Liquid composition, prepreg, metal base with resin, wiring board and silica particles

By adjusting the particle size and shape of the silica particles, combining specific solvents and thermosetting resins, the liquid composition is prepared, and the problems of aggregation and unevenness of silica particles in the liquid composition are solved, and the advantages of the metal substrate layer are achieved Adhesiveness and surface smoothness improve the performance of the electrical insulation layer.

CN119013354APending Publication Date: 2024-11-22AGC INC +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380033495.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2023-04-04
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When the existing liquid composition forms an electrically insulating layer, the aggregation and uneven existence of silica particles lead to a decrease in adhesion and water absorption, affecting the performance of the metal substrate layer, and the characteristics of silica particles cannot be sufficient during high filling. The surface smoothness is also affected.

Method used

By adjusting the particle size, specific surface area and shape of silica particles, combining specific solvents and thermosetting resins, liquid compositions are prepared to inhibit particle aggregation and uneven presence, improve viscosity and dispersion, and form excellent cured substances and prepregs , used to manufacture metal substrates and wiring boards with resin.

Benefits of technology

It realizes excellent adhesion to the metal substrate layer, reduces water absorption and dielectric loss, improves the surface smoothness of the molded object and the high filling effect of silica particles, and enhances the low dielectric characteristics of the electrical insulating layer. and high temperature and high humidity resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005078478610000271
    Figure BDA0005078478610000271
  • Figure BDA0005078478610000281
    Figure BDA0005078478610000281
  • Figure BDA0005078478610000291
    Figure BDA0005078478610000291
Patent Text Reader

Abstract

A liquid composition and an application thereof, the liquid composition containing a thermosetting resin and silica particles, and (1) the d50 and the specific surface area of the silica particles are within a specific range, and the viscosity of the composition is within a specific range; (2) the d50 of the silica particles and the product of the specific surface area and d50 are within a specific range, and the silica particles further contain a solvent having a specific surface tension; (3) the silica particles have d50 / d10 in a specific range and further contain a solvent having a specific boiling point and evaporation rate, and the thixotropic ratio of the composition is in a specific range; or (4) the ratio of particles having a particle diameter of 10 [mu] m or more, the coefficient of variation of the particle diameter, and d50 of the silica particles are within specific ranges.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a liquid composition, a prepreg, a metal substrate with a resin, a wiring board, and silica particles. Background Art

[0002] A liquid composition containing a thermosetting resin and silica particles is used to manufacture an electrical insulating layer of a metal-clad laminate that can be processed into a printed wiring board (see Patent Documents 1 and 2). Specifically, a metal-clad laminate having a semi-cured product of the liquid composition laminated on the surface of a metal substrate layer as an electrical insulating layer; a metal-clad laminate having a glass cloth impregnated with a liquid composition as an electrical insulating layer and laminated on the surface of a metal substrate layer. In recent years, the electrical insulating layer of a printed wiring board has been required to have higher properties such as a low dielectric constant, a low dielectric loss tangent, and a low linear expansion coefficient.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2013-212956

[0006] Patent Document 2: Japanese Patent Application Publication No. 2015-36357 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] On the other hand, from the viewpoint of reliability of the wiring board, etc., the liquid composition used to form an electrical insulating layer such as a semi-cured product impregnated with the liquid composition or a glass cloth of the liquid composition is also required to have excellent adhesion to the metal substrate layer when forming a cured product. The silica particles contained in the liquid composition can be expected to improve the properties of the electrical insulating layer formed therefrom, but the effect on the adhesion to the metal substrate layer is not clear in most cases.

[0009] The present inventors have found that the physical properties of the semi-cured product or the impregnated state change depending on the content of the silica particles in the liquid composition and the physical properties of the silica particles, and there is a concern that the adhesion to the metal substrate layer may decrease.

[0010] The problem to be solved by one embodiment of the present disclosure is to provide: a liquid composition and a prepreg capable of forming a cured product having excellent adhesion to a metal substrate layer. The problem to be solved by one embodiment of the present disclosure is to provide: a liquid composition, a cured product, a metal substrate with resin, and a wiring board having excellent adhesion to a metal substrate layer. The problem to be solved by one embodiment of the present disclosure is to provide: silica particles for adjusting the viscosity of a liquid composition having excellent adhesion to a metal substrate layer.

[0011] In addition, the inventors have obtained the following findings: depending on the content of silica particles in the liquid composition, the physical properties of the silica particles, and the shape of the silica particles, aggregation of silica particles occurs in the liquid composition, its semi-cured product, its cured product, etc., the silica particles are unevenly distributed, the water absorption of the semi-cured product, the cured product, etc. increases, and there is a concern that the adhesion is reduced.

[0012] The problem to be solved by one embodiment of the present disclosure is to provide a liquid composition, a prepreg, a metal substrate with a resin, and a wiring board that can suppress the uneven distribution of silica particles and reduce the water absorption when forming a cured product. The problem to be solved by one embodiment of the present disclosure is to provide silica particles for adjusting the viscosity of a liquid composition that can suppress the uneven distribution of silica particles and reduce the water absorption when forming a cured product.

[0013] In addition, in a liquid composition containing a thermosetting resin and silica particles, from the viewpoint of improving the low dielectric properties, high temperature and high humidity resistance, etc. of a molded body formed from the liquid composition, a method of increasing the amount of silica particles added and performing high filling is sometimes adopted. However, the inventors have found that: in this case, the aggregation of the silica particles is improved, the impregnation of the silica particles into the liquid composition is reduced, and sometimes the properties of the silica particles in the molded body cannot be fully utilized.

[0014] An embodiment of the present disclosure aims to provide a liquid composition capable of suppressing aggregation of silica particles, a prepreg, a metal substrate with a resin, and a wiring board using the liquid composition, and silica particles used in the liquid composition.

[0015] In addition, when a formed article such as an electrical insulating layer is produced using a liquid composition containing silica particles, the surface of the formed article is preferably smooth from the viewpoint of reducing transmission loss, etc. On the other hand, silica particles aggregate when preparing the liquid composition, which may affect the surface smoothness of the formed article.

[0016] An embodiment of the present disclosure aims to provide a liquid composition capable of producing a molded product having excellent surface smoothness, a prepreg, a metal substrate with a resin, and a wiring board using the liquid composition, and silica particles used in the liquid composition.

[0017] Solutions for solving problems

[0018] Means for solving the above-mentioned problems include the following aspects.

[0019] <1> A liquid composition comprising: a thermosetting resin and a particle size d50 of 0.5 to 20.0 μm and a specific surface area of ​​0.1 to 3.5 m 2 / g of silica particles, and the viscosity of the liquid composition measured at 25°C and a rotation speed of 1 rpm is 100 to 10000 mPa·s.

[0020] <2> according to <1> The liquid composition, wherein the content of the silica particles is 50 to 400 parts by mass based on 100 parts by mass of the thermosetting resin.

[0021] <3> according to <1> or <2> The liquid composition further contains a solvent, and the solvent contains at least one selected from the group consisting of toluene, cyclohexanone, methyl ethyl ketone and N-methyl-2-pyrrolidone.

[0022] <4> A liquid composition comprising: a thermosetting resin; a median particle size d50 of 0.5 to 20.0 μm and a product of a specific surface area and the median particle size d50 of 2.7 to 5.0 μm·m 2 / g of silica particles; and a solvent having a surface tension of 45 mN / m or less.

[0023] <5> according to <4> The liquid composition, wherein the specific surface area of ​​the silicon dioxide particles is 0.5 to 3.5 m 2 / g.

[0024] <6> according to <4> or <5> In the liquid composition, the content of the silica particles is 10 to 400 parts by mass based on 100 parts by mass of the thermosetting resin.

[0025] <7> according to <4> ~ <6> The liquid composition according to any one of the preceding claims, wherein the solvent comprises at least one selected from the group consisting of toluene, cyclohexanone, methyl ethyl ketone and N-methyl-2-pyrrolidone.

[0026] <8> A liquid composition comprising: a thermosetting resin; silicon dioxide particles having a median particle size d50 of 0.5 to 20.0 μm and a ratio of the median particle size d50 to the 10% particle size d10 of more than 1.0 and less than 5.0; and a solvent having a boiling point of 75° C. or higher and an evaporation rate of 0.3 to 4.0 based on butyl acetate, wherein the thixotropic ratio of the liquid composition calculated by dividing the viscosity measured at a rotation speed of 1 rpm by the viscosity measured at a rotation speed of 60 rpm is less than 3.0.

[0027] <9> according to <8> The liquid composition, wherein the ratio of the median particle size d50 of the silicon dioxide particles to the 10% particle size d10 is 1.2 to 2.4.

[0028] <10> according to <8> or <9> In the liquid composition, the content of the silica particles is 10 to 400 parts by mass based on 100 parts by mass of the thermosetting resin.

[0029] <11> according to <8> ~ <10> The liquid composition according to any one of the preceding claims, wherein the solvent comprises at least one selected from the group consisting of toluene, cyclohexanone, methyl ethyl ketone and N-methyl-2-pyrrolidone.

[0030] <12> A liquid composition comprising: a thermosetting resin and silica particles, wherein the silica particles have a particle size distribution obtained by a Coulter counter method in which the proportion of particles with a particle size of 10 μm or more is less than 500 ppm, a coefficient of variation of the particle size is 30 to 80%, and a median particle size d50 of more than 1.0 μm and less than 5.0 μm.

[0031] <13> according to <12> The liquid composition, wherein the specific surface area of ​​the silicon dioxide particles is 0.1 to 5.0 m 2 / g.

[0032] <14> according to <12> or <13> The liquid composition, wherein the ratio of the silica particles having a particle size of 10 μm or more is 300 ppm or less.

[0033] <15> according to <12> ~ <14> The liquid composition described above further comprises at least one solvent selected from the group consisting of toluene, methyl ethyl ketone, and N-methylpyrrolidone.

[0034] <16> according to <12> ~ <15> The liquid composition described in any one of the above, wherein the content of the silica particles is 10 to 400 parts by mass based on 100 parts by mass of the thermosetting resin.

