Modified defect carbon nitride as well as preparation method and application thereof
By introducing modified metals and forming defect sites in defective carbon nitride, a highly efficient modified defective carbon nitride material was prepared, which solved the problems of low photogenerated carrier recombination efficiency and complex preparation of existing photocatalytic materials, and realized the industrial application of efficient photocatalytic reduction of CO2 to produce CO and CH4.
Patent Information
- Application Number
- CN202310584686.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
AI Technical Summary
Existing photocatalytic materials, such as graphitic carbon nitride, have high photogenerated carrier recombination efficiency but poor visible light absorption range. Furthermore, existing preparation methods are complex and costly, making them unsuitable for industrial applications.
By introducing specific types and amounts of modified metals (such as Mn, Cu, and Co) into defective carbon nitride, and combining this with the formation of defect sites, modified defective carbon nitride is prepared by low-temperature hydrothermal reaction under normal pressure, simplifying the preparation process and improving catalytic activity.
It significantly improves the catalytic activity and visible light absorption capacity of carbon nitride materials, increases the generation rate of CO and CH4, and has a simple process, high safety, and is suitable for industrial applications.
Smart Images

Figure BDA0004242953300000101 
Figure HDA0004242953310000011 
Figure HDA0004242953310000012
Abstract
Description
Technical Field
[0001] The present invention relates to the field of industrial catalysis, and in particular to a modified defective carbon nitride and a preparation method and use thereof, and also to a method for preparing CO and CH4 by photocatalytic reduction of CO2. Background Art
[0002] Photocatalytic technology uses solar energy to drive catalytic reactions, which can achieve energy conversion and storage. Among them, photocatalytic reduction of carbon dioxide (CO2) technology can convert CO2 into high value-added products such as hydrocarbon fuels such as methanol, methane, carbon monoxide (CO), and is a very promising way to utilize CO2. The development of photocatalytic technology began in the 1970s. However, the low efficiency and poor stability of photocatalytic materials limit its feasibility in industrial promotion and application.
[0003] Graphitic carbon nitride (g-C3N4) has been favored by researchers due to its suitable energy band gap (2.7 eV), low cost, and high thermal and chemical stability. However, graphitic carbon nitride materials still have the following disadvantages: high recombination efficiency of photogenerated carriers, poor conductivity and visible light absorption range. To solve the above problems, a large number of strategies for modifying carbon nitride materials have emerged, such as structural design, co-catalysts or heteroatom loading. From the perspective of heteroatom loading, rich heteroatoms (including metal heteroatoms and non-metal heteroatoms) with different functions have been successfully introduced into the surface or skeleton of carbon nitride, such as metal heteroatoms platinum and palladium acting as co-catalysts, and non-metallic elements sulfur and phosphorus used to change the surface electronic structure.
[0004] In addition, the presence of defect sites is often an effective way to improve reaction activity. Literature has reported that defective carbon nitride can be prepared through post-treatment with reducing substances such as hydrogen, ammonia or sodium borohydride, and the performance of defective carbon nitride is greatly improved. However, the use of reducing atmosphere or solvent has certain risks and poor safety, which is not suitable for industrial application.
[0005] Invention patent CN 115254162A discloses a defective g-C3N4 photocatalytic material and its preparation method and application. The preparation is carried out according to the following steps: using distilled water as solvent, melamine and tartaric acid as precursors, performing thermal polymerization after stirring and freeze drying, grinding, multiple washing and centrifugation, drying and secondary grinding to obtain the defective g-C3N4 photocatalytic material. This patent can enhance the activity of g-C3N4 photocatalyst through defect regulation method.
[0006] Invention patent CN 114931965A relates to a porous graphite phase carbon nitride loaded with non-precious metal bismuth catalyst, and applies it to photocatalytic CO2 reduction. Its preparation method includes: using melamine, phosphorous acid and bismuth salicylate as raw materials, preparing a precursor by hydrothermal method, dispersing the precursor in a mixed solvent of ethanol and glycerol, stirring and refluxing in a 90°C water bath, then separating and washing, drying for standby use, and then calcining the dried intermediate at high temperature in an inert atmosphere to prepare a bismuth-loaded porous graphite phase carbon nitride (Bi-PCN) catalyst. In the catalyst of this patent, the porous structure of carbon nitride promotes the effective contact between the material and the adsorbed molecules and the dispersion of heteroatom bismuth, and the loading of non-precious metal bismuth greatly improves the light absorption of carbon nitride materials in the visible light range. In addition, the composite material obtained after loading non-precious metal bismuth has high catalytic stability and durability. Under the irradiation of visible light, the CO generation rate of the catalyst can reach 13.07μmol·g -1 ·h -1 .
