Catalytic separation membrane based on copper oxide activated persulfate and application
By combining copper oxide with cellulose film, a catalytic separation membrane is formed, and using copper oxide to activate persulfate to produce reactive oxygen species, the problem that cellulose film cannot degrade organic pollutants is solved, efficient decolorization and degradation effects are achieved, and the effect of improving the The stability and recovery efficiency of the membrane are achieved.
Patent Information
- Application Number
- CN202411276070.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-26
AI Technical Summary
The existing cellulose membranes only have a filtration effect when treating printing and dyeing wastewater, and cannot effectively degrade organic pollutants, and it is difficult to separate and recover the copper oxide powder.
Copper oxide is used as the catalytic layer to combine with the cellulose membrane, and a catalytic separation membrane is formed through suction filtration and high-pressure fixation, so as to realize the in-situ activation of persulfate persulfate to produce reactive oxygen, and combine membrane separation technology to improve degradation efficiency.
It realizes efficient decolorization of dye wastewater and degradation of organic pollutants, improves the quality of the effluent, reduces membrane pollution, and solves the problem of separation and recovery of powder catalysts, extends the service life of the membrane.
Smart Images

Figure CN119015904A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of environmental protection and relates to a preparation method and application of a catalytic separation membrane for activating persulfate with copper oxide. Background Art
[0002] In recent years, with the continuous development of my country's industrialization process, environmental pollution problems have also emerged. Among them, the printing and dyeing industry has a huge amount of wastewater discharge, and the printing and dyeing wastewater has the characteristics of high chromaticity, complex water quality and difficulty in degradation. The discharge of printing and dyeing wastewater has significant mutagenicity to humans and organisms, threatening the ecosystem and endangering human health. Therefore, it is very necessary to fully treat the printing and dyeing wastewater. Membrane separation technology has the advantages of simple operation, stable effluent quality, and high degree of automation control, and has attracted much attention in the field of water treatment. However, in the process of treating printing and dyeing wastewater, cellulose membrane only has a filtering effect and does not have the ability to degrade organic pollutants. At present, SR-AOPs is a sewage treatment technology that has emerged in recent years. The efficient active species produced by it can mineralize organic pollutants into CO2 and H2O or non-toxic and low-toxic small molecules. It has the advantages of a wide pH range, high treatment efficiency, and low secondary pollution. Therefore, coupling SR-AOPs with membrane separation technology can efficiently degrade organic pollutants in sewage, making up for the defect of membrane separation technology in completely decomposing organic pollutants. The membrane filtration process strengthens the mass transfer between the catalytic functional layer and the organic pollutants, which is beneficial to improving the degradation efficiency. Copper oxide has been widely used in SR-AOPs in recent years because of its low toxicity, harmlessness, and high catalytic activity against persulfate. Therefore, copper oxide is selected as the catalytic functional layer and cellulose membrane is used as the membrane substrate. The two are combined to form a catalytic separation membrane, which can realize the in-situ activation of persulfate by copper oxide to produce active oxygen free radicals, so that the membrane has the functions of filtering and degrading organic pollutants, improving the effluent quality of the membrane and reducing membrane pollution. It shows good catalytic activity and stability for the treatment of dye wastewater.
[0003] The present invention combines the catalytic functional layer with the membrane substrate through suction filtration and high-pressure fixation to prepare a copper oxide catalytic separation membrane. The copper oxide catalytic separation membrane has good stability, a wide pH adaptation range, good anti-interference ability, good adaptability and a high decolorization rate for dye wastewater. The catalytic separation membrane has the functions of intercepting and degrading organic pollutants. The filtration strengthens the mass transfer between copper oxide and organic pollutants, which is beneficial to improving the catalytic efficiency. The membrane substrate solves the problem that powdered copper oxide is difficult to separate and recycle, and the decomposition of pollutants during the degradation process is beneficial to reducing membrane pollution. Summary of the invention
[0004] The present invention provides a method for preparing a catalytic separation membrane based on copper oxide-activated persulfate. In order to achieve the above-mentioned purpose, the present invention adopts the following technical scheme: copper oxide is used as a catalytic layer for activating persulfate to generate active oxygen species (mainly singlet oxygen), a cellulose membrane is used as a base membrane, and the catalytic functional layer is combined with the membrane base by suction filtration and pressure fixation to form an integrated catalytic separation membrane. The preparation method is as follows:
[0005] Preparation of copper oxide by coprecipitation method
[0006] Step 1: weigh 5-15 g (preferably 5-8 g) (30 mmol) of CuNO3·3H2O and dissolve it in 40 mL of deionized water, and add 20-50 mL (preferably 30-50 mL) of NaOH (4 mol / L).