[0035] <17> according to <1> ~ <16> The liquid composition described above, wherein the thermosetting resin is an epoxy resin, a polyphenylene ether resin or an o-divinylbenzene resin.

[0036] <18> A prepreg comprising: <1> ~ <16> The liquid composition or a semi-cured product thereof as described above; and a fibrous substrate.

[0037] <19> A metal substrate with resin, comprising: <1> ~ <16> The liquid composition or semi-cured product thereof according to any one of the above <18> The prepreg; and a metal substrate layer.

[0038] <20> according to <19> The metal substrate with resin, wherein the metal substrate layer is copper foil.

[0039] <21> according to <20> In the metal substrate with resin, the maximum height roughness Rz of the surface of the copper foil located on the liquid composition, the semi-cured product or the prepreg side is 2 μm or less.

[0040] <22> A wiring board comprising: <1> ~ <16> A cured product of the liquid composition described above; and a metal wiring.

[0041] <23> A silica particle for adjusting the viscosity of a liquid composition containing a thermosetting resin, wherein the average particle size d50 is 0.5 to 20.0 μm and the specific surface area is 0.1 to 3.5 m 2 / g.

[0042] <24> according to <23> The silicon dioxide particles have a specific surface area of ​​0.8 to 2.0 m 2 / g.

[0043] <25> A silica particle is added to a liquid composition containing a thermosetting resin and used, wherein the median particle size d50 is 0.5 to 20 μm and the product of the specific surface area and the median particle size d50 is 2.7 to 5.0 μm·m 2 / g.

[0044] <26> according to <25> The silicon dioxide particles have a specific surface area of ​​0.5 to 3.5 m 2 / g.

[0045] <27> A silica particle for adjusting the thixotropy of a liquid composition containing a thermosetting resin, wherein the median particle size d50 is 0.5 to 20.0 μm and the ratio of the median particle size d50 to the 10% particle size d10 is greater than 1 and less than 5.

[0046] <28> according to <27> The silica particles, wherein the ratio is 1.2 to 2.4.

[0047] <29> A silica particle is used for mixing with a liquid composition containing a thermosetting resin to form a prepreg, wherein the proportion of particles with a particle size of 10 μm or more in the particle size distribution obtained by the Coulter counter method is 500 ppm or less, the coefficient of variation of the particle size is 0.30 to 0.80, and the median particle size d50 exceeds 1.0 μm and is 5.0 μm or less.

[0048] <30> according to <29> The silicon dioxide particles have a specific surface area of ​​0.1 to 5.0 m 2 / g.

[0049] Effects of the Invention

[0050] According to one embodiment of the present disclosure, there are provided: a liquid composition and a prepreg having excellent adhesion to a metal substrate layer when a cured product is formed. According to one embodiment of the present disclosure, there are provided: a metal substrate with a resin and a wiring board having excellent adhesion between a liquid composition or a cured product and a metal substrate layer. According to one embodiment of the present disclosure, there are provided: silica particles for adjusting the viscosity of a liquid composition having excellent adhesion to a metal substrate layer.

[0051] According to one embodiment of the present disclosure, there are provided: a liquid composition, a prepreg, a metal substrate with a resin, and a wiring board that can suppress the uneven distribution of silica particles and reduce the water absorption of a cured product, etc. According to one embodiment of the present disclosure, there are provided: silica particles for adjusting the viscosity of a liquid composition that can suppress the uneven distribution of silica particles and reduce the water absorption of a cured product, etc.

[0052] According to one embodiment of the present disclosure, there are provided: a liquid composition capable of suppressing aggregation of silica particles, a prepreg, a metal substrate with a resin, and a wiring board using the liquid composition, and silica particles used in the liquid composition.

[0053] According to one embodiment of the present disclosure, there are provided: a liquid composition capable of producing a molded product having excellent surface smoothness; a prepreg, a metal substrate with a resin, and a wiring board using the liquid composition; and silica particles used in the liquid composition. DETAILED DESCRIPTION

[0054] The following describes the embodiments of the present disclosure in detail. However, the embodiments of the present disclosure are not limited to the following embodiments. In the following embodiments, the constituent elements (including element steps, etc.) are not required unless specifically indicated. The same is true for numerical values ​​and their ranges, which do not limit the embodiments of the present disclosure.

[0055] In the numerical range expressed by "to" in the present disclosure, the numerical values ​​described before and after "to" are respectively regarded as the minimum value and the maximum value.

[0056] In the present disclosure, each component may include a plurality of corresponding substances. When a plurality of corresponding substances exist in the composition, the content or content of each component refers to the total content or content of the plurality of substances present in the composition unless otherwise specified.

[0057] In the present disclosure, particles corresponding to each component may include multiple types. When multiple types of particles corresponding to each component exist in a composition, the particle size of each component refers to a value for a mixture of the multiple types of particles present in the composition unless otherwise specified.

[0058] In the present disclosure, “silicon dioxide particles” refers to a group of a plurality of silicon dioxide particles unless otherwise specified.

[0059] In the present disclosure, the "median particle size d50 (hereinafter also referred to as "d50")" in the description of the particles contained in the present compositions 1 to 3 described later is the volume-based cumulative 50% diameter of the particles determined by a laser diffraction particle size distribution measuring device (e.g., "MT3300EXII" manufactured by MicrotracBEL Corp.). That is, the particle size distribution is measured by the laser diffraction / scattering method, and a cumulative curve is obtained with the total volume of the particles as 100%, and the particle size at the point where the cumulative volume becomes 50% on the cumulative curve.

[0060] In the present disclosure, d50 in the description of particles contained in the present composition 4 described later is a volume-based cumulative 50% diameter of silica particles obtained from a volume-based particle size distribution obtained by a Coulter counter method.

[0061] In the present disclosure, the "10% particle diameter d10" (hereinafter also referred to as "d10") in the description of the particles contained in the present compositions 1 to 3 described later is the volume-based cumulative 10% diameter of the particles determined by a laser diffraction particle size distribution measuring device (e.g., "MT3300EXII" manufactured by MicrotracBEL Corp.). That is, the particle size distribution is measured by a laser diffraction scattering method, and a cumulative curve is obtained with the total volume of the particles as 100%, and the particle size at the point where the cumulative volume from the smaller particle size side becomes 10% on the cumulative curve.

[0062] In the present disclosure, d10 in the description of particles contained in the present composition 4 described later is a volume-based cumulative 10% diameter of silica particles obtained from a volume-based particle size distribution obtained by a Coulter counter method.

[0063] In the present disclosure, the "ratio of particles with a particle size of 10 μm or more" is the ratio of particles obtained from the particle size distribution based on the number obtained by the Coulter counter method. The number of particles with a particle size of 10 μm or more among 50,000 particles is calculated, and the ratio of particles with a particle size of 10 μm or more to the total number of measured particles (number ppm) is calculated.

[0064] In the present disclosure, the "coefficient of variation" (hereinafter also referred to as "CV value") of particle size is an index of relative fluctuation of particle size, and is a value obtained by dividing the standard deviation of particle size by the average value (d50 of particle size) as a percentage. The standard deviation and average value of particle size are obtained from the volume-based particle size distribution obtained by the Coulter counter method.

[0065] The Coulter counter method is performed using, for example, a precision particle size distribution measuring apparatus Multisizer 4e manufactured by Beckman Coulter.

[0066] In the present disclosure, the “specific surface area” is determined by the BET method based on a nitrogen adsorption method using a specific surface area / pore distribution measuring apparatus (for example, “Tristar II” manufactured by Micromeritics).

[0067] In the present disclosure, "sphericity" is expressed as follows: for any 100 particles in a projection image of a photograph obtained by taking a scanning electron microscope (SEM) photograph, the maximum diameter (DL) and the short diameter (DS) orthogonal thereto are measured, and the average value of the ratio (DS / DL) of the short diameter (DS) to the maximum diameter (DL) is calculated.

[0068] In the present disclosure, the "dielectric loss tangent" and the "dielectric constant" are measured by a resonant method using a dedicated device (for example, "Vector Network Analyzer E5063A" manufactured by Keycom Co., Ltd.).

[0069] In the present disclosure, the term "viscosity" refers to the viscosity at 30 seconds measured at a shear rate of 1 rpm for 30 seconds at 25°C using a rotational rheometer (for example, modular rheometer Physica MCR-301 manufactured by Anton Paar).

[0070] In the present disclosure, the “thixotropic ratio” is calculated by dividing the viscosity measured at a rotation speed of 1 rpm by the viscosity measured at a rotation speed of 60 rpm using a rotational rheometer.

[0071] In the present disclosure, the "weight average molecular weight" is determined by gel permeation chromatography (GPC) in terms of polystyrene.

[0072] In the present disclosure, the "surface tension" is measured using a surface tensiometer according to the Wilhelmy method for a solvent at 25°C.

[0073] In this disclosure, the "boiling point" is 1.013×10 5 Boiling point under Pa.

[0074] In the present disclosure, the “evaporation rate” is a relative evaporation rate when the evaporation rate of butyl acetate at 23° C. is set to 1.

[0075] In the present disclosure, a "liquid composition" refers to a composition that is liquid at 25°C.

[0076] In the present disclosure, "semi-cured product" refers to a cured product of a liquid composition in which an exothermic peak accompanying the curing of a thermosetting resin appears when a cured product of the liquid composition is measured by differential scanning calorimetry. In other words, a semi-cured product refers to a cured product in which uncured thermosetting resin remains.

[0077] In the present disclosure, the term "cured product" refers to a cured product in which the exothermic peak accompanying the curing of the thermosetting resin does not appear when the cured product of the liquid composition is measured by differential scanning calorimetry. In other words, the term "cured product" refers to a cured product in which no uncured thermosetting resin remains.

[0078] In the present disclosure, the maximum height roughness Rz is measured in accordance with JIS B 0601 (2013).

[0079] In the present disclosure, the ten-point average roughness Rzjis is measured in accordance with the ten-point average roughness Rz of JIS B 0601 (1994).

