FeCoNi medium-entropy alloy loaded carbon nanofiber aerogel as well as preparation method and application thereof
Through the carbon nanofiber aerogel loaded with FeCoNi entropy alloy, the problem of single loss mechanism and impedance mismatch in the existing electromagnetic wave material is solved, and efficient electromagnetic wave absorption performance is achieved, showing low density, low cost and excellent impedance matching. The capability has opened up a new way for carbon-based high-performance electromagnetic wave absorption materials.
Patent Information
- Application Number
- CN202411099981.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
AI Technical Summary
The loss mechanism of existing electromagnetic wave materials is single and the impedance is mismatched, resulting in poor absorption performance.
Using carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy, bacterial cellulose hydrogel precursors loaded with Fe, Co, Ni metal ions were synthesized and annealed to prepare Get CA@FeCoNi composite material. This method uniformly introduces FeCoNi metal nanoparticles into the carbon nanofiber matrix, optimizes impedance matching, and improves electromagnetic wave absorption performance through a synergistic action of multiple loss mechanisms.
CA@FeCoNi composite material exhibits excellent electromagnetic wave absorption performance, has low density, low cost, high attenuation constant and excellent impedance matching ability. With a low filler content of 5 wt%, its minimum reflection loss reaches -56.7dB, and its effective bandwidth It is 5.28GHz, which significantly improves electromagnetic wave absorption performance.
Smart Images

Figure CN119012669A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electromagnetic wave absorbing materials, and in particular to a carbon nanofiber aerogel loaded with a FeCoNi medium-entropy alloy, and a preparation method and application thereof. Background Art
[0002] In recent decades, with the rapid development of modern electromagnetic technology, while bringing convenience and speed to people's lives, it also generates a large amount of electromagnetic radiation, causing serious electromagnetic wave pollution, which not only has adverse effects on the human body, but also interferes with the normal operation of electronic equipment. In order to solve these problems, it is very important to develop and prepare new materials with good electromagnetic wave absorption performance.
[0003] Carbon-based materials are considered to have the potential to become a new generation of high-performance electromagnetic wave absorption materials due to their simple manufacturing process, high cost-effectiveness and light weight. Among various carbon materials, carbon-based aerogels have attracted increasing attention due to their advantages such as low density, high specific surface area and excellent chemical stability. The constituent units of these materials have many unique structures, such as 0D nanoparticles, 1D nanofibers, 2D nanosheets and 3D network structures. In the field of electromagnetic wave absorption, the 3D network structure has extremely low volume density and thermal conductivity due to its porosity, and is conducive to the penetration of electromagnetic waves, thereby reducing surface reflection. In addition, the three-dimensional interconnected structure inside the material causes multiple scattering of the incident electromagnetic wave, while the abundant air / carbon heterogeneous interface causes significant attenuation of the electromagnetic wave, and the interface polarization and dielectric relaxation are intensified. For example, Gu et al. prepared grapefruit peel aerogels with a porous network structure by freeze-drying and calcination processes, and the minimum reflection loss (RLmin) value of its absorption performance reached -29.50dB. However, the relatively single loss mechanism of carbon-based aerogels limits its performance improvement. At the same time, impedance mismatch also has an adverse effect on its electromagnetic wave absorption capacity. Therefore, coupling pure carbon materials with other materials to optimize impedance matching and introduce multiple loss mechanisms has become a research hotspot for developing high-performance electromagnetic wave absorption materials.
[0004] The introduction of magnetic metals or magnetic metal oxides can optimize impedance matching while increasing magnetic losses. In addition, the generation of abundant heterogeneous interfaces induces a significant interface polarization effect and improves the polarization relaxation response, which plays a key role in stimulating excellent electromagnetic absorption performance. Therefore, the combination of pure carbon materials with magnetic materials has become an effective method to improve the electromagnetic wave absorption performance.