[0007] Invention patent CN 112742435A provides a method for preparing an iron-doped defect-rich carbon nitride nanotube photocatalyst, which first obtains a modified intermediate by a hydrothermal method, and then obtains a defect-rich carbon nitride nanotube with a porous structure by calcining in a muffle furnace. The porous structure and active sites created by iron doping solve the problems of low visible light utilization, poor nitrogen adsorption and activation ability, and low nitrogen fixation synthesis efficiency of existing photocatalysts.
[0008] The above invention patents prove that the presence of defect sites in carbon nitride and the introduction of heteroatoms can effectively promote the adsorption and activation of the catalyst to the reactants, thereby improving the photocatalytic performance. However, these preparation processes are relatively complicated, the material cost is also high, and the industrial applicability is not strong. Summary of the invention
[0009] In order to make up for the deficiencies in the prior art, an object of the present invention is to provide a modified defective carbon nitride, which can have more excellent catalytic performance by co-modification of defect sites and specific types of metal elements.
[0010] Another object of the present invention is to provide a preparation method and use of the modified defective carbon nitride.
[0011] Another object of the present invention is to provide a method for preparing CO and CH4 by photocatalytic reduction of CO2.
[0012] The first aspect of the present invention provides a modified defective carbon nitride, which consists of defective carbon nitride and a modified metal, wherein the modified metal is selected from one or more of Mn, Cu, and Co, and its content is 1 to 10% by mass of the modified defective carbon nitride.
[0013] The modified defective carbon nitride provided by the present invention has the following two characteristics: (1) it has defect sites, and (2) it contains a specific type and content of modified metal. Through the combined action of the defect sites and the modified metal, the carbon nitride material can expose more reactive sites, thereby significantly improving its catalytic activity.
[0014] In some preferred embodiments, the content of the modified metal in the modified defective carbon nitride can be 1.5-6.5% by mass (for example, about 1.5%, about 2.0%, about 2.5%, about 3.0%, about 3.5%, about 4.0%, about 4.5%, about 5.0%, about 5.5%, about 6.0%, about 6.5% or any combination of mass percentage intervals). In some more preferred embodiments, the content of the modified metal in the modified defective carbon nitride can be 3-5% by mass.
[0015] In other preferred embodiments, the modifying metal may be selected from Mn.
[0016] The second aspect of the present invention provides a method for preparing the modified defective carbon nitride according to any one of the above technical solutions, which comprises the following steps:
[0017] S1: preparing defective carbon nitride using thiourea and carbon nitride precursor materials; and
[0018] S2: dispersing the defective carbon nitride in a solution containing modified metal ions, performing a hydrothermal reaction at 100-150° C. under normal pressure, and separating and drying the obtained product after the reaction to obtain the modified defective carbon nitride;
[0019] Wherein, the carbon nitride precursor material is selected from one or more of urea, cyanamide, and dicyandiamide, and the modified metal ion is selected from Mn 2+ , Cu 2+ 、Co 2+ One or more of .
[0020] The preparation method provided by the present invention uses carbon nitride precursor materials such as thiourea and urea as raw materials. Thiourea and carbon nitride precursor materials form carbon nitride precursors through self-assembly. Thiourea decomposes during high-temperature calcination to produce reducing gases such as NH3 and H2S, which can partially reduce the formed carbon nitride, thereby manufacturing defect sites, without the need to additionally use external reducing atmospheres or substances such as hydrogen, ammonia, and sodium borohydride. The preparation method provided by the present invention also uses modified metals such as Mn, Cu, and Co to further modify the obtained defective carbon nitride. The introduction of the modified metal can be carried out by normal pressure and low-temperature hydrothermal reaction, without the need for high-temperature calcination treatment. By manufacturing defects and introducing modified metals, the catalytic activity of carbon nitride materials can be significantly improved. Moreover, the preparation method provided by the present invention is simple in process, high in safety, low in cost, and strong in industrial practicality.
[0021] Through the preparation method provided by the present invention, the modified metal finally coexists in the framework of defective carbon nitride in the form of atoms and divalent ions.
[0022] In some preferred embodiments, the preparation method provided by the present invention uses Mn 2+ As a modified metal ion, the introduction of Mn can greatly improve the catalytic performance of defective carbon nitride.