[0080] The liquid composition 1 of the present disclosure (hereinafter also referred to as "the present composition 1") contains a thermosetting resin and a d50 of 0.5 to 20 μm and a specific surface area of ​​0.1 to 3.5 m 2 / g of silica particles, and the viscosity of the liquid composition 1 measured at 25°C and 1 rpm is 100 to 10000 mPa·s. In other words, the present composition 1 is a liquid thermosetting composition.

[0081] The liquid composition 2 of the present disclosure (hereinafter, also referred to as "the present composition 2") comprises: a thermosetting resin; a d50 of 0.5 to 20.0 μm and a product of a specific surface area and d50 of 2.7 to 5.0 μm·m 2 / g of silica particles; and a solvent having a surface tension of 45 mN / m or less. In other words, the present composition 2 is a liquid thermosetting composition.

[0082] The liquid composition 3 disclosed in the present invention (hereinafter, also referred to as "the present composition 3") contains: a thermosetting resin; silica particles having a d50 of 0.5 to 20.0 μm and a ratio of d50 to d10 (hereinafter, also referred to as "d50 / d10") exceeding 1.0 and being 5.0 or less; and a solvent having a boiling point of 75°C or more and an evaporation rate of 0.3 to 4.0, wherein the thixotropic ratio of the liquid composition 3 is 3.0 or less. In other words, the present composition 3 is a liquid thermosetting composition.

[0083] The liquid composition 4 disclosed in the present invention (hereinafter also referred to as the present composition 4) contains: a thermosetting resin and silica particles, wherein the proportion of particles having a particle size of 10 μm or more in the particle size distribution obtained by the Coulter counter method is 500 ppm or less, the coefficient of variation of the particle size is 30 to 80%, and d50 is greater than 1.0 μm and less than 5.0 μm. In other words, the present composition 4 is a liquid thermosetting composition.

[0084] The present composition 1 has excellent adhesion to the metal substrate layer. Its mechanism of action is uncertain, but it is roughly presumed as follows. The present composition 1 contains silica particles having a specific range of d50 and specific surface area. As a result, the wettability of the silica particles contained in the present composition 1 is improved, and their aggregation is suppressed. Therefore, the uniform dispersibility of the silica particles in the present composition 1 is improved, and the viscosity of the composition is limited to a specified range. It is believed that by using the present composition 1 containing silica particles in the above state, the formation of a solidified product in which the uneven presence of silica particles is suppressed is promoted, in other words, the formation of a solidified product in which the silica particles are not excessively exposed on the surface is promoted. As a result, it is believed that the adhesion of the solidified product obtained by the present composition 1 to the metal substrate layer is improved. Hereinafter, the adhesion to the metal substrate layer is referred to as "adhesion".

[0085] The present composition 2 can suppress the uneven distribution of silica particles and reduce the water absorption of the cured product. The mechanism of action is uncertain, but it is roughly estimated as follows. The d50 of the silica particles in the present composition 2 is within a specific range (0.5 to 20.0 μm) and the product of the specific surface area and d50 is within a specific range (2.7 to 5.0 μm·m 2 / g). In other words, the silica particles in the present composition 2 are densely shaped and have a large specific surface area per unit mass, and are also considered to have a particle size of μm-level silica particles. When the above-mentioned silica particles are acted on a solvent having a predetermined low surface tension, the wettability of the silica particles derived from the specific surface area is balanced with the dispersibility derived from the particle size, and it is thus believed that the silica particles are highly uniformly dispersed in the composition. As a result, the uneven presence of the silica particles in the present composition 2 or its cured product is suppressed, and therefore it is estimated that the water absorption rate of the cured product is reduced.

[0086] It was found that the aggregation of silica particles was also suppressed when the present composition 3 was heated and used, showing a high degree of fluidity and impregnation, and the molded product formed therefrom can well exert the silica characteristics. The reason may not be clear, but it is speculated as follows. The low-viscosity solvent improves the impregnation of the particle amount (d10 part) of the silica particles, so it is considered to be conducive to the high filling of silica particles. However, if the particle amount of silica particles is large, the volatilization of the solvent during heating becomes slow, which induces the aggregation of silica particles, and as a result, it is considered that the silica characteristics of the molded product become insufficiently improved. On the other hand, in the present composition 3, the d50 / d10 of the silica particles exceeds 1.0 and is less than 5.0, and then the evaporation rate of the solvent is within the specified range, and the thixotropic ratio is adjusted to within the specified range. In other words, the present composition 3 is in a state where the filling property of the silica particles and the volatility of the solvent are well balanced. This is presumably because aggregation of silica particles in the present composition 3 is suppressed, and therefore, when the present composition 3 is heated and molded into a molded product, aggregation or segregation of silica particles in the molded product can be suppressed, thereby obtaining a molded product that highly utilizes the properties of silica particles.

[0087] According to the present composition 4, a molded product with excellent surface smoothness can be produced. The reason may not be clear, but it is considered as follows. The silica particles in the present composition 4 are silica particles with a constant particle distribution with particles of μm level as the main particles, and the proportion of coarse particles is highly suppressed, and they are also regarded as silica particles containing microparticles in a specified proportion. It is believed that by mixing the above-mentioned silica particles with a thermosetting resin to form a liquid composition, the aggregation of the microparticles themselves and the aggregation of silica particles with coarse particles as the core in the liquid composition are suppressed. The uneven existence of silica particles caused by the aggregation. In addition, it is believed that the microparticles improve the dispersibility of the main particles and improve the interaction between the silica particles and the thermosetting resin. It is also believed that if a molded product is formed by a liquid composition in the above state, the microparticles fill the gaps of the main particles to form a molded product, and therefore, the surface smoothness of the molded product is improved. It is further believed that according to the present composition 4, the aggregation of silica particles can be suppressed and high filling is performed, and the silica physical properties are highly reflected in the molded product.

[0088] The viscosity of the present composition 1 measured at a rotation speed of 1 rpm is 100 to 10000 mPa·s, preferably 130 to 5000 mPa·s, more preferably 150 to 3000 mPa·s, further preferably 180 to 1500 mPa·s, and particularly preferably 200 to 1000 mPa·s. Within this viscosity range, aggregation of silica particles can be more effectively suppressed.

[0089] The viscosity measured at a rotation speed of 1 rpm of the present composition 2 and the present composition 3 is preferably 100 to 10000 mPa·s, more preferably 130 to 5000 mPa·s, further preferably 150 to 3000 mPa·s, particularly preferably 180 to 1500 mPa·s, and most preferably 200 to 1000 mPa·s. Within this viscosity range, aggregation of silica particles can be more effectively suppressed.

[0090] The viscosity of the present composition 4 measured at a rotation speed of 1 rpm is preferably 130 to 5000 mPa·s, more preferably 150 to 3000 mPa·s, further preferably 180 to 1500 mPa·s, and particularly preferably 200 to 1000 mPa·s. Within this viscosity range, aggregation of silica particles can be more effectively suppressed.

[0091] The thixotropic ratio of the present composition 1, the present composition 2 and the present composition 4 is preferably 3.0 or less, more preferably 2.5 or less, and further preferably 2.0 or less. The lower limit of the thixotropic ratio is not particularly limited, but is set to be 0.5 or more. Within this thixotropic ratio range, the ease of storage, state stability and fluidity during use of the present composition 1 become good.

[0092] The thixotropic ratio of the present composition 3 is 3.0 or less, preferably 2.5 or less, and more preferably 2.0 or less from the viewpoint of better suppressing the aggregation of silica particles. The lower limit of the thixotropic ratio is not particularly limited, and 1.0 can be cited. If it is within this thixotropic ratio range, the ease of storage, state stability and fluidity during use of the present composition 1 become good.

[0093] The present composition 1, the present composition 2, the present composition 3 and the present composition 4 contain a thermosetting resin. For each composition, one thermosetting resin may be used, or two or more thermosetting resins may be used in combination. As the thermosetting resin, epoxy resin, polyphenylene ether resin, polyimide resin, phenolic resin, o-divinylbenzene resin, etc. may be cited. From the viewpoints of adhesion, heat resistance, etc., the thermosetting resin is preferably an epoxy resin, a polyphenylene ether resin or an o-divinylbenzene resin. The thermosetting resin preferably contains a resin of at least one selected from the group consisting of phenyl and phenylene.

[0094] Examples of the epoxy resin include bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, alicyclic epoxy resin, phenol novolac epoxy resin, cresol novolac epoxy resin, bisphenol A novolac epoxy resin, diglycidyl ethers of polyfunctional phenols, and diglycidyl ethers of polyfunctional alcohols.

[0095] The polyphenylene ether resin may be a modified polyphenylene ether or an unmodified polyphenylene ether. From the viewpoint of adhesion, a modified polyphenylene ether is preferred. The modified polyphenylene ether has a polyphenylene ether chain or a substituent bonded to the end of the polyphenylene ether chain. The substituent preferably has a reactive group, more preferably a vinyl, (meth)acryloyloxy or epoxy group.

[0096] The hydrogen atoms of the phenylene group in the polyphenylene ether chain may be substituted with an alkyl group, an alkenyl group, an alkynyl group, a formyl group, an alkylcarbonyl group, an alkenylcarbonyl group or an alkynylcarbonyl group.

[0097] The weight average molecular weight of the thermosetting resin is preferably 1,000 to 7,000, more preferably 1,000 to 5,000, and even more preferably 1,000 to 3,000 from the viewpoint of adhesion, dielectric properties, and the like.

[0098] From the viewpoint of adhesion of the prepreg obtained from the present composition 1, the present composition 2, the present composition 3 or the present composition 4 to the metal substrate layer etc. of the wiring board, the content of the thermosetting resin in the present composition 1, the present composition 2, the present composition 3 or the present composition 4 relative to the total mass of each composition is preferably 10 to 40% by mass, more preferably 15 to 35% by mass, and further preferably 20 to 30% by mass.