[0005] Compared with single magnetic metals or magnetic oxides, the high configurational entropy and lattice distortion of medium-entropy alloys lead to a more complex microstructure, which promotes more efficient electromagnetic wave scattering and absorption. In addition, compared with the loss mechanism of single magnetic metals that mainly relies on magnetic loss, medium-entropy alloys can absorb electromagnetic waves through the synergistic action of multiple mechanisms including magnetic loss and electrical loss. However, there are few reports on the technology of in-situ loading of medium-entropy alloy nanoparticles. Summary of the invention
[0006] 1. Technical issues to be resolved
[0007] In view of the shortcomings of the prior art, the present invention provides a carbon nanofiber aerogel loaded with FeCoNi medium-entropy alloy and a preparation method and application thereof, which solves the technical problems of poor wave absorption performance caused by the single loss mechanism and impedance mismatch of existing electromagnetic wave materials.
[0008] (II) Technical solution
[0009] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0010] Carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy, bacterial cellulose was used as a carrier and carbon source to synthesize a bacterial cellulose hydrogel precursor loaded with Fe, Co, and Ni metal ions, and then the bacterial cellulose hydrogel precursor was annealed to obtain CA@FeCoNi.
[0011] The preparation method of carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy specifically comprises the following steps:
[0012] S1. Purification of bacterial cellulose
[0013] The bacterial cellulose was boiled in a sodium hydroxide solution and washed with distilled water until it became neutral to obtain a pure bacterial cellulose hydrogel;
[0014] S2. Preparation of metal ion loaded bacterial cellulose hydrogel precursor
[0015] The pure bacterial cellulose hydrogel was immersed in a mixed solution of Fe, Co, and Ni metal salts to fully absorb Fe 3+ 、Co 2+ 、Ni 2+ , and using liquid nitrogen for directional freeze drying to obtain a bacterial cellulose hydrogel precursor loaded with metal ions;
[0016] Preparation of S3.CA@FeCoNi
[0017] The precursor is subjected to high temperature annealing treatment to obtain the final product, carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy, namely CA@FeCoNi.
[0018] The carbon nanofiber aerogel loaded with FeCoNi medium-entropy alloy as described above or the carbon nanofiber aerogel prepared by the preparation method of the carbon nanofiber aerogel loaded with FeCoNi medium-entropy alloy as described above is applied in the field of electromagnetic wave absorption.
[0019] (III) Beneficial effects
[0020] The present invention provides a carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy and a preparation method and application thereof. Compared with the prior art, it has the following beneficial effects:
[0021] 1. FeCoNi metal nanoparticles are uniformly introduced into the carbon nanofiber matrix, and Fe-Co-Ni cooperates synergistically to effectively optimize and enhance the impedance matching of CA@FeCoNi. CA@FeCoNi exhibits excellent performance in the field of electromagnetic wave absorption by utilizing the synergistic effect of electromagnetic composite loss mechanism, rich heterogeneous interface, periodic ordered conductive network and three-dimensional porous structure.