[0023] In some preferred embodiments, the step S1 may further include the following steps:
[0024] S101: preparing a thiourea aqueous solution and a carbon nitride precursor material (e.g., urea) aqueous solution with a concentration of 0.1-0.5 g / ml (e.g., about 0.1 g / ml, about 0.15 g / ml, about 0.2 g / ml, about 0.25 g / ml, about 0.3 g / ml, about 0.4 g / ml, about 0.5 g / ml, or any combination of concentration ranges), respectively, mixing equal volumes, and drying to obtain an intermediate; and
[0025] S102: calcining the intermediate at 400-700°C (for example, about 400°C, about 450°C, about 500°C, about 550°C, about 600°C, about 650°C, about 700°C or any combination of temperature ranges) to obtain the defective carbon nitride.
[0026] In some preferred embodiments, in step S101, the drying temperature may be 50-80°C, and the drying time may be 10-30 hours. In some more preferred embodiments, in step S101, the drying temperature may be 55-65°C, and the drying time may be 15-25 hours.
[0027] In some preferred embodiments, in the step S102, the calcination time may be 2 to 6 hours. In some more preferred embodiments, in the step S102, the calcination time may be 2 to 4 hours.
[0028] In some preferred embodiments, in step S2, the solution containing modified metal ions can be a soluble salt solution of modified metal ions (for example, an aqueous solution of nitrates), wherein the concentration of the modified metal ions can be 10 to 50 mmol / l (for example, about 10 mmol / l, about 15 mmol / l, about 20 mmol / l, about 25 mmol / l, about 30 mmol / l, about 35 mmol / l, about 40 mmol / l, about 50 mmol / l or any combination of concentration intervals).
[0029] In some preferred embodiments, in the step S2, the mass ratio of the defective carbon nitride to the modified metal ion can be 5:1 to 40:1 (for example, about 5:1, about 8:1, about 10:1, about 12:1, about 15:1, about 20:1, about 22:1, about 25:1, about 30:1, about 40:1 or any combination of mass ratio intervals). In some more preferred embodiments, in the step S2, the mass ratio of the defective carbon nitride to the modified metal ion can be 5:1 to 35:1. In some further preferred embodiments, in the step S2, the mass ratio of the defective carbon nitride to the modified metal ion can be 5:1 to 15:1.
[0030] In some preferred embodiments, step S2 may further include the following process:
[0031] The defective carbon nitride is dispersed in a solution containing modified metal ions, and subjected to a hydrothermal reaction at normal pressure for 4 to 15 hours at 100 to 150° C. (for example, about 100° C., about 110° C., about 120° C., about 130° C., about 140° C., about 150° C., or any combination of temperature ranges). After the reaction is completed, the product is allowed to stand for 6 to 20 hours, the product is separated, washed with water, and dried at 50 to 80° C. for 10 to 30 hours to obtain the modified defective carbon nitride.
[0032] In some more preferred embodiments, step S2 may further include the following process:
[0033] The defective carbon nitride is dispersed in a solution containing modified metal ions, and subjected to a hydrothermal reaction at 100 to 120° C. under normal pressure for 6 to 10 hours. After the reaction is completed, the product is allowed to stand for 8 to 15 hours, and the product is separated, washed with water, and dried at 50 to 65° C. for 10 to 18 hours to obtain the modified defective carbon nitride.
[0034] The third aspect of the present invention provides the use of the modified defective carbon nitride described in any one of the above technical solutions or the modified defective carbon nitride prepared by the preparation method described in any one of the above technical solutions as a photocatalyst.
[0035] In some preferred embodiments, the photocatalyst is a photocatalyst for reducing CO2 to prepare CO and CH4. Using the modified defective carbon nitride provided by the present invention as a photocatalyst can significantly increase the yield of CO.
[0036] The fourth aspect of the present invention provides a method for preparing CO and CH4 by photocatalytic reduction of CO2, the method using the modified defective carbon nitride described in any one of the above technical solutions or the modified defective carbon nitride prepared by the preparation method described in any one of the above technical solutions as a photocatalyst.
[0037] The technical solution provided by the present invention has the following advantages:
[0038] (1) The modified defective carbon nitride provided by the present invention simultaneously performs dual modification of the carbon nitride material with specific metal elements (especially Mn element) and defect sites. Through the combined effect of the two modifications, the catalytic performance of the carbon nitride material can be significantly improved.
[0039] (2) The preparation method provided by the present invention uses cheap and readily available materials such as urea, thiourea, and metal nitrates as raw materials, and produces defect sites by generating reducing gas through the self-decomposition of thiourea during high-temperature calcination. No external reducing atmosphere or reducing material is required, the process is simpler, and the operability and safety are better, and thus the industrial applicability is also stronger.