[0099] The present composition 1 and the present composition 2 contain silica particles having a d50 of 0.5 to 20.0 μm. The d50 of the silica particles in the present composition 1 and the present composition 2 is preferably 1.0 to 10.0 μm, and more preferably more than 1.0 μm and 5.0 μm or less, from the viewpoint of highly balancing the physical properties of the present composition 1 and the present composition 2 themselves, such as dispersion stability, suppression of uneven presence of silica particles, and fluidity, and the physical properties of the molded product formed by the present composition 1 and the present composition 2, such as reduced water absorption, adhesion, and low dielectric loss tangent.

[0100] From the viewpoint of accelerating the above-mentioned mechanism of action and facilitating adjustment of the thixotropic ratio, the d50 of the silica particles in the present composition 3 is 0.5 to 20.0 μm, preferably 1.0 to 10.0 μm, more preferably more than 1.0 μm and 5.0 μm or less. In particular, when the d50 of the silica particles is 0.5 μm or more, aggregation of the silica particles can be suppressed.

[0101] The d50 of the silica particles in the present composition 4 is more than 1.0 μm and is 5.0 μm or less, and is preferably 1.5 to 4.0 μm, and more preferably 2.0 to 3.5 μm, from the viewpoint of suppressing aggregation of the silica particles and excellent surface smoothness of the molded product.

[0102] From the viewpoint of improving uniform dispersibility in the present composition 1, the present composition 2, and the present composition 4 and enhancing the interaction between the silica particles and the thermosetting resin, the d10 of the silica particles is preferably 0.5 to 5.0 μm, more preferably 1.0 to 3.0 μm.

[0103] From the viewpoint of accelerating the above-mentioned action mechanism and facilitating adjustment of the thixotropic ratio, d10 of the silica particles in the present composition 3 is preferably 0.2 to 10.0 μm, more preferably 0.5 to 5.0 μm, and even more preferably 1.0 to 2.5 μm.

[0104] From the viewpoint of achieving a more highly balanced physical property of the present composition 1 or the present composition 2 itself, such as dispersion stability and fluidity, and the physical property of a molded product formed from the present composition 1 or the present composition 2, such as adhesion and low dielectric loss tangent, the specific surface area of ​​the silica particles in the present composition 1 and the present composition 2 is preferably 0.3 to 3.0 m 2 / g, more preferably 0.8 to 2.0 m 2 / g.

[0105] From the viewpoint of further suppressing the aggregation of silica particles and making the present composition 3 more stable, the specific surface area of ​​the silica particles in the present composition 3 is preferably 0.1 to 3.5 m 2 / g, more preferably 0.3 to 3.0 m 2 / g, more preferably 0.8 to 2.0 m 2 / g.

[0106] From the viewpoint of the above-mentioned mechanism of action, in particular, of suppressing the aggregation of silica particles, the specific surface area of ​​the silica particles in the present composition 4 is preferably 0.1 to 5.0 m 2 / g, more preferably 0.2 to 3.5 m 2 / g, more preferably 0.3 to 3.0 m 2 / g, particularly preferably 0.6 to 2.4 m 2 / g, most preferably 0.8 to 2.0 m 2 In this case, the wettability of the silica particles is particularly improved, and the above-mentioned mechanism of action is likely to be manifested significantly.

[0107] From the viewpoint of improving the uniform dispersibility of the silica particles in the present compositions 1, 2 and 4 and enhancing the interaction between the silica particles and the thermosetting resin, the ratio of d50 to d10 (d50 / d10) of the silica particles in the present compositions 1, 2 and 4 is preferably greater than 1.0 and less than 5.0, more preferably 1.3 to 4.0, and still more preferably 1.5 to 3.0.

[0108] The present composition 3 contains silica particles having a d50 / d10 of more than 1.0 and not more than 5.0. From the viewpoint of accelerating the above-mentioned action mechanism and facilitating adjustment of the thixotropic ratio, d50 / d10 is preferably 1.1 to 4.0, more preferably 1.2 to 2.4, and even more preferably 1.3 to 2.2.

[0109] From the viewpoint of reducing the water absorption of the present composition 1, the present composition 2, the present composition 3 and the present composition 4 and their cured products and from the viewpoint of suppressing the aggregation of the silica particles, the product A of the specific surface area of ​​the silica particles and the d50 of the silica particles is preferably 2.7 to 5.0 μm·m 2 / g, more preferably 2.9 to 4.5 μm·m 2 / g.

[0110] The particle size distribution of the silica particles contained in the present composition 1, the present composition 2, the present composition 3 or the present composition 4 is preferably unimodal. The unimodal particle size distribution of the silica particles can be confirmed by the presence of one peak in the particle size distribution by the laser diffraction / scattering method.

[0111] The CV value of the particle size of the silica particles in the present composition 1, the present composition 2 and the present composition 3 is preferably 30 to 80%, more preferably 30 to 70%, further preferably 30 to 60%, and particularly preferably 35 to 55%, from the viewpoint of suppressing aggregation of the silica particles and excellent surface smoothness of the molded product.

[0112] The CV value of the particle size of the silica particles in the present composition 4 is 30 to 80%, preferably 30 to 70%, more preferably 30 to 60%, and further preferably 35 to 55%, from the perspective of the above-mentioned mechanism of action, in particular, suppressing the aggregation of silica particles, and excellent surface smoothness of the molded product.

[0113] Among the silica particles in the present composition 1, the present composition 2 and the present composition 3, the proportion of particles having a particle size of 30 μm or more is preferably 500 ppm or less, and particularly preferably 300 ppm or less, further preferably 200 ppm or less, and particularly preferably 100 ppm or less, from the viewpoint of excellent surface smoothness of the molded product.

[0114] Among the silica particles in the present composition 4, the proportion of particles having a particle size of 10 μm or more is 500 ppm or less, preferably 300 ppm or less, more preferably 200 ppm or less, and further preferably 100 ppm or less from the viewpoint of the above-mentioned mechanism of action and excellent surface smoothness of the molded product. The above-mentioned particle proportion is preferably 0 ppm or more.

[0115] In the present composition 1, the present composition 2, the present composition 3 or the present composition 4, from the viewpoint of highly balancing the physical properties of the present composition 1, the present composition 2, the present composition 3 or the present composition 4 itself, such as dispersion stability and fluidity, with the physical properties of the prepreg or other molded products formed by the present composition 1, the present composition 2, the present composition 3 or the present composition 4, such as high toughness, adhesion to the metal substrate layer, and low dielectric loss tangent, the shape of each silica particle contained in the silica particles is preferably spherical. From the same viewpoint, the sphericity of the spherical silica particles is preferably 0.75 or more, more preferably 0.90 or more, further preferably 0.93 or more, and particularly preferably 1.00. In addition, from the same viewpoint, the silica particles are preferably non-porous particles.

[0116] From the viewpoint of reducing transmission loss in a circuit when the metal substrate with resin is used as a printed wiring board, the dielectric loss tangent of the silica particles is preferably 0.0020 or less, more preferably 0.0010 or less, and further preferably 0.0008 or less at a frequency of 1 GHz.

[0117] From the same viewpoint, the dielectric constant of the silica particles is preferably 5.0 or less, more preferably 4.5 or less, and even more preferably 4.1 or less at a frequency of 1 GHz.

[0118] Each silica particle may be treated with a silane coupling agent. By treating the surface of the silica particle with a silane coupling agent, the residual amount of silanol groups on the surface is reduced, the surface is hydrophobized, moisture adsorption is suppressed, dielectric loss can be improved, and affinity with thermosetting resin is improved, which can improve dispersibility and strength of the resin film.

[0119] Examples of the silane coupling agent include aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, silane coupling agents, and organic silazane compounds. The silane coupling agent may be used alone or in combination of two or more.

[0120] The amount of the silane coupling agent attached is preferably 0.01 to 5 parts by mass, more preferably 0.10 to 2 parts by mass, based on 100 parts by mass of the silica particles.

[0121] Whether the surface of the silica particles is treated with a silane coupling agent can be confirmed by detecting a peak generated by a substituent of the silane coupling agent by IR. Alternatively, the amount of the silane coupling agent attached can be measured by the amount of carbon.

[0122] On the other hand, from the viewpoint of enhancing the interaction between the silica particles and the thermosetting resin and improving the toughness of the molded product, each silica particle may not be surface-treated with a silane coupling agent or the like.

[0123] The silica particles preferably contain 30 to 1500 mass ppm of titanium (Ti), more preferably 100 to 1000 mass ppm, and further preferably 100 to 500 mass ppm. Ti is an arbitrary component contained in the manufacture of silica particles. When the silica particles are manufactured, the generation of fine powders caused by the rupture of the silica particles will increase the specific surface area of ​​the particles. By including Ti during the manufacture of silica particles, it is easy to shrink and shrink during sintering, and the rupture of the particles can be suppressed. As a result, the generation of fine powders can be suppressed, and the attached particles attached to the surface of the mother particles of the silica particles can be reduced, thereby making it easy to adjust the specific surface area of ​​the silica particles. By including more than 30 mass ppm of Ti, it is easy to shrink during sintering, so the generation of fine powders caused by rupture can be suppressed. If the Ti content is less than 1500 mass ppm, the above-mentioned effect is obtained, and the increase in the amount of silanol groups can be suppressed, and the dielectric loss tangent can be increased.

[0124] The silica particles may contain impurity elements other than titanium (Ti) within a range that does not hinder the effects of the present disclosure. As impurity elements, in addition to Ti, for example, Na, K, Mg, Ca, Al, Fe, etc. may be mentioned. The total content of alkali metals and alkaline earth metals in the impurity elements is preferably 2000 mass ppm or less, more preferably 1000 mass ppm or less, and further preferably 200 mass ppm or less.

[0125] The silica particles are preferably silica particles manufactured by a wet method. The wet method refers to a method including a process of using a liquid as a silica source and gelling it to obtain a raw material for the silica particles. By using the wet method, it becomes easy to adjust the shape of the silica particles, especially spherical silica particles, without the need to make the shape of the particles consistent by crushing, etc., and as a result, it is easy to obtain particles with a small specific surface area. In addition, the wet method has a tendency to be difficult to generate particles that are significantly smaller than the average particle size, and the specific surface area tends to become smaller after sintering. In addition, in the wet method, by adjusting the impurities in the silica source, the amount of impurity elements such as titanium can be adjusted, and then a state in which the aforementioned impurity elements are uniformly dispersed in the particles can be formed.