[0007] Step 2: Stir the mixed solution in the above step 1 at 80-150° C. (preferably 90-100° C.) for 1-2 h (preferably 1.5-2 h).
[0008] Step 3: centrifuge and wash the precipitate obtained in the above step 2, and calcine it at 400-500°C (preferably 400-450°C) at a speed of 5-10°C / min (preferably 5-8°C / min) for 2-3h (preferably 2-2.5h).
[0009] Step 4: weigh 0.01-0.1 g of the copper oxide powder obtained in step 3 above and evenly disperse it in 20-100 mL (preferably 20-50 mL) of deionized water.
[0010] Step 5: Fix the copper oxide powder on the cellulose filter membrane by suction filtration and high pressure fixation of the solution obtained in the above step 4 to prepare a copper oxide catalytic separation membrane.
[0011] The present invention couples membrane separation technology with sulfate radical advanced oxidation technology (SR-AOPs) to enable the membrane to have the functions of intercepting and degrading organic pollutants. The membrane filtration process strengthens the mass transfer between the catalytic functional layer and the organic pollutants, thereby improving the degradation efficiency.
[0012] The present invention has the following beneficial effects: the present invention couples SR-AOPs with membrane separation technology to prepare a catalytic separation membrane based on copper oxide-activated persulfate, realizes in-situ activation of persulfate, enables the membrane to have both the function of filtering and generating singlet oxygen to degrade organic pollutants, improves the effluent quality of the membrane and reduces membrane pollution, and exhibits good decolorization performance for dye wastewater.
[0013] The present invention couples membrane separation technology with advanced oxidation technology, so that the catalytic separation membrane has the functions of intercepting and degrading organic pollutants. The membrane filtration process strengthens the mass transfer between the catalytic functional layer and the organic pollutants, which is conducive to improving the degradation efficiency of pollutants. The membrane substrate solves the problem of separation and recovery of powdered catalysts, and the decomposition of pollutants during the degradation process is conducive to alleviating membrane pollution. This technology not only has a high removal efficiency for organic pollutants, but also improves the service life of the membrane. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a scanning electron micrograph of copper oxide.
[0015] Figure 2 This is a diagram of the water treatment working system of the catalytic separation membrane.
[0016] Figure 3 This is the pure water flux curve of the catalytic separation membrane.
[0017] Figure 4 This is a diagram showing the treatment performance and stability of the catalytic separation membrane.
[0018] Figure 5 Cl - Effect curve of concentration on MB removal rate.
[0019] Figure 6 HCO3 - Effect curve of concentration on MB removal rate.
[0020] Figure 7 This is the effect curve of copper oxide powder on MB removal.
[0021] Figure 8 This is the effect curve of prepared copper oxide and commercial copper oxide on MB removal rate. DETAILED DESCRIPTION
[0022] The outstanding features and remarkable improvements of the present invention are further explained below in conjunction with the embodiments, which are only intended to illustrate the present invention and are not limited to the following examples.
[0023] Embodiment 1:
[0024] Weigh 7.2g (30mmol) of Cu(NO3)2·3H2O and dissolve it in 40mL of deionized water, add 30mL of NaOH (4mol / L), and then stir it for 2h under the condition of heating in a water bath at 90℃. Finally, the precipitate is centrifuged and washed and then calcined in a muffle furnace. The calcination temperature is 400℃, the heating rate from room temperature to the calcination temperature is 5℃ / min, and the calcination time is 2h. The obtained copper oxide powder particles show an irregular flaky structure in microscopic terms. The thickness of the copper oxide nanosheets formed by accumulation or aggregation is 30-32nm, and the particle size of the copper oxide particles ranges from 300 to 1000nm.
[0025] Embodiment 2:
[0026] 0.02 g, 0.04 g, 0.06 g, 0.08 g and 0.1 g of the copper oxide powder prepared in Example 1 were uniformly dispersed in 20 mL of deionized water, 5 cellulose membranes (with a diameter of 47 mm and a pore size of 0.22 μm) were placed on the surface of the filter head of the suction filtration sand core, and a suction filtration funnel was pressed on the surface. The joint was clamped with a clip, and deionized water with copper oxide powder was slowly poured into the funnel. A vacuum pump was used for suction filtration. At a pressure of 5×10 -3 MPa, the copper oxide powder was fixed on the cellulose filter membrane using a vacuum pump, and different copper oxide loadings (15.91 g / m 2 , 31.82g / m 2 , 47.73g / m 2 , 63.64g / m 2 , 79.55g / m 2 The effective loading area of the catalytic functional layer of the cellulose membrane is 1.257×10 -3 m 2 )'s copper oxide catalytic separation membrane.