[0022] 2. CA@FeCoNi composite material has low density, low cost, high attenuation constant and excellent impedance matching ability, which enhances the dissipation ability of electromagnetic waves. In addition, it also exhibits multiple dissipation mechanisms, including polarization loss caused by heterogeneous interface, dipole polarization caused by heteroatom doping, and optimized conduction loss caused by the presence of periodic ordered conductive network, which makes CA@FeCoNi have excellent electromagnetic wave absorption performance. At a low filler content of 5wt%, the minimum reflection loss of CA@FeCoNi is -56.7dB and the effective bandwidth is 5.28GHz. The results show that CA@FeCoNi composite material has opened up a new way for the widespread application of carbon-based high-performance electromagnetic wave absorption materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0024] Figure 1(a) and (b) are SEM images of CA@FeCoNi prepared in Example 1 at different magnifications, (c) and (d) are TEM images of CA@FeCoNi prepared in Example 1 at different magnifications, and (e) is a HRTEM image of CA@FeCoNi prepared in Example 1;
[0025] Figure 2 Schematic diagram of the process for preparing the CA@FeCoNi composite material in Example 1 of the present invention;
[0026] Figure 3 is the XRD diagram of the CA@FeCoNi composite material in Example 1 of the present invention;
[0027] Figure 4 This is the minimum reflection loss diagram of CA@FeCoNi in Example 1 of the present invention;
[0028] Figure 5 It is the minimum reflection loss diagram of CA, CA@Fe, CA@Co and CA@Ni in the comparative example of the present invention;
[0029] Figure 6 It is the minimum reflection loss diagram of CA@FeCo, CA@FeNi and CA@CoNi in the comparative example of the present invention;
[0030] Figure 7 This is the minimum reflection loss diagram of CA@FeCoNi (-20°C) prepared using traditional freeze-drying technology in the comparative example of the present invention. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] The embodiments of the present invention provide a carbon nanofiber aerogel loaded with FeCoNi medium-entropy alloy and a preparation method and application thereof, thereby solving the technical problems of poor absorption performance caused by the single loss mechanism and impedance mismatch of existing electromagnetic wave materials. The prepared CA@FeCoNi is applied to the electromagnetic wave field and has excellent absorption performance.
[0033] The general idea of the present invention is: first prepare a 3+ ,Co 2+ and Ni 2+The cellulose hydrogel is immersed in a salt mixed solution of ions, and the washed and purified bacterial cellulose hydrogel is immersed in it. Through the electrostatic attraction between the large number of hydroxyl functional groups contained in it and the metal ions, liquid nitrogen is used for directional freeze drying, and the precursor is obtained after drying; the precursor is placed in a tubular furnace and annealed at high temperature in an argon / hydrogen flow to obtain an ordered structure carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy in situ for electromagnetic wave absorption. The obtained ordered structure carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy retains the advantages of light density of carbon materials, while also introducing magnetic loss and unique medium entropy effect, and has relatively excellent electromagnetic wave absorption characteristics, solving the drawbacks of existing technologies.
[0034] Carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy, bacterial cellulose was used as a carrier and carbon source to synthesize a bacterial cellulose hydrogel precursor loaded with Fe, Co, and Ni metal ions, and then the bacterial cellulose hydrogel precursor was annealed to obtain CA@FeCoNi.
[0035] The interior of CA@FeCoNi is carbon nanofibers arranged in a periodic and orderly structure, and FeCoNi alloy particles are embedded on the surface of the carbon nanofibers.
[0036] The preparation method of carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy specifically comprises the following steps:
[0037] S1. Purification of bacterial cellulose
[0038] The bacterial cellulose was boiled in a sodium hydroxide solution and washed with distilled water until it became neutral to obtain a pure bacterial cellulose hydrogel;
[0039] S2. Preparation of metal ion loaded bacterial cellulose hydrogel precursor
[0040] The pure bacterial cellulose hydrogel was immersed in a mixed solution of Fe, Co, and Ni metal salts to fully absorb Fe 3+ 、Co 2+ 、Ni 2+ , and using liquid nitrogen for directional freeze drying to obtain a bacterial cellulose hydrogel precursor loaded with metal ions;
[0041] Preparation of S3.CA@FeCoNi
[0042] The precursor is subjected to high temperature annealing treatment to obtain the final product, carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy, namely CA@FeCoNi.
[0043] In some embodiments, the concentration of the sodium hydroxide solution in S1 is 1-5 wt %.
[0044] In some embodiments, the immersion time of the precursor in S2 is 24-96 hours.
[0045] In some embodiments, the Fe, Co, and Ni metal salts in S3 are Fe(NO3)3·9H2O, Co(NO3)2·6H2O, and Ni(NO3)2·6H2O, respectively.
[0046] In some embodiments, the total metal content in the mixed solution in S3 is 0.01-0.05 mol / L, wherein the molar ratio of Fe(NO3)3·9H2O, Co(NO3)2·6H2O and Ni(NO3)2·6H2O is 1:1:1.