[0126] As wet method, spray method, emulsion / gelation method etc. can be cited. As emulsion / gelation method, for example, dispersed phase and continuous phase containing silica precursor are emulsified, and the obtained emulsion is gelled to obtain spherical silica precursor. As emulsification method, preferably dispersed phase containing silica precursor is supplied to continuous phase by micropore part or porous film so as to make emulsion method. Thus, emulsion with uniform droplet diameter is made, and as a result, spherical silica particles with uniform particle size are obtained. As such emulsification method, micro-mixing method, membrane emulsification method etc. can be cited. For example, micro-mixing method is disclosed in International Publication No. 2013 / 062105.

[0127] The silica particles are obtained by heat treating the aforementioned silica precursor. The heat treatment has the following effects: the spherical silica precursor is sintered to densify the shell, while reducing the amount of silanol groups on the surface to reduce the dielectric loss tangent. The heat treatment temperature is preferably above 700°C. In addition, from the viewpoint of inhibiting the aggregation of particles, the heat treatment temperature is preferably below 1600°C. In addition, the obtained silica particles can be surface treated with a silane coupling agent.

[0128] From the viewpoint of suppressing the uneven existence of silica particles, reducing water absorption, low dielectric loss tangent, adhesion, etc., the content of silica particles in this composition 1, this composition 2, this composition 3 or this composition 4 relative to 100 parts by mass of thermosetting resin is preferably 10 parts by mass or more, more preferably 50 parts by mass or more, further preferably 70 parts by mass or more, particularly preferably 90 parts by mass or more, and can be 100 parts by mass or more. In addition, the aforementioned content is preferably 600 parts by mass or less, more preferably 400 parts by mass or less, further preferably 300 parts by mass or less, and particularly preferably 250 parts by mass or less. In particular, when it is desired to make the silica particles highly filled, the content of the aforementioned silica particles is preferably 80 parts by mass or more, more preferably 90 parts by mass or more, and particularly preferably 100 parts by mass or more. In addition, the content of silica particles at this time is preferably 600 parts by mass or less, more preferably 300 parts by mass or less. Even if the content of the silica particles is large, a molded product having a particularly low water absorption rate can be obtained from the present composition 1, the present composition 2, the present composition 3 or the present composition 4 due to the above-mentioned mechanism of action.

[0129] The silica particles in the present composition 1, the present composition 2, the present composition 3 or the present composition 4 are in a state of being fully wetted and uniformly dispersed, and are in a state of being easily and highly interactive with the thermosetting resin. Therefore, in the present composition in which the silica particles are filled more with respect to the thermosetting resin, both components are easily stabilized, and a molded product having excellent adhesion to the metal substrate layer can be formed.

[0130] The present composition 1, the present composition 2, the present composition 3 or the present composition 4 may contain one or more curing agents. The curing agent is an agent that initiates the curing reaction of the thermosetting resin by the action of heat, and specifically includes α,α'-bis(tert-butylperoxy-m-isopropyl)benzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne, benzoyl peroxide, 3,3',5,5'-tetramethyl-1,4-diphenoquinone, tetrachlorobenzoquinone, 2,4,6-tri-tert-butylphenol, tert-butylperoxyisopropyl monocarbonate, azobisisobutyronitrile, etc. The content of the curing agent is preferably 0.1 to 5 parts by mass relative to 100 parts by mass of the thermosetting resin.

[0131] The present composition 1, the present composition 2, the present composition 3 or the present composition 4 may contain one or more curing accelerators. Examples of the curing accelerator include triallyl isocyanurate compounds such as triallyl isocyanurate, polyfunctional acrylic compounds having two or more acryloyl or methacryloyl groups in the molecule, polyfunctional vinyl compounds having two or more vinyl groups in the molecule, and vinylbenzyl compounds such as styrene having vinylbenzyl groups in the molecule. The content of the curing accelerator is preferably 10 to 100 parts by mass relative to 100 parts by mass of the thermosetting resin.

[0132] The present composition 1 and the present composition 4 may contain one or more solvents. From the viewpoint of reducing the water absorption of the present composition 1 and its cured product, the surface tension of the solvent is preferably 45 mN / m or less, more preferably 40 mN / m or less, further preferably 35 mN / m or less, and particularly preferably 30 mN / m or less. The lower limit of the surface tension is not particularly limited, and can be set to 5 mN / m or more.

[0133] The present composition 2 contains a solvent having a surface tension of 45 mN / m or less. From the viewpoint of suppressing the uneven distribution of silica particles and reducing water absorption, the surface tension of the solvent is preferably 40 mN / m or less, more preferably 35 mN / m or less, and further preferably 30 mN / m or less. The lower limit of the surface tension is not particularly limited and can be set to 0.05 mN / cm or more.

[0134] The present composition 3 contains a solvent. From the viewpoint of suppressing the uneven distribution of silica particles and reducing water absorption, the surface tension of the solvent contained in the present composition 3 is preferably 45 mN / m or less, more preferably 40 mN / m or less, and further preferably 5 mN / m or less. The lower limit of the surface tension is not particularly limited, and an example thereof is 5 mN / m.

[0135] From the viewpoint of improving the fluidity and handling properties of the composition when the present composition 1, the present composition 2 or the present composition 4 is thermally cured to form a molded article such as a prepreg, the boiling point of the solvent in the present composition 1, the present composition 2 and the present composition 4 is preferably 75° C. or higher, more preferably 80° C. or higher, and further preferably 90° C. or higher. The upper limit of the boiling point is not particularly limited, and can be 200° C. or lower.

[0136] The boiling point of the solvent of the present composition 3 is 75° C. or higher, preferably 80° C. or higher, more preferably 90° C. or higher from the viewpoint of accelerating the above-mentioned action mechanism. The upper limit of the boiling point is not particularly limited, but can be 200° C. or lower.

[0137] From the viewpoint of operability when thermally curing the present composition 1, the present composition 2 or the present composition 4 to form a molded product such as a prepreg and suppressing aggregation of silica particles associated with solvent volatilization during heating, the evaporation rate of the solvent in the present composition 1, the present composition 2 and the present composition 4 is preferably 0.3 to 3.0, more preferably 0.4 to 2.0.

[0138] The evaporation rate of the solvent of the present composition 3 is 0.3 to 4.0, and preferably 0.4 to 2.0 from the viewpoint of workability when the present composition 3 is thermally cured to form a molded product such as a prepreg and suppression of aggregation of silica particles associated with solvent volatilization during heating.

[0139] Examples of the solvent in the present composition 1, the present composition 2 or the present composition 4 include acetone, methanol, ethanol, butanol, 2-propanol, 2-methoxyethanol, 2-ethoxyethanol, toluene, xylene, methyl ethyl ketone, N,N-dimethylformamide, methyl isobutyl ketone, N-methyl-2-pyrrolidone, n-hexane, cyclohexane and the like. From the viewpoint of adhesion of a molded article such as a prepreg to a metal substrate layer, the solvent preferably includes at least one selected from the group consisting of toluene (110°C, 28mN / cm, 0.58), cyclohexanone (156°C, 35mN / cm, 0.32), methyl ethyl ketone (80°C, 24.6mN / cm, 3.7) and N-methyl-2-pyrrolidone (202°C, 42mN / m, 0.3 to 4.0). It should be noted that the boiling point, surface tension and evaporation rate are indicated in order in parentheses.

[0140] Examples of the solvent in the present composition 3 include hydrocarbons such as toluene (111°C, 2.0), methylcyclohexane (101°C, 3.20), n-heptane (98°C, 3.62), and m-xylene (139°C, 0.76); alcohols such as ethanol (78°C, 1.54), isopropanol (82°C, 1.5), 1-propanol (97°C, 0.94), isobutanol (107°C, 0.64), 1-butanol (118°C, 0.47), and 2-butanol (100°C, 0.89); acetates such as propyl acetate (102°C, 2.14), isobutyl acetate (118°C, 1.45), and butyl acetate (126°C, reference value); and methyl ethyl ketone (80°C, 3.7). , methyl isobutyl ketone (116°C, 1.6), cyclohexanone (156°C, 0.32) and other ketones; ethylene glycol monomethyl ether (125°C, 0.53), ethylene glycol monoethyl ether (136°C, 0.38) and other cellosolves; 1-methoxy-2-propanol (120°C, 0.71), 1-methoxypropyl-2-acetate (146°C, 0.44), 1-ethoxy-2-propanol (132°C, 0.34), 3-ethoxypropionic acid ethyl ester (170°C, 0.34) and other glycol ethers; trichloroethylene (87°C, 3.22), tetrachloroethylene (121°C, 1.29) and other chlorinated hydrocarbons; N-methyl-2-pyrrolidone (202°C, 0.3-4.0), etc. It should be noted that the boiling point and evaporation rate are indicated in parentheses.

[0141] Among them, from the viewpoint of adhesion and the like, the solvent preferably contains at least one selected from the group consisting of toluene, cyclohexanone, methyl ethyl ketone, and N-methyl-2-pyrrolidone.

[0142] The present composition 3 contains a solvent having a boiling point of 75° C. or higher and an evaporation rate of 0.3 to 4.0, and may contain other solvents as long as it does not contradict the purpose of the present disclosure.

[0143] Other solvents include hydrocarbons such as hexane, cyclohexane, and benzene; alcohols such as methanol; acetates such as methyl acetate and ethyl acetate; ketones such as acetone, diisobutyl ketone, 4-hydroxy-4-methyl-2-pentanone, and isophorone; cellosolves such as ethylene glycol mono-n-butyl ether, ethylene glycol mono-tert-butyl ether, and 2-ethoxyethyl acetate; glycol ethers such as 3-methoxy-3-methylbutanol, 3-methoxy-3-methylbutyl acetate, propylene glycol monopropyl ether, 3-methoxybutyl acetate, propylene glycol monomethyl ether acrylate, diethylene glycol monobutyl ether, and triethylene glycol monobutyl ether; ethers such as tetrahydrofuran and diethyl ether; chlorinated hydrocarbons such as dichloromethane, 1,1,1-trichloroethane, and 1,1-dichloro-1-fluoroethane; and the like.