[0027] Embodiment 3:
[0028] The copper oxide catalytic separation membrane prepared in Example 2 was placed on the surface of the filter head of the suction filtration sand core (the copper oxide powder on the separation membrane was located on the side away from the filter head surface), the suction filtration funnel was pressed on the surface, the joint was clamped with a clamp, deionized water was slowly poured into the funnel, and suction filtration was performed using a vacuum pump. Figure 3 It can be seen that the pure water flux of the catalytic separation membrane with different copper oxide loadings is positively correlated with the pressure in a first order linear manner, indicating that the pores of the catalytic separation membrane are incompressible. Under a vacuum pump pressure of 0.05 MPa, the pure water flux of the catalytic separation membrane can be between 2800-7000 L / (m 2 h) Controllability adjustment.
[0029] Embodiment 4:
[0030] The catalytic separation membrane (79.55 g / m 2 ) was treated with a methylene blue aqueous solution (MB) with a volume of 100 mL and a concentration of 0.5 mmol / L, and 100 μL of potassium persulfate (0.5 mol / L) was added to the solution to obtain a water sample; the copper oxide catalytic separation membrane (79.55 g / m 2 ) is placed on the surface of the filter head of the suction filter sand core (the copper oxide powder on the separation membrane is located on the side away from the filter head surface), the suction funnel is pressed on its surface, the joint is clamped with a clip, the methylene blue aqueous solution is slowly poured into the funnel, and the vacuum pump is used for suction filtration. When the vacuum pump pressure is 5×10 -3 MPa, the water sample was continuously filtered using a vacuum pump. The decolorization rate of MB by the catalytic separation membrane was as high as 98%. After 10 consecutive cycles, the decolorization rate could still be maintained at 98%.
[0031] Embodiment 5:
[0032] The catalytic separation membrane treated with MB solution in Example 4 was dried at 70° C. for 6 hours, and copper oxide powder was scraped off the dried catalytic separation membrane with a spatula. The copper oxide powder was recovered and weighed, and the recovery rate could reach 90%.
[0033] Embodiment 6:
[0034] The copper oxide catalytic separation membrane (79.55 g / m 2 ) The treatment volume is 100 mL, Cl - The copper oxide catalytic separation membrane (79.55 g / m 2 ) was placed on the surface of the filter head of the suction filter sand core (the copper oxide powder on the separation membrane was located on the side away from the filter head surface), the suction filter funnel was pressed on its surface, and the joint was clamped with a clip. - The aqueous solution was slowly poured into the funnel and filtered using a vacuum pump. When the vacuum pump pressure was 5×10 -3 MPa, the water sample was filtered by vacuum pump. - When the concentration was 0.2 mol / L, the removal rate of MB by copper oxide catalytic separation membrane decreased by only 3%, indicating that the removal rate of MB by copper oxide catalytic separation membrane was - Has good anti-interference ability.
[0035] Embodiment 7:
[0036] The copper oxide catalytic separation membrane (79.55 g / m2) prepared in Example 2 was treated with a volume of 100 mL, HCO3 -The copper oxide catalytic separation membrane (79.55 g / m2) prepared in Example 2 was placed on the surface of the filter head of the suction filtration sand core (the copper oxide powder on the separation membrane was located on the side away from the filter head surface), and the suction filtration funnel was pressed on its surface. The joint was clamped with a clip, and the HCO3 containing different concentrations was added. - The aqueous solution was slowly poured into the funnel and filtered using a vacuum pump. When the vacuum pump pressure was 5×10-3MPa, the water sample was filtered using a vacuum pump. - When the concentration was 0.1 mol / L, the removal rate of MB by copper oxide catalytic separation membrane only decreased by 4%, indicating that the removal rate of MB by copper oxide catalytic separation membrane was - Has good anti-interference ability.
[0037] Embodiment 8:
[0038] The copper oxide powder obtained in Example 1 was added to a methylene blue aqueous solution (MB) with a volume of 100 mL and a concentration of 0.5 mmol / L, and stirred using a magnetic stirrer at a speed of 100 r / min. When the copper oxide powder was added in an amount of 0.1 g, the removal rate of MB was 95.1%, indicating that the copper oxide powder has a good removal ability for MB.