[0047] In some embodiments, the precursor in S3 is subjected to high temperature annealing treatment under an argon / hydrogen gas flow, wherein the argon / hydrogen gas flow includes 1-10% H2 and 90-99% Ar.
[0048] In some embodiments, the specific operation of high temperature annealing of the precursor in S3 is: heating from room temperature to 200-600°C at a rate of 1-5°C / min, keeping warm for 1-5 hours, then heating to 700-1000°C at a rate of 2-10°C / min, keeping warm for 1-5 hours, and then naturally cooling to room temperature.
[0049] Example 1
[0050] The ordered structure carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy, the preparation method thereof is as follows Figure 2 As shown, specifically including:
[0051] S1. Purification of bacterial cellulose:
[0052] Prepare a 1.5 wt% sodium hydroxide solution, put the bacterial cellulose in it, boil the sodium hydroxide solution, purify the bacterial cellulose and wash away its impurities, and wash with deionized water until the pH is 7.0;
[0053] S2. Preparation of FeCoNi-loaded bacterial fiber hydrogel precursor:
[0054] Prepare a multi-metal mixed solution with a total metal concentration of 0.02 mol / L, of which Fe 3+ ,Co 2+ and Ni 2+ The molar ratio is 1:1:1;
[0055] Weigh 0.0847g Fe(NO3)3·9H2O, 0.1018g Co(NO3)2·6H2O, and 0.1018g Ni(NO3)2·6H2O respectively and place them in a beaker with 50ml deionized water, and stir them magnetically until they are completely dissolved, thereby obtaining a multi-metal mixed solution;
[0056] The purified bacterial cellulose was immersed in a multi-metal mixed solution for 48 hours to allow the hydroxyl functional groups on the surface of the nanofibers to fully absorb the metal ions;
[0057] The metal-filled bacterial cellulose hydrogel was then freeze-casted in liquid nitrogen (-196°C) and finally dried at -80°C and 1Pa to obtain a dry precursor.
[0058] S3. Preparation of CA@FeCoNi
[0059] The completely dried precursor is placed in a porcelain boat, which is placed in a tubular furnace and then an argon-hydrogen flow (5% hydrogen and 95% argon) is introduced. The temperature is raised from room temperature to 400°C at a rate of 2°C / min, and then kept at this temperature for two hours. The temperature is then raised to 800°C at a rate of 5°C / min, and after being kept at this temperature for two hours, the temperature is naturally cooled to room temperature to obtain an ordered structure carbon nanofiber aerogel loaded with FeCoNi medium-entropy alloy, namely CA@FeCoNi.
[0060] CA@FeCoNi morphology characterization Figure 1 As shown, it can be seen that the originally disordered fiber structure inside it forms a periodic ordered structure under the physical confinement of the directional growth of ice crystals during the directional freeze casting process, and still maintains the integrity of the morphology after high-temperature annealing.
[0061] Figure 3 The XRD patterns in Figure 4 demonstrate the formation of entropy alloy nanoparticles in FeCoNi.
[0062] like Figure 4 As shown in (a) and (b) in the figure, the prepared CA@FeCoNi has a minimum reflection loss of -56.7dB in the range of 2-18GHz, and an effective absorption bandwidth of 5.28GHz.