[0144] Among the solvents contained in the present composition 3, the proportion of the solvent having a boiling point of 75° C. or higher and an evaporation rate of 0.3 to 4.0 is preferably 70% by volume or higher, more preferably 80% by volume or higher, further preferably 90% by volume or higher, and particularly preferably 100% by volume. That is, it is particularly preferred to use only solvents having a boiling point of 75° C. or higher and an evaporation rate of 0.3 to 4.0 as solvents.

[0145] The content of the solvent relative to the total mass of the present composition 1, the present composition 2, the present composition 3 or the present composition 4 is not particularly limited and may be 10 to 60 mass %, 20 to 50 mass % or 30 to 40 mass %.

[0146] In addition, the content of the silica particles is preferably 50 to 550 parts by mass, 100 to 500 parts by mass, 125 to 400 parts by mass, or 150 to 300 parts by mass relative to 100 parts by mass of the solvent in the present composition 1, the present composition 2, the present composition 3, or the present composition 4. Even if the amount of silica particles relative to the amount of solvent is large, the silica particles are highly wetted by the above-mentioned mechanism of action, so that the uniform dispersibility and the viscosity of the composition are easily balanced. Therefore, even if the amount of the aforementioned silica particles is large, the viscosity of the composition is not easy to increase.

[0147] The present composition 1, the present composition 2, the present composition 3 or the present composition 4 may contain one or more plasticizers. Examples of the plasticizer include butadiene-styrene copolymers, etc. The content of the plasticizer is preferably 10 to 50 parts by mass, more preferably 20 to 40 parts by mass, relative to 100 parts by mass of the thermosetting resin.

[0148] The present composition 1, the present composition 2, the present composition 3 or the present composition 4 may contain, in addition to the above-mentioned components, other components such as surfactants, thixotropy imparting agents, pH adjusters, pH buffers, viscosity adjusters, defoaming agents, silane coupling agents, dehydrating agents, weathering agents, antioxidants, heat stabilizers, lubricants, antistatic agents, whitening agents, colorants, conductive materials, release agents, surface treatment agents, flame retardants, various organic or inorganic fillers, etc., within a range that does not impair their effects.

[0149] The prepreg 1 of the present disclosure comprises the present composition 1 or a semi-cured product thereof and a fibrous base material.

[0150] The prepreg 2 of the present disclosure comprises the present composition 2 or a semi-cured product thereof and a fibrous base material.

[0151] The prepreg 3 of the present disclosure comprises the present composition 3 or a semi-cured product thereof and a fibrous base material.

[0152] The prepreg 4 of the present disclosure comprises the present composition 4 or a semi-cured product thereof and a fibrous base material.

[0153] The fibrous substrate preferably contains a glass component. As the fibrous substrate, glass cloth, aramid cloth, polyester cloth, glass nonwoven fabric, aramid nonwoven fabric, polyester nonwoven fabric, pulp paper, etc. can be cited. The thickness of the fibrous substrate is not particularly limited and can be set to 3 to 10 μm. It should be noted that, as described above, the description of the present composition 1, the present composition 2, the present composition 3 and the present composition 4 is omitted here.

[0154] The prepreg 1, prepreg 2, prepreg 3 or prepreg 4 of the present disclosure can be produced by coating or impregnating a fibrous substrate with the corresponding present composition 1, present composition 2, present composition 3 or present composition 4. After coating or impregnation with the present composition 1, present composition 2, present composition 3 or present composition 4, the liquid composition can be heated to semi-cure.

[0155] The metal substrate 1 with resin of the present disclosure comprises the present composition 1 or its semi-cured product or the above-mentioned prepreg 1 and a metal substrate layer. The metal substrate layer may be provided on one surface of the present composition 1 or its semi-cured product or the above-mentioned prepreg 1, or may be provided on both surfaces.

[0156] The metal substrate 2 with resin disclosed in the present invention comprises the present composition 2 or its semi-cured product or the above-mentioned prepreg 2 and a metal substrate layer. The metal substrate layer may be provided on one surface of the present composition 2 or its semi-cured product or the above-mentioned prepreg 2, or may be provided on both surfaces.

[0157] The metal substrate 3 with resin of the present disclosure comprises the present composition 3 or its semi-cured product or the above-mentioned prepreg 3 and a metal substrate layer. The metal substrate layer may be provided on one surface of the present composition 3 or its semi-cured product or the above-mentioned prepreg 3, or may be provided on both surfaces.

[0158] The metal substrate 4 with resin disclosed in the present invention comprises the present composition 4 or its semi-cured product or the above-mentioned prepreg 4 and a metal substrate layer. The metal substrate layer may be provided on one surface of the present composition 4 or its semi-cured product or the above-mentioned prepreg 4, or may be provided on both surfaces.

[0159] The type of metal substrate layer is not particularly limited. As the metal constituting the metal substrate, copper, copper alloy, stainless steel, nickel, nickel alloy (also including 42 alloy), aluminum, aluminum alloy, titanium, titanium alloy, etc. can be cited. The metal substrate layer is preferably a metal foil, and more preferably a copper foil such as a rolled copper foil and an electrolytic copper foil. The surface of the metal foil can be treated with rust prevention (oxide coating such as chromate, etc.) or roughening. As the metal foil, a metal foil with a carrier formed by a carrier copper foil (thickness: 10 to 35 μm) and an extremely thin copper foil (thickness: 2 to 5 μm) laminated on the surface of the carrier copper foil via a peeling layer can also be used. The surface of the metal substrate layer can be treated with a silane coupling agent. In this case, the entire surface of the metal substrate layer can be treated with a silane coupling agent, and a portion of the surface of the metal substrate layer can be treated with a silane coupling agent. As a silane coupling agent, the above-mentioned substances can be used.

[0160] The thickness of the metal substrate layer is preferably 1 to 40 μm, more preferably 2 to 15 μm. From the viewpoint of reducing the transmission loss when using a metal substrate with a resin as a printed wiring board, the maximum height roughness (Rz) of the metal substrate layer (e.g., copper foil) is preferably 2 μm or less, more preferably 1.2 μm or less. Preferably, the Rz of the surface of the metal substrate layer (e.g., copper foil) located on the liquid composition, semi-cured material or prepreg side is in the above range. When a metal substrate with a resin is used as a printed wiring board, transmission loss can usually be reduced, but there is a tendency that the adhesion between the metal substrate layer and the prepreg, etc. is usually reduced. According to the prepreg 1, prepreg 2, prepreg 3 or prepreg 4 using the present composition 1, the present composition 2, the present composition 3 or the present composition 4 disclosed herein, the reduction in the above-mentioned adhesion can be suppressed and the transmission loss can be reduced.

[0161] In one embodiment, the metal substrate with resin 1, metal substrate with resin 2, metal substrate with resin 3, or metal substrate with resin 4 disclosed herein can be manufactured by coating the surface of the metal substrate layer with the corresponding present composition 1, present composition 2, present composition 3, or present composition 4. After coating the present composition 1, present composition 2, present composition 3, or present composition 4, the liquid composition can be heated to semi-cured.

[0162] In another embodiment, the metal substrate 1 with resin, the metal substrate 2 with resin, the metal substrate 3 with resin, or the metal substrate 4 with resin of the present disclosure can be manufactured by laminating the prepreg 1, prepreg 2, prepreg 3, or prepreg 4 corresponding to the metal substrate layer. As a method for laminating the metal substrate layer and the prepreg 1, prepreg 2, prepreg 3, or prepreg 4, a method of thermocompression bonding them can be cited.

[0163] Wiring board 1 of the present disclosure includes a cured product of present composition 1 and metal wiring.

[0164] Wiring board 2 of the present disclosure includes a cured product of present composition 1 and metal wiring.

[0165] Wiring board 3 of the present disclosure includes a cured product of present composition 1 and metal wiring.

[0166] Wiring board 4 of the present disclosure includes a cured product of present composition 1 and metal wiring.

[0167] As the metal wiring, one produced by etching the above-mentioned metal base material layer or the like can be used.

[0168] The wiring board 1, wiring board 2, wiring board 3 or wiring board 4 disclosed in the present invention can be manufactured by a method of etching the metal substrate layer possessed by the above-mentioned corresponding metal substrate with resin 1, metal substrate with resin 2, metal substrate with resin 3 or metal substrate with resin 4, a method of forming a pattern circuit on the surface of the cured product of the present composition 1, the present composition 2, the present composition 3 or the present composition 4 by using an electrolytic plating method (semi-additive method (SAP method), modified semi-additive method (MSAP method) etc.).

[0169] In one embodiment, the silica particles are used to adjust the viscosity of a liquid composition containing a thermosetting resin, and the silica particles have a d50 of 0.5 to 20.0 μm and a specific surface area of ​​0.1 to 3.5 m 2 / g.

[0170] In another embodiment, the silica particles are added to a liquid composition containing a thermosetting resin and used, wherein the silica particles have a d50 of 0.5 to 20 μm and a product of the specific surface area and the d50 of 2.7 to 5.0 μm·m 2 / g.

[0171] In another embodiment, the silica particles are used to adjust the thixotropy of a liquid composition containing a thermosetting resin, and the silica particles have a d50 of 0.5 to 20.0 μm and a d50 / d10 of more than 1.0 and not more than 5.0.

[0172] In another embodiment, silica particles are used to be mixed with a liquid composition containing a thermosetting resin to form a prepreg, wherein the proportion of particles with a particle size of 10 μm or more in the particle size distribution obtained by a Coulter counter method is less than 500 ppm, the coefficient of variation of the particle size is 0.30 to 0.80, and d50 is greater than 1.0 μm and less than 5.0 μm.

[0173] The details of the d50, d10, specific surface area, the product of the specific surface area and the d50 of the silica particles, d50 / d10, CV value, the proportion of particles with a particle size of 10 μm or more, particle size distribution, shape, sphericity, dielectric loss tangent, dielectric constant, surface treatment, elements that can be contained, manufacturing method, etc. of the silica particles are as described above, and therefore, are omitted here.

