions. Use a vernier caliper to measure the thickness L of the ceramic sheet, use an ion sputtering instrument to evaporate the gold blocking electrode, and use AC impedance to test the ionic conductivity of the mixed ion conductor, recorded as σ5.

[0250] 5. Test electronic conductivity

[0251] Based on the principle of testing the electronic conductivity of powder by the four-probe method, the electronic conductivity of the mixed ion conductor was tested. 10g of the above mixed ion conductor material Li3PO4@Li3AlF6&AlPO4 was added to the powder resistance tester for testing. The electronic conductivity of the sample was tested at a pressure of 300MPa, which was recorded as ρ5.

[0252] 6. The subsequent steps are consistent with Example 1.

[0253] Comparative Example 11 ((Li3PO4@Li3AlF6-AlPO4-conductive carbon black)@graphite control group)

[0254] 1. Preparation of Li3AlF6 materials

[0255] Weigh 86.25g of lithium nitrate, 21.25g of aluminum oxide and 92.57g of ammonium fluoride, disperse the above powders in a solvent by planetary ball milling, add 400g of isopropanol, and grind for 6h, wherein the ball-to-material mass ratio is 5, the mass of the grinding ball is 1000g, the material of the grinding ball is zirconia ball, and the diameter of the grinding ball is 5mm.

[0256] After grinding, the slurry was dried at 80° C. After drying, a powder agglomerated into a block was obtained, and the powder was ground with a mortar and passed through a 200-mesh sieve.

[0257] The ground and sieved powder was placed in an alumina crucible, heated to 500°C at 2°C / min, kept warm for 6 hours, and then cooled naturally to obtain Li3AlF6 powder material.

[0258] 2. Use 107.49g of commercial AlPO4, 92.51g of the prepared Li3AlF6 and 4g of conductive carbon black and mix them at 300rpm for 10min using a planetary mill to obtain a Li3AlF6-AlPO4-conductive carbon black mixed powder.

[0259] 3. Preparation of Li3PO4@Li3AlF6-AlPO4-conductive carbon black composite powder by microwave heterogeneous precipitation method

[0260] 10g Li3AlF6-AlPO4-conductive carbon black powder, 800g deionized water and 0.1g polyethylene glycol dispersant were mixed and ultrasonically dispersed to obtain Li3AlF6-AlPO4-conductive carbon black suspension; 0.124g LiOH was added to a double-necked round-bottom flask, and 50g deionized water was added, and the mixture was placed in a laboratory microwave oven and stirred to obtain a LiOH solution; the Li3AlF6-AlPO4-conductive carbon black suspension was added to the LiOH solution, and 0.169g H3PO4 was added at the same time, the microwave power was 800W, the reaction temperature was controlled to be 60°C, the mixture was reacted for 10min under stirring, and the mixture was allowed to stand for solid-liquid separation. The obtained powder precipitate was washed with water and centrifuged, and dried in an oven at 50°C to obtain Li3PO4@Li3AlF6-AlPO4-conductive carbon black composite powder.

[0261] 4. Commercial graphite and 2 wt.% of Li3PO4@Li3AlF6-AlPO4-conductive carbon black powder were used to prepare a composite slurry, and the slurry was dried into (Li3PO4@Li3AlF6-AlPO4-conductive carbon black)@graphite material by spray drying.

[0262] 5. (Li3PO4@Li3AlF6-AlPO4-conductive carbon black)@graphite was used as the active material to prepare a button cell according to step 7 of Example 1 and then tested. The test results are shown in Table 1

[0263] Table 1 Performance test results of materials and batteries in Examples and Comparative Examples

[0264]

[0265]

[0266] Embodiment 1-5 is a graphite negative electrode coated with a Li3PO4@Li3AlF6&AlPO4 composite material. After forming a heterogeneous isomorph, the material has electronic conductivity and becomes a mixed ion electronic conductor. Compared with the comparative example, the electronic conductivity is significantly superior. The thin layer of Li3PO4 uniformly coated on the surface can increase the desolvation rate of lithium ions. Therefore, it can effectively promote the lithium ion transmission kinetics on the negative electrode surface, reduce polarization, and significantly improve the cycle performance and rate performance of the battery. At the same time, the coating layer reduces the side reaction between the electrolyte and the negative electrode, which improves the first effect. Comparative Example 1 is a blank graphite group, and its overall performance is lower than that of each embodiment; Comparative Example 2 is Li3AlF6-coated graphite, which lacks the synergistic effect of electronic conductivity and the desolvation effect of Li3PO4, and has poor performance; Comparative Example 3 is AlPO4-coated graphite, AlPO4 does not have ionic conductivity and electronic conductivity, and can only inhibit side reactions to a certain extent, and has poor performance; Comparative Example 4 is Li3PO4-coated graphite, Li3PO4 does not have electronic conductivity, but has a certain ionic conductivity, and its ability to promote lithium ion migration is limited, and its performance is poor; Comparative Example 5 is (Li3AlF6&AlPO4)-coated graphite, which lacks a thin coating layer of Li3PO4 and cannot increase the desolvation rate of lithium ions, and has poor performance; Comparative Example 6 is (Li3AlF6-AlPO4)-coated graphite, Li3AlF6 and AlPO4 are simply mixed, and no heterogeneous isomorphs are formed, and they do not have electronic conductivity. conductivity, and the performance is poor; Comparative Examples 7-9 are (Li3PO4@Li3AlF6) coated graphite, (Li3PO4@AlPO4) coated graphite and (Li3PO4@(Li3AlF6-AlPO4)) coated graphite, respectively, which lack the synergistic effect of electronic conductivity and have poor performance; Comparative Example 10 uses a conventional water bath heated heterogeneous precipitation when coating Li3PO4 on the surface of Li3AlF6&AlPO4, and the uneven local temperature distribution leads to different degrees of reaction in each area, and the coated Li3PO4 is uneven, which hinders the lithium ion dissolution ability; Comparative Example 11 does not generate electronic conductivity of the raw material by forming a heterogeneous isomorph, but by adding a conductive substance to make the material have electronic conductivity, resulting in poor contact between the ion conductors. At the same time, the interlaced network constructed as a split ion conductor and an electronic conductor is inferior to the mixed ion electronic conductor.