[0063] Example 2
[0064] The ordered structure carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy, the preparation method thereof is as follows Figure 2 As shown, specifically including:
[0065] S1. Purification of bacterial cellulose:
[0066] Prepare a 2.5 wt% sodium hydroxide solution, put the bacterial cellulose in it, boil the sodium hydroxide solution, purify the bacterial cellulose and wash away its impurities, and wash with deionized water until the pH is 7.0;
[0067] S2. Preparation of FeCoNi-loaded bacterial fiber hydrogel precursor:
[0068] Prepare a multi-metal mixed solution with a total metal concentration of 0.01 mol / L, of which Fe 3+ ,Co 2+ and Ni 2+ The molar ratio is 1:1:1;
[0069] Weigh 0.0847g Fe(NO3)3·9H2O, 0.1018g Co(NO3)2·6H2O, and 0.1018g Ni(NO3)2·6H2O respectively and place them in a beaker with 50ml deionized water, and stir them magnetically until they are completely dissolved, thereby obtaining a multi-metal mixed solution;
[0070] The purified bacterial cellulose was immersed in a multi-metal mixed solution for 24 hours to allow the hydroxyl functional groups on the surface of the nanofibers to fully absorb the metal ions;
[0071] The metal-filled bacterial cellulose hydrogel was then freeze-casted in liquid nitrogen (-196°C) and finally dried at -80°C and 1Pa to obtain a dry precursor.
[0072] S3. Preparation of CA@FeCoNi
[0073] The completely dried precursor is placed in a porcelain boat, which is placed in a tubular furnace and then an argon-hydrogen flow (5% hydrogen and 95% argon) is introduced. The temperature is raised from room temperature to 200°C at a rate of 1°C / min, and after being kept warm for 1 hour, the temperature is raised to 700°C at a rate of 2°C / min. After being kept warm for 5 hours, the temperature is naturally cooled to room temperature to obtain an ordered structure carbon nanofiber aerogel loaded with FeCoNi medium-entropy alloy, namely CA@FeCoNi.
[0074] Example 3
[0075] The ordered structure carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy, the preparation method thereof is as follows Figure 2 As shown, specifically including:
[0076] S1. Purification of bacterial cellulose:
[0077] Prepare a 5wt% sodium hydroxide solution, put the bacterial cellulose in it, boil the sodium hydroxide solution, purify the bacterial cellulose and wash away its impurities, and wash with deionized water until the pH is 7.0;
[0078] S2. Preparation of FeCoNi-loaded bacterial fiber hydrogel precursor:
[0079] Prepare a multi-metal mixed solution with a total metal concentration of 0.05 mol / L, of which Fe 3+ ,Co 2+ and Ni 2+ The molar ratio is 1:1:1;
[0080] Weigh 0.0847g Fe(NO3)3·9H2O, 0.1018g Co(NO3)2·6H2O, and 0.1018g Ni(NO3)2·6H2O respectively and place them in a beaker with 50ml deionized water, and stir them magnetically until they are completely dissolved, thereby obtaining a multi-metal mixed solution;
[0081] The purified bacterial cellulose was immersed in a multi-metal mixed solution for 96 hours to allow the hydroxyl functional groups on the surface of the nanofibers to fully absorb the metal ions.
[0082] The metal-filled bacterial cellulose hydrogel was then freeze-casted in liquid nitrogen (-196°C) and finally dried at -80°C and 1Pa to obtain a dry precursor.
[0083] S3. Preparation of CA@FeCoNi
[0084] The completely dried precursor is placed in a porcelain boat, which is placed in a tubular furnace and then an argon-hydrogen flow (5% hydrogen and 95% argon) is introduced. The temperature is raised from room temperature to 600°C at a rate of 5°C / min, and then kept at this temperature for 5 hours. The temperature is then raised to 1000°C at a rate of 10°C / min, and after being kept at this temperature for 1 hour, the temperature is naturally cooled to room temperature to obtain an ordered structure carbon nanofiber aerogel loaded with FeCoNi medium-entropy alloy, namely CA@FeCoNi.
[0085] Example 4
[0086] The carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy prepared in Example 1-3 is applied in the field of electromagnetic wave absorption.
[0087] Comparative Example 1
[0088] The purified bacterial cellulose is not immersed in a multi-metal mixed solution, but directly subjected to directional freeze drying and high temperature annealing. The directional freeze drying and high temperature annealing process is consistent with that in Example 1, and the obtained electromagnetic wave absorbing material is marked as CA.
[0089] like Figure 5 As shown in (a) and (b), its minimum reflection loss is -9.5dB and the effective absorption bandwidth is 0GHz.