[0174] Example

[0175] Hereinafter, the embodiments of the present disclosure will be described in detail based on examples, but the embodiments of the present disclosure are not limited to these.

[0176] (Method for measuring d10 and d50 of silicon dioxide particles)

[0177] The d10 and d50 of the silica particles in Examples 11 to 19, 21 to 27, and 31 to 35 were measured by a laser diffraction / scattering method using a particle size distribution measuring device (MicrotracBEL Corp., MT3300EXII). Specifically, ultrasonic irradiation was performed 3 times for 60 seconds in the device to disperse the silica particles and then measured. d10 and d50 were measured twice within 60 seconds and taken as their average values. The pore size was set to 20 μm.

[0178] The d50 of the silica particles in Examples 41 to 48 was measured by the Coulter counter method as described below.

[0179] (Method for measuring specific surface area of ​​silicon dioxide particles)

[0180] The following silica particles were dried under reduced pressure at 230°C to completely remove moisture to prepare a sample. The specific surface area of ​​the sample was determined by a multi-point BET method using nitrogen gas using an automatic specific surface area / pore distribution measuring device "Tristar II" manufactured by Micromeritics.

[0181] (Method for measuring viscosity and thixotropic ratio)

[0182] The measurement was carried out using a rotational rheometer (manufactured by Anton Paar, modular rheometer Physica MCR-301).

[0183] The viscosity was measured at 25°C at a shear rate of 1 rpm for 30 seconds, and the viscosity at 30 seconds was taken as the above viscosity. The thixotropic ratio was calculated by dividing the viscosity measured at a rotation speed of 1 rpm by the viscosity measured at a rotation speed of 60 rpm.

[0184] 1. Preparation of ingredients for making liquid composition

[0185] [Thermosetting resin]

[0186] Polyphenylene ether resin: a modified polyphenylene ether obtained by modifying the terminal hydroxyl group of polyphenylene ether with a methacryloyloxy group (manufactured by SABIC: Noryl SA9000, Mw: 1700, number of functional groups per molecule: 2)

[0187] [Silicon dioxide particles]

[0188] Silica particles A: 15 g of silica powder 1 (AGC-Si-Tech Co., Ltd., manufactured by a wet method: H-31, d50: 3.5 μm) produced as a spherical silica precursor was filled into an alumina crucible, heated at 1200° C. for 1 hour in an electric furnace, cooled to 25° C., and ground with an agate mortar to obtain silica particles.

[0189] Silica particles B: 15 g of silica powder 2 (E-2C, d50: 2.5 μm, manufactured by Suzuki Oil & Fats Co., Ltd.) produced by a wet method as a spherical silica precursor was filled into an alumina crucible, heated at 1200°C in an electric furnace for 1 hour, cooled to 25°C, and ground with an agate mortar to obtain silica particles.

[0190] Silica particles C: Silica particles produced by VMC (Vaporized Metal Combustion) method (Admatechs: SC5500-SQ).

[0191] Silica particles D: Silica particles produced by a dry method (manufactured by Micron: SPH516).

[0192] Silica particles E: Silica particles produced by a wet method (manufactured by AAGC-Si-Tech Co., Ltd.: H-201, d50: 20.0 μm).

[0193] Silica particles F: Silica powder produced by a wet method (manufactured by Suzuki Oil & Fats Co., Ltd., E-2C, d50: 2.5 μm).

[0194] Silica particles G: Silica particles produced by the VMC method (Admatechs: SO-C1).

[0195] Silica particles 3C: silica particles described in Example 1 of JP-A-2018-145037.

[0196] Silica particles 4B: The silica particles A were prepared by adjusting the silica particles using a precision air classifier (Turbo Classifier TC-10 manufactured by Nisshin Engineering Inc.) so that no particles with a particle size of 10 μm or more were observed.

[0197] Silica particles 4C: The silica particles A were pulverized by a jet mill (manufactured by Nisshin Engineering Inc., Super Jet Mill SJ-100)-10 at a pulverization pressure of 0.5 MPa.

[0198] Silica particles 4D: manufactured by Ube Exsymo Co., Ltd., trade name "Hipresica (registered trademark)"

[0199] Silica particles 4E: manufactured by Nippon Shokubai Co., Ltd., trade name "Seahostar (registered trademark) KE-S S50"

[0200] Silica particles 4F: manufactured by Denka Company Limited, trade name "FB-5D"

[0201] [Solvent]

[0202] Toluene: boiling point 111°C, evaporation rate 2.0

[0203] Diisobutyl ketone (DIBK): boiling point 168°C, evaporation rate 0.2

[0204] Cyclohexanone: boiling point 156°C, evaporation rate 0.32

[0205] [Plasticizer]

[0206] Butadiene-styrene random copolymer (Ricon 100, Cray Valley)

[0207] [Curing accelerator]

[0208] Triallyl isocyanurate (TAIC, Mitsubishi Chemical Corporation)

[0209] [Curing agent]

[0210] α,α'-Di(tert-butylperoxy)diisopropylbenzene (Perbutyl(registered trademark) P, NOF Corporation)

[0211] 2. Manufacture of liquid composition, prepreg and metal substrate with resin

[0212] <Example 11>

[0213] 59 parts by mass of polyphenylene ether resin, 16 parts by mass of butadiene / styrene random copolymer, 25 parts by mass of triallyl isocyanurate, 1 part by mass of α,α'-di(tert-butylperoxy)diisopropylbenzene, 55 parts by mass of silica particles A, and 80 parts by mass of toluene were placed in a plastic bottle, and alumina balls of Φ20 mm were added, mixed at 30 rpm for 12 hours, and the alumina balls were removed to obtain a liquid composition. The liquid composition contained 68.75 parts by mass of silica particles A relative to 100 parts by mass of toluene, and contained 93 parts by mass of silica particles A relative to 100 parts by mass of polyphenylene ether resin.

[0214] The liquid composition was impregnated and coated on a glass cloth of IPC Spec 2116, and then heated and dried at 160° C. for 4 minutes to obtain a prepreg.

[0215] A 18 μm thick copper foil with a carrier (thickness of the copper foil: 3 μm, maximum height roughness Rz: 2 μm, manufactured by Mitsui Kinzoku Co., Ltd., MT18E) was laminated on both sides of the prepreg and heated at 230°C and a pressure of 30 kg / cm 2 The metal substrate with resin was obtained by heating and forming for 120 minutes.

[0216] <Examples 12~17>

[0217] The as-made composition, the prepreg, and the metal substrate with the resin were prepared in the same manner as in Example 11 except that the silica particles A were changed to the silica particles described in Table 1.

[0218] <Examples 18~19>

[0219] The liquid composition of Example 18 containing 137.5 parts by mass of silica particles A per 100 parts by mass of toluene was obtained in the same manner except that the amount of toluene in Example 11 was 40 parts by mass. The liquid composition of Example 19 containing 137.5 parts by mass of silica particles C per 100 parts by mass of toluene was obtained in the same manner except that the amount of toluene in Example 13 was 40 parts by mass. A prepreg and a metal substrate with a resin were produced in the same manner as in Example 11 using the obtained liquid composition.

[0220] [Determination of peel strength]

[0221] The peel strength between the prepreg and the copper foil with a carrier was measured using a TENSILON universal testing machine (RTC-1250A manufactured by A&D Co., Ltd.) in accordance with IPC-TM650-2.4.8.

[0222] It should be noted that Examples 11 to 13, 18, and 19 are embodiments, and Examples 14 to 17 are comparative examples.

[0223] [Table 1]

[0224]

[0225] As can be seen from Table 1, the prepreg 1 using the present composition 1 has excellent adhesion to the metal base material layer.

[0226] <Example 21>

[0227] In Example 11, a liquid composition, a prepreg, and a metal substrate with a resin were produced in the same manner except that toluene was replaced with cyclohexanone.

[0228] <Examples 22~25>

[0229] A liquid composition, a prepreg, and a metal substrate with a resin were produced in the same manner as in Example 21 except that at least one of the solvent and the silica particles A was changed as described in Table 2.

[0230] <Examples 26~27>

[0231] In Example 22, except that the amount of the polyphenylene ether resin was 40 parts by mass, a liquid composition of Example 26 containing 138 parts by mass of silica particles A relative to 100 parts by mass of the polyphenylene ether resin was obtained in the same manner. In addition, in Example 23, except that the amount of the polyphenylene ether resin was 40 parts by mass, a liquid composition of Example 27 containing 138 parts by mass of silica particles B relative to 100 parts by mass of the polyphenylene ether resin was obtained in the same manner. Using the obtained liquid composition, a prepreg and a metal substrate with a resin were produced in the same manner as in Example 21.

[0232] [Confirmation of the presence or absence of aggregation of silica particles]

[0233] The prepregs produced in Examples 21 to 27 were visually observed to confirm the presence or absence of aggregation of silica particles. The results are summarized in Table 2, with A being the case where no aggregation of silica particles was observed, B being the case where slight aggregation of silica particles was observed, and C being the case where much aggregation of silica particles was observed.

[0234] 〔Determination of water absorption〕

[0235] The water absorption of the metal substrate with resin was measured according to IPC TM-650 2.6.2.1. The water absorption of Example 24 was set to 1.00, and the water absorption of other examples was calculated as a relative value. The results are summarized in Table 2.

[0236] It should be noted that Examples 21 to 23, 26, and 27 are embodiments, and Examples 24 and 25 are comparative examples.

[0237] [Table 2]

[0238]

[0239] As can be seen from Table 2, in the prepreg 2 using the present composition 2, the uneven distribution of silica particles is suppressed, and the absorption rate is reduced.

[0240] <Example 31>

[0241] In the same manner as in Example 11, a liquid composition, a prepreg, and a metal substrate with a resin were produced.

[0242] <Examples 32~35>

[0243] A liquid composition, a prepreg, and a metal substrate with a resin were produced in the same manner as in Example 31 except that the silica particles and the solvent described in Table 3 were used.