[0039] Embodiment 9:
[0040] The cellulose membrane was placed on the surface of the filter head of the suction filtration sand core, and the suction filtration funnel was pressed on the surface. The joint was clamped with a clamp, and the MB aqueous solution treated in Example 8 was slowly poured into the funnel and filtered by a vacuum pump. When the vacuum pump pressure was 5×10 -3 MPa, a water sample was filtered using a vacuum pump to load the copper oxide powder in the water onto the cellulose surface and dried at 70°C for 6 h. The dried catalytic separation membrane was scraped off with a spatula and the copper oxide powder was recovered and weighed. The recovery rate was 83%, indicating that the recovery efficiency of copper oxide powder was lower than that of the copper oxide catalytic separation membrane (nearly 100%).
[0041] Embodiment 10:
[0042] The copper oxide powder obtained in Example 1 and commercial CuO were respectively added to a methylene blue aqueous solution (MB) with a volume of 100 mL and a concentration of 0.5 mmol / L, and stirred using a magnetic stirrer at a speed of 100 r / min. When the addition amounts of the copper oxide powder and the commercial CuO were both 0.1 g, the removal rate of MB by the prepared copper oxide powder was 95.1%, and the removal rate of MB by the commercial CuO was 90.53%, indicating that the prepared copper oxide powder had a good removal ability for MB compared with the commercial CuO.
Claims
1. A catalytic separation membrane based on copper oxide activated persulfate, characterized in that: Copper oxide is used as the catalytic functional layer for activating persulfate to produce singlet oxygen, and a cellulose membrane is used as a separation membrane substrate. The catalytic functional layer and the membrane substrate are stably combined by filtration and / or pressure fixation to form an integrated catalytic separation membrane (the catalytic functional layer is attached to one side of the membrane substrate).
2. The catalytic separation membrane according to claim 1, characterized in that: The diameter of the copper oxide particles ranges from 300 to 1000 nm, and the copper oxide particles are formed by aggregation or accumulation of copper oxide nanosheets with a thickness of 30 to 32 nm.
3. The catalytic separation membrane according to claim 1, characterized in that: The pore size of the cellulose membrane is 0.22-0.25 μm.
4. The catalytic separation membrane according to claim 1, characterized in that: The copper oxide was dispersed in water for suction loading or pressure loading. When the catalytic functional layer was loaded onto the fiber membrane surface by suction, the pressure formed by suction on the side of the fiber membrane away from the catalytic functional layer was 5×10 -3 ~5×10 -2 Mpa (preferably 5×10 -3 ~1×10 -2 Mpa); When the catalytic functional layer is loaded onto the fiber membrane surface, the pressure (gauge pressure) formed by the pressure on the fiber membrane side close to the catalytic functional layer is 5×10 -3 ~5×10 -2 MPa (preferably 5×10 -3 ~1×10 -2 Mpa); The mass ratio of copper oxide to water is 1:200 to 1:1000 (preferably 1:200 to 1:500).
5. The catalytic separation membrane according to claim 1, characterized in that: The loading amount of the catalytic functional layer is 15 to 80 g / m 2 (Preferably 47 to 80 g / m 2 ).
6. Use of the catalytic separation membrane according to any one of claims 1 to 5 for catalytic treatment of dye wastewater, characterized in that: With potassium persulfate (PMS) as an oxidant, the dye wastewater containing PMS passes through the separation membrane, and the catalytic separation membrane can catalytically treat the dye wastewater.
7. The use according to claim 6, characterized in that: The amount of dye wastewater is 100mL, the PMS concentration is 100-500μL and the concentration is 0.3-0.5mol / L (preferably 100-200μL).
8. The use according to claim 6 or 7, characterized in that: The PMS dye wastewater was pumped at a vacuum pump pressure of 5×10 -3 ~5×10 -2 MPa conditions, the filter passes through the separation membrane; The dye wastewater treated by the catalytic separation membrane contains methylene blue dye wastewater with a concentration of 20 to 25 mg / L.
9. The use according to claim 8, characterized in that: When the PMS concentration is 0.5mmol / L, the decolorization rate of dye wastewater by the catalytic separation membrane can be as high as 98%.
10. The catalytic separation membrane according to claim 6 or 7, characterized in that: The inorganic anions treated by the catalytic separation membrane are Cl - and HCO3 - , the aqueous solution is 100mL, Cl - Concentration is 0~0.2mol / L, HCO3 - The concentration is 0~0.1mol / L.
Citation Information
Cited By
Method for catalytically degrading dye wastewater based on tetrahedrite
CN121405238A
Composite membrane with functions of adsorption separation and catalytic degradation of new pollutants as well as preparation method and application of composite membrane
CN121911246A
A composite membrane with adsorption separation-catalytic degradation of new pollutants and a preparation method and application thereof
CN121911246B