[0090] Comparative Example 2
[0091] The multi-metal mixed solution in Example 1 was changed to a single metal solution with a total metal content of 0.02 mol / L, 0.404 g Fe(NO3)3·9H2O was weighed into 50 ml deionized water, and the other steps remained unchanged. The obtained electromagnetic wave absorbing material was marked as CA@Fe.
[0092] like Figure 5 As shown in (c) and (d), its minimum reflection loss is -21.5dB and the effective absorption bandwidth is 4.4GHz.
[0093] Comparative Example 3
[0094] The multi-metal mixed solution in Example 1 was changed to a single metal solution with a total metal content of 0.02 mol / L, 0.291 g Co(NO3)2·6H2O was weighed into 50 ml deionized water, and the other steps remained unchanged. The obtained electromagnetic wave absorbing material was marked as CA@Co.
[0095] like Figure 5 As shown in (e) and (f), its minimum reflection loss is -36.7dB and the effective absorption bandwidth is 6.48GHz.
[0096] Comparative Example 4
[0097] The multi-metal mixed solution in Example 1 was changed to a single metal solution with a total metal content of 0.02 mol / L, 0.291 g Ni(NO3)2·6H2O was weighed into 50 ml deionized water, and the other steps remained unchanged. The obtained electromagnetic wave absorbing material was marked as CA@Ni.
[0098] like Figure 5 As shown in (g) and (h), its minimum reflection loss is -25.7dB and the effective absorption bandwidth is 6GHz.
[0099] Comparative Example 5
[0100] The multi-metal mixed solution in Example 1 was changed to a bimetallic mixed solution with a total metal content of 0.02 mol / L, and 0.202 g Fe(NO3)3·9H2O and 0.1455 g Co(NO3)2·6H2O were weighed into 50 ml deionized water respectively. The other steps remained unchanged, and the obtained electromagnetic wave absorbing material was marked as CA@FeCo.
[0101] like Figure 6 As shown in (a) and (b), its minimum reflection loss is -43.3dB and the effective absorption bandwidth is 5.44GHz.
[0102] Comparative Example 6
[0103] The multi-metal mixed solution in Example 1 was changed to a bimetallic mixed solution with a total metal content of 0.02 mol / L, and 0.202 g Fe(NO3)3·9H2O and 0.1454 g Ni(NO3)2·6H2O were weighed into 50 ml deionized water respectively. The other steps remained unchanged, and the obtained electromagnetic wave absorbing material was marked as CA@FeNi.
[0104] like Figure 6 As shown in (c) and (d), its minimum reflection loss is -35.7dB and the effective absorption bandwidth is 5.84GHz.
[0105] Comparative Example 7
[0106] The multi-metal mixed solution in Example 1 was changed to a bimetallic mixed solution with a total metal content of 0.02 mol / L, and 0.1455 g Co(NO3)2·6H2O and 0.1454 g Ni(NO3)2·6H2O were weighed into 50 ml of deionized water respectively. The other steps remained unchanged, and the obtained electromagnetic wave absorbing material was marked as CA@CoNi.
[0107] like Figure 6 As shown in (e) and (f), its minimum reflection loss is -36.6dB and the effective absorption bandwidth is 6.48GHz.
[0108] Comparative Example 8
[0109] In order to verify the advantages of the periodic ordered structure, the drying method in Example 1 was changed from directional freeze casting to traditional freeze drying (-20°C), and the other steps remained unchanged. The obtained electromagnetic wave absorbing material was labeled CA@FeCoNi (-20°C).
[0110] like Figure 7 As shown in (a) and (b), its minimum reflection loss is -24.1dB and the effective absorption bandwidth is 5.04GHz.