[0244] 〔Standard deviation of dielectric constant〕

[0245] The dielectric constant was measured by the resonant resonance method using a "vector network analyzer E5063A" manufactured by Keycom Co., Ltd. The dielectric constants were measured at 1L / 4, 2L / 4, and 3L / 4 from the long side L in the center of the short side direction of the obtained prepreg, and the standard deviation of the three points was calculated. The measurement results are summarized in Table 3.

[0246] It should be noted that Examples 31 and 32 are embodiments, and Examples 33 to 35 are comparative examples.

[0247] [Table 3]

[0248]

[0249] As can be seen from Table 3, in the prepreg 3 using the present composition 3, the standard deviation of the dielectric constant is low and the aggregation of the silica particles is suppressed. It is therefore considered that the properties of the silica particles can be well exhibited by making the silica particles highly filled.

[0250] <Example 41>

[0251] In Example 11, a liquid composition and a prepreg were produced in the same manner except that 55 parts by mass of the silica particles A were replaced by 220 parts by mass.

[0252] Three prepregs were stacked, and ultra-thin copper foil with a thickness of 18 μm and a carrier (thickness of the copper foil: 3 μm, Rz: 2 μm, manufactured by Mitsui Kinzoku Co., Ltd., MT18E) was laminated on top and bottom. The prepreg was heated to 230°C and a pressure of 60 kg / cm 2 The metal substrate with resin was obtained by heating and forming for 120 minutes.

[0253] <Examples 42~46>

[0254] A liquid composition, a prepreg, and a metal substrate with a resin were produced in the same manner as in Example 41 except that the silica particles A were changed to the silica particles described in Table 4.

[0255] <Examples 47~48>

[0256] In Example 41, except that the amount of toluene was 40 parts by mass and the amount of polyphenylene ether resin was 40 parts by mass, a liquid composition of Example 47 was obtained in the same manner, which contained 550 parts by mass of silica particles A per 100 parts by mass of toluene and 550 parts by mass of silica particles A per 100 parts by mass of polyphenylene ether. In addition, except that the amount of toluene was 40 parts by mass and the amount of polyphenylene ether resin was 40 parts by mass in Example 43, a liquid composition of Example 48 was obtained in the same manner, which contained 550 parts by mass of silica particles 4C per 100 parts by mass of toluene and 550 parts by mass of silica particles 4C per 100 parts by mass of polyphenylene ether resin. Using the obtained liquid composition, a prepreg and a metal substrate with a resin were manufactured in the same manner as in Example 41.

[0257] In each example, the d50 of the silica particles, the coefficient of variation of the particle size, and the proportion of particles having a particle size of 10 μm or more were measured by the Coulter counter method using the above-mentioned equipment. The aperture was set to 20 μm.

[0258] [Measurement of Rzjis of metal substrate with resin]

[0259] The Rzjis value of the surface (matt surface) of the copper foil was measured using a contact surface roughness meter ("SURFCOM NEX001" manufactured by Tokyo Seimitsu Co., Ltd.) on the back side (bright side) of the copper foil with the prepreg bonded to the metal substrate with resin. The measurement terminal with a tip radius of 2 μm and a cone (cone angle: 60 degrees) was used, and the cutoff value was as follows: λc was set to 0.8 mm, λs was set to 2.5 μm, the reference length of the roughness curve was set to 0.8 mm, and the evaluation length of the roughness curve was set to 4.0 mm.

[0260] It should be noted that Examples 41 to 43 and 47 to 48 are embodiments, and Examples 44 to 46 are comparative examples.

[0261] [Table 4]

[0262]

[0263] As can be seen from Table 4, in Examples 41 to 43 and 47 to 48 using the present composition 4, the Rzjis of the molded product surface was low, and a molded product having excellent surface smoothness was obtained.

[0264] The disclosed contents of Japanese Patent Application No. 2022-065910 filed on April 12, 2022, Japanese Patent Application No. 2022-065911 filed on April 12, 2022, Japanese Patent Application No. 2022-065665 filed on April 12, 2022, and Japanese Patent Application No. 2022-075145 filed on April 28, 2022 are incorporated herein by reference in their entirety.

[0265] All documents, patent applications, and technical standards described in this specification are incorporated herein by reference to the same extent as if each document, patent application, and technical standard was specifically and individually described and was incorporated by reference.

Claims

1. A liquid composition comprising: a thermosetting resin and a particle size d50 of 0.5 to 20.0 μm and a specific surface area of ​​0.1 to 3.5 m 2 / g of silica particles, and the viscosity of the liquid composition measured at 25°C and a rotation speed of 1 rpm is 100 to 10000 mPa·s.

2. The liquid composition according to claim 1, wherein The content of the silica particles is 50 to 400 parts by mass based on 100 parts by mass of the thermosetting resin. 3 . The liquid composition according to claim 1 , further comprising a solvent, wherein the solvent comprises at least one selected from the group consisting of toluene, cyclohexanone, methyl ethyl ketone and N-methyl-2-pyrrolidone.

4. A liquid composition comprising: a thermosetting resin; a median particle size d50 of 0.5 to 20.0 μm and a product of a specific surface area and a median particle size d50 of 2.7 to 5.0 μm·m 2 / g of silica particles; and a solvent having a surface tension of 45 mN / m or less.

5. The liquid composition according to claim 4, wherein The specific surface area of ​​the silicon dioxide particles is 0.5 to 3.5 m 2 / g.

6. The liquid composition according to claim 4, wherein The content of the silica particles is 10 to 400 parts by mass based on 100 parts by mass of the thermosetting resin.

7. The liquid composition according to claim 4, wherein The solvent includes at least one selected from the group consisting of toluene, cyclohexanone, methyl ethyl ketone, and N-methyl-2-pyrrolidone.

8. A liquid composition comprising: a thermosetting resin; silica particles having a median particle size d50 of 0.5 to 20.0 μm and a ratio of the median particle size d50 to the 10% particle size d10 of more than 1.0 and less than 5.0; and a solvent having a boiling point of 75° C. or higher and an evaporation rate of 0.3 to 4.0 based on butyl acetate, wherein the thixotropic ratio of the liquid composition, calculated by dividing the viscosity measured at a rotation speed of 1 rpm by the viscosity measured at a rotation speed of 60 rpm, is less than 3.

0.

9. The liquid composition according to claim 8, wherein The ratio of the median particle size d50 of the silicon dioxide particles to the 10% particle size d10 is 1.2 to 2.

4.

10. The liquid composition according to claim 8, wherein The content of the silica particles is 10 to 400 parts by mass based on 100 parts by mass of the thermosetting resin.

11. The liquid composition according to claim 8, wherein The solvent includes at least one selected from the group consisting of toluene, cyclohexanone, methyl ethyl ketone, and N-methyl-2-pyrrolidone.

12. A liquid composition comprising: a thermosetting resin and silica particles, wherein the proportion of particles with a particle size of 10 μm or more in the particle size distribution obtained by a Coulter counter method is less than 500 ppm, the coefficient of variation of the particle size is 30 to 80%, and the median particle size d50 is greater than 1.0 μm and less than 5.0 μm.

13. The liquid composition according to claim 12, whereinThe specific surface area of ​​the silicon dioxide particles is 0.1 to 5.0 m 2 / g.

14. The liquid composition according to claim 12, wherein The ratio of the silica particles having a particle size of 10 μm or more is 300 ppm or less. 15 . The liquid composition according to claim 12 , further comprising at least one solvent selected from the group consisting of toluene, methyl ethyl ketone, and N-methylpyrrolidone.

16. The liquid composition according to claim 12, wherein The content of the silica particles is 10 to 400 parts by mass based on 100 parts by mass of the thermosetting resin.

17. The liquid composition according to any one of claims 1 to 16, wherein The thermosetting resin is epoxy resin, polyphenylene ether resin or o-divinylbenzene resin. 18 . A prepreg comprising: the liquid composition according to claim 1 or a semi-cured product thereof; and a fibrous base material.

19. A metal substrate with a resin, comprising: the liquid composition according to any one of claims 1 to 16 or a semi-cured product thereof, or the prepreg according to claim 18; and a metal substrate layer.

20. The metal substrate with resin according to claim 19, wherein The metal substrate layer is copper foil.

21. The metal substrate with resin according to claim 20, wherein The maximum height roughness Rz of the surface of the copper foil located on the liquid composition, the semi-cured product, or the prepreg side is 2 μm or less.

22. A wiring board comprising: a cured product of the liquid composition according to any one of claims 1 to 16; and metal wiring.

23. A silica particle for adjusting the viscosity of a liquid composition containing a thermosetting resin, wherein the average particle size d50 is 0.5 to 20.0 μm and the specific surface area is 0.1 to 3.5 m 2 / g.

24. The silicon dioxide particles according to claim 23, having a specific surface area of ​​0.8 to 2.0 m 2 / g.

25. Silica particles, which are added to a liquid composition containing a thermosetting resin and used, wherein the median particle size d50 is 0.5 to 20 μm and the product of the specific surface area and the median particle size d50 is 2.7 to 5.0 μm·m 2 / g.

26. The silicon dioxide particles according to claim 25, having a specific surface area of ​​0.5 to 3.5 m 2 / g.

27. Silica particles for adjusting the thixotropy of a liquid composition containing a thermosetting resin, wherein the median particle size d50 is 0.5 to 20.0 μm, and the ratio of the median particle size d50 to the 10% particle size d10 is greater than 1 and less than 5.

28. The silicon dioxide particles according to claim 27, wherein The ratio is 1.2 to 2.

4.

29. A silica particle used for mixing with a liquid composition containing a thermosetting resin to form a prepreg, wherein the proportion of particles with a particle size of 10 μm or more in the particle size distribution obtained by the Coulter counter method is less than 500 ppm, the coefficient of variation of the particle size is 0.30 to 0.80, and the median particle size d50 is greater than 1.0 μm and less than 5.0 μm.

30. The silicon dioxide particles according to claim 29, having a specific surface area of ​​0.1 to 5.0 m 2 / g.