[0040] (3) The modified defective carbon nitride provided by the present invention has excellent catalytic performance and is very suitable for use as a photocatalyst, especially for the process of photocatalytic reduction of CO2 to prepare CO and CH4, which is beneficial to the resource utilization of CO2 and is green and environmentally friendly. Therefore, it has very important economic value and social significance. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 This is the infrared spectrum of d-CN-4 prepared in Example 4;
[0042] Figure 2 The SEM images of Mn-d-CN-4 and common bulk carbon nitride materials prepared in Example 4, wherein the left image is a SEM image of Mn-d-CN-4, and the right image is a SEM image of common bulk carbon nitride materials;
[0043] Figure 3 This is the full XPS spectrum of Mn-d-CN-4 prepared in Example 4;
[0044] Figure 4This is the XPS spectrum of Mn 2p of Mn-d-CN-4 prepared in Example 4;
[0045] Figure 5 This is a comparison chart of the yields of defective carbon nitride materials prepared in Example 1, Comparative Example 1 and Comparative Example 3 to generate CO by photocatalytic reduction of CO2 and H2O under the same conditions. DETAILED DESCRIPTION
[0046] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments.
[0047] Unless otherwise specified, the raw materials or reagents used in the examples and comparative examples of the present invention are commercially available products.
[0048] The percentages used in the embodiments and comparative examples of the present invention are all mass percentages unless otherwise specified.
[0049] Example 1
[0050] (1) Prepare 25 ml of 0.2 g / ml thiourea aqueous solution and 25 ml of urea aqueous solution, mix and stir for 2 h, and then dry in an oven at 60 °C for 20 h to obtain a white powder;
[0051] (2) placing the above powder in a 100 ml crucible with a lid, placing it in a muffle furnace and calcining it at 550 ° C for 2 h, and obtaining defective carbon nitride (d-CN) after cooling, which was collected and ground for subsequent use;
[0052] (3) preparing a 25 mmol / l manganese nitrate solution;
[0053] (4) Weigh 0.25 g of d-CN and disperse it in 20 ml of 25 mmol / l manganese nitrate solution in a beaker. The beaker is sealed and heated to 100°C. The temperature is maintained under normal pressure and stirred for 8 h. The mixture is allowed to stand for 10 h, centrifuged, and washed three times with deionized water. The resulting precipitate is placed in an oven and dried at 60°C for 12 h to obtain manganese-modified defective carbon nitride (Mn-d-CN). XPS testing shows that the mass fraction of manganese is 3.7%.
[0054] Example 2
[0055] (1) Prepare 25 ml of 0.2 g / ml thiourea aqueous solution and 25 ml of urea aqueous solution, mix and stir for 2 h, and then dry in an oven at 60 °C for 20 h to obtain a white powder;
[0056] (2) placing the above powder in a 100 ml crucible with a lid, placing it in a muffle furnace and calcining it at 550 ° C for 2 h, and obtaining defective carbon nitride (d-CN) after cooling, which was collected and ground for subsequent use;
[0057] (3) preparing a 25 mmol / l copper nitrate solution;
[0058] (4) Weigh 0.25 g of d-CN and disperse it in 20 ml of 25 mmol / l copper nitrate solution in a beaker. The beaker is sealed and heated to 100°C. The temperature is maintained under normal pressure and stirred for 8 hours. The mixture is allowed to stand for 10 hours, centrifuged, and washed three times with deionized water. The resulting precipitate is placed in an oven and dried at 60°C for 12 hours to obtain copper-modified defective carbon nitride (Cu-d-CN). XPS testing shows that the mass fraction of copper is 4.4%.
[0059] Example 3
[0060] (1) Prepare 25 ml of 0.2 g / ml thiourea aqueous solution and 25 ml of urea aqueous solution, mix and stir for 2 h, and then dry in an oven at 60 °C for 20 h to obtain a white powder;
[0061] (2) placing the above powder in a 100 ml crucible with a lid, placing it in a muffle furnace and calcining it at 550 ° C for 2 h, and obtaining defective carbon nitride (d-CN) after cooling, which was collected and ground for subsequent use;
[0062] (3) preparing a 25 mmol / l cobalt nitrate solution;
[0063] (4) Weigh 0.25 g of d-CN and disperse it in 20 ml of 25 mmol / l cobalt nitrate solution in a beaker. The beaker is sealed and heated to 100°C. The temperature is maintained under normal pressure and stirred for 8 hours. The mixture is allowed to stand for 10 hours, centrifuged, and washed three times with deionized water. The resulting precipitate is placed in an oven and dried at 60°C for 12 hours to obtain cobalt-modified defective carbon nitride (Co-d-CN). XPS testing shows that the mass fraction of the cobalt element is 5.0%.