[0111] In Example 1 of the present invention, the electromagnetic parameters were obtained using a vector network analyzer. Paraffin wax was uniformly mixed with 5 wt% of the prepared microwave absorbing material, and after being melted by vacuum heating, the samples were pressed into annular coaxial samples with an outer diameter of 7.0 mm, an inner diameter of 3.04 mm, and different thicknesses using a mold, and the electromagnetic parameters were tested using a vector network analyzer (model AV3629D). The minimum reflection loss (RL) at different thicknesses was fitted by the transmission line theory formula.
[0112]
[0113] Among them, Z in and Z0 are the effective input impedance and free space impedance respectively, ε r and μ r are the complex permittivity and complex permeability, respectively, and ε r =ε′-jε",μ r =μ′+jμ"; where ε" is the real part of the complex dielectric constant, ε" is the imaginary part of the complex dielectric constant; μ′ is the real part of the complex magnetic permeability, μ" is the imaginary part of the complex magnetic permeability; f is the frequency, d is the sample thickness, and c is the speed of light in a vacuum.
[0114] This experiment calculated the electromagnetic wave absorption performance of the absorbing material at 1mm, 1.5mm, 2.0mm, 2.5mm, 3.0mm, 3.5mm, 4.0mm, 4.5mm and 5.0mm without metal loading and with different metal loading, and plotted the Figure 3 and Figure 4 .
[0115] Will Figure 3 and Figure 4 By comparison, it can be seen that the CA@FeCoNi provided by the present invention has excellent electromagnetic wave absorption performance, and its performance mainly comes from the following:
[0116] 1. Carbon nanofiber aerogel has a porous structure with a large amount of air in the pores, which has superior impedance matching performance compared with traditional materials. In addition, the Fe-Co-Ni interaction further enhances the impedance matching and promotes more electromagnetic waves to enter the material. When electromagnetic waves penetrate the absorber, the conductive network formed by the one-dimensional carbon nanofibers composed of high-density and uniformly distributed FeCoNi metal nanoparticles is conducive to multiple scattering and reflection of electromagnetic waves.
[0117] 2. In addition, the ordered arrangement of carbon nanofibers achieved by directional freeze drying can establish a continuous conductive network, promote rapid electron transfer and energy dissipation. At the same time, it is conducive to improving the absorption capacity of electromagnetic waves. Moreover, the ordered structure can enhance the impedance matching between the absorber and the free space, thereby reducing electromagnetic wave reflection and absorbing more electromagnetic waves.
[0118] 3. Dipole polarization caused by the introduction of heteroatoms. Under the action of electromagnetic waves, the charge distribution of molecules or atoms in CA@FeCoNi changes, forming transient dipoles. These dipoles then rearrange in response to the external electric field, causing overall polarization, thereby converting electromagnetic wave energy into heat energy. In addition, the defects generated during the high-temperature carbonization process can also act as polarization centers under the alternating electromagnetic field. The polarization relaxation process caused by dipoles and defects helps to improve the electromagnetic wave absorption performance.
[0119] 4. The presence of multiple heterogeneous interfaces leads to strong polarization losses. The prepared CA@FeCoNi composite material exhibits a large number of heterogeneous interfaces between FeCoNi metal nanoparticles, carbon matrix and air. When electromagnetic waves are transmitted to these interfaces, carriers are aggregated and redistributed at the heterogeneous interfaces under the influence of the electromagnetic field, resulting in dielectric relaxation and strong polarization losses. At the same time, Fe-Co-Ni coupling gives CA@FeCoNi excellent magnetic losses, including eddy current losses and natural resonance.
[0120] In summary, compared with the prior art, the present invention has the following beneficial effects:
[0121] 1. FeCoNi metal nanoparticles are uniformly introduced into the carbon nanofiber matrix, and Fe-Co-Ni cooperates synergistically to effectively optimize and enhance the impedance matching of CA@FeCoNi. CA@FeCoNi exhibits excellent performance in the field of electromagnetic wave absorption by utilizing the synergistic effect of electromagnetic composite loss mechanism, rich heterogeneous interface, periodic ordered conductive network and three-dimensional porous structure.