[0267] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. An additive material for a negative electrode of a lithium ion battery, It is characterized in that It includes a core and a coating layer, wherein the core is made of Li 3 AlF 6 and AlPO 4 The heterogeneous isomorph constructed, the coating layer is Li 3 PO 4 .

2. The additive material according to claim 1, It is characterized in that Said by Li 3 AlF 6 and AlPO 4 The preparation method of the constructed heteromeric isomers comprises the following steps: Under protective atmosphere, Li 3 AlF 6 and AlPO 4 After high-energy ball milling, the mixture is dried and calcined to obtain Li 3 AlF 6 and AlPO 4 Constructed heterogeneous isoforms.

3. The additive material according to claim 2, It is characterized in that The Li 3 AlF 6 and AlPO 4 The molar ratio is 1:(2-3); The protective atmosphere condition is argon; During the high energy ball milling, the amount of grinding balls added is equal to Li 3 AlF 6 and AlPO 4 The mass ratio of the total amount of the grinding solvent is (5-10):

1. 3 AlF 6 and AlPO 4 The mass ratio of the total amount is (3-4):1, and the grinding solvent is stearic acid; The temperature of the high energy ball mill is 25-35°C, the time of the high energy ball mill is 30-40h, and the speed of the high energy ball mill is 1600-1800rpm; The drying temperature is 100-200°C; The calcination atmosphere is argon atmosphere, the calcination temperature is 400-500° C., and the calcination time is 4-6 hours.

4. The additive material according to claim 1, It is characterized in that Said by Li 3 AlF 6 and AlPO 4 The particle size of the constructed heterogeneous isomorph is 100±20 nm, and the thickness of the coating layer is 5-10 nm.

5. A method for preparing the additive material for lithium ion battery negative electrode according to any one of claims 1 to 4, It is characterized in that The following steps are involved: A) Will be by Li 3 AlF 6 and AlPO 4 The constructed heterogeneous isomer, water and a dispersant are mixed in a mass ratio of 10:(500-1000):(0.1-0.3) to obtain a suspension; B) mixing a lithium compound, a phosphoric acid compound and a suspension to react, and after the reaction is completed, standing and separating the solid and the liquid to obtain an additive material for a negative electrode of a lithium ion battery.

6. The preparation method according to claim 5, It is characterized in that In step A), the dispersant is selected from one of polyethylene glycol, polyacrylamide, methylpentanol and triethylhexyl phosphoric acid.

7. The preparation method according to claim 5, It is characterized in that In step B), the lithium compound is selected from LiOH, Li 2 CO 3 , CH 3 One or more of COOLi; The phosphoric acid compound is selected from H 3 PO 4 NH 4 H 2 PO 4 NH 4 ) 2 HPO 4 One or more of; Said by Li 3 AlF 6 and AlPO 4 The mass ratio of the constructed isomers, lithium compounds, and phosphoric acid compounds is 10:(0.124-0.512):(0.169-0.253); The reaction is a microwave heating reaction, the microwave power is 800-1000W, the reaction temperature is 60-80°C, and the reaction time is 10-20min.

8. A negative electrode material, It is characterized in that The invention comprises a negative electrode active material and an additive material coated on the surface of the negative electrode active material, wherein the additive material is selected from the additive material for the negative electrode of a lithium ion battery according to any one of claims 1 to 4.

9. The negative electrode material according to claim 8, It is characterized in that The negative electrode active material is selected from one or more of graphite, silicon-carbon material, and silicon-oxygen material; The mass ratio of the negative electrode active material to the additive material is 49-99.

10. A method for preparing the negative electrode material according to claim 8 or 9, It is characterized in that The following steps are involved: preparing a composite slurry of negative electrode active material and additive material; The composite slurry is spray-dried to obtain a negative electrode active material coated with the additive material.

11. A lithium ion battery, It is characterized in that Comprising the negative electrode material according to claim 8 or 9.

Citation Information

Cited By

  • Solid electrolyte, electrode material, and battery

    WO2026140603A1

  • Solid electrolyte, electrode material, and battery

    WO2026172651A1