[0064] Example 4
[0065] (1) Prepare 25 ml of 0.1 g / ml thiourea aqueous solution and 25 ml of urea aqueous solution, mix and stir for 2 h, and then dry in an oven at 60 °C for 20 h to obtain a white powder;
[0066] (2) The above powder was placed in a 100 ml crucible with a lid, and calcined in a muffle furnace at 550° C. for 4 h. After cooling, defective carbon nitride (d-CN-4) was obtained, which was collected and ground for subsequent use. The infrared spectrum of d-CN-4 is shown in Figure 1 As shown, 2140cm -1 A -C≡N peak defect appeared nearby;
[0067] (3) preparing a 25 mmol / l manganese nitrate solution;
[0068] (4) Weigh 0.25 g of d-CN-4 and disperse it in 20 ml of 25 mmol / l manganese nitrate solution in a beaker. The beaker is sealed and heated to 100°C. The temperature is maintained at normal pressure and stirred for 8 hours. The mixture is allowed to stand for 10 hours, centrifuged, and washed three times with deionized water. The resulting precipitate is placed in an oven and dried at 60°C for 12 hours to obtain manganese-modified defective carbon nitride (Mn-d-CN-4). XPS testing shows that the mass fraction of manganese is 3.3%.
[0069] The SEM image of Mn-d-CN-4 is shown in Figure 2 As shown in the left figure of the invention, it can be seen that the carbon nitride obtained by the preparation method of the present invention presents a loose porous structure, while the block carbon nitride prepared by conventional thermal polycondensation (the product obtained by calcining urea powder directly at 500-550°C for 2-4h) presents an irregular block (such as Figure 2 As shown in the right figure, the diameter reaches several microns to tens of microns). Loose and porous carbon nitride has more advantages than ordinary bulk carbon nitride in both absorbing incident light and adsorbing reactants.
[0070] The XPS spectrum of Mn-d-CN-4 is shown in Figure 3-4 As shown, XPS analysis indicates that the manganese exists in the framework of carbon nitride in the form of manganese atoms and divalent manganese ions.
[0071] Comparative Example 1
[0072] (1) Prepare 25 ml of 0.2 g / ml thiourea aqueous solution and 25 ml of urea aqueous solution, mix and stir for 2 h, and then dry in an oven at 60 °C for 20 h to obtain a white powder;
[0073] (2) The above powder was placed in a 100 ml crucible with a lid, and calcined at 550 °C in a muffle furnace for 2 h. After cooling, defective carbon nitride (d-CN) was obtained, which was collected and ground.
[0074] Comparative Example 2
[0075] (1) Prepare 25 ml of 0.2 g / ml thiourea aqueous solution and 25 ml of urea aqueous solution, mix and stir for 2 h, and then dry in an oven at 60 °C for 20 h to obtain a white powder;
[0076] (2) placing the above powder in a 100 ml crucible with a lid, placing it in a muffle furnace and calcining it at 550 ° C for 2 h, and obtaining defective carbon nitride (d-CN) after cooling, which was collected and ground for subsequent use;
[0077] (3) preparing a 25 mmol / l manganese nitrate solution;
[0078] (4) Weigh 0.25 g of d-CN and disperse it in 20 ml of 25 mmol / l manganese nitrate solution in a beaker. The beaker is sealed at 25°C and maintained at this temperature under normal pressure and stirred for 8 hours. The mixture is allowed to stand for 10 hours, centrifuged, and washed three times with deionized water. The resulting precipitate is placed in an oven and dried at 60°C for 12 hours to obtain defective carbon nitride adsorbed with manganese ions (Mn / d-CN).
[0079] Comparative Example 3
[0080] (1) Prepare 25 ml of 0.2 g / ml thiourea aqueous solution and 25 ml of urea aqueous solution, mix and stir for 2 h, and then dry in an oven at 60 °C for 20 h to obtain a white powder;
[0081] (2) placing the above powder in a 100 ml crucible with a lid, placing it in a muffle furnace and calcining it at 550 ° C for 2 h, and obtaining defective carbon nitride (d-CN) after cooling, which was collected and ground for subsequent use;
[0082] (3) preparing a 25 mmol / l manganese nitrate solution;
[0083] (4) Weigh 0.25 g of d-CN and disperse it in 20 ml of 25 mmol / l manganese nitrate solution in a beaker, place it in a hydrothermal kettle and heat it to 180°C, maintain this temperature for 8