[0122] 2. CA@FeCoNi composite material has low density, low cost, high attenuation constant and excellent impedance matching ability, which enhances the dissipation ability of electromagnetic waves. In addition, it also exhibits multiple dissipation mechanisms, including polarization loss caused by heterogeneous interface, dipole polarization caused by heteroatom doping, and optimized conduction loss caused by the presence of periodic ordered conductive network, which makes CA@FeCoNi have excellent electromagnetic wave absorption performance. At a low filler content of 5wt%, the minimum reflection loss of CA@FeCoNi is -56.7dB and the effective bandwidth is 5.28GHz. The results show that CA@FeCoNi composite material has opened up a new way for the widespread application of carbon-based high-performance electromagnetic wave absorption materials.
[0123] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0124] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy, characterized in that: Using bacterial cellulose as a carrier and carbon source, a bacterial cellulose hydrogel precursor loaded with Fe, Co, and Ni metal ions was synthesized, and then the bacterial cellulose hydrogel precursor was annealed to obtain a carbon nanofiber aerogel loaded with Fe-Co-Ni alloy nanoparticles, namely CA@FeCoNi.
2. The carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy according to claim 1, characterized in that: The CA@FeCoNi contains carbon nanofibers with a periodic and ordered structure, and the FeCoNi alloy particles are embedded on the surface of the carbon nanofibers.
3. A method for preparing a carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy, characterized in that: The specific steps include: S1. Purification of bacterial cellulose The bacterial cellulose was boiled in a sodium hydroxide solution and washed with distilled water until it became neutral to obtain a pure bacterial cellulose hydrogel; S2. Preparation of metal ion loaded bacterial cellulose hydrogel precursor The pure bacterial cellulose hydrogel was immersed in a mixed solution of Fe, Co, and Ni metal salts to fully absorb Fe 3+ 、Co 2+ 、Ni 2+ , and using liquid nitrogen for directional freeze drying to obtain a bacterial cellulose hydrogel precursor loaded with metal ions; Preparation of S3.CA@FeCoNi The precursor is subjected to high temperature annealing treatment to obtain the final product, carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy, namely CA@FeCoNi.
4. The method for preparing the carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy according to claim 3, characterized in that: The concentration of the sodium hydroxide solution in S1 is 1-5 wt %.
5. The method for preparing the carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy according to claim 3, characterized in that: The soaking time in S2 is 24-96h.
6. The method for preparing the carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy according to claim 3, characterized in that: The Fe, Co and Ni metal salts in the S3 are Fe(NO3)3·9H2O, Co(NO3)2·6H2O and Ni(NO3)2·6H2O respectively.
7. The method for preparing the carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy according to claim 3, characterized in that: The total metal content in the mixed solution in S3 is 0.01-0.05 mol / L, wherein the molar ratio of Fe(NO3)3·9H2O, Co(NO3)2·6H2O and Ni(NO3)2·6H2O is 1:1:
1.
8. The method for preparing the carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy according to claim 3, characterized in that: In S3, a high temperature annealing treatment is performed under an argon / hydrogen gas flow, wherein the argon / hydrogen gas flow comprises 1-10% H2 and 90-99% Ar.
9. The method for preparing the carbon nanofiber aerogel loaded with FeCoNi medium entropy alloy according to claim 3, characterized in that: The specific operation of the high temperature annealing in S3 is: heating from room temperature to 200-600°C at a rate of 1-5°C / min, keeping it at that temperature for 1-5 hours, then heating to 700-1000°C at a rate of 2-10°C / min, keeping it at that temperature for 1-5 hours, and then naturally cooling to room temperature.
10. The carbon nanofiber aerogel loaded with FeCoNi medium-entropy alloy as claimed in any one of claims 1 to 2 or the carbon nanofiber aerogel prepared by the method for preparing the carbon nanofiber aerogel loaded with FeCoNi medium-entropy alloy as claimed in any one of claims 3 to 9 is applied in the field of electromagnetic wave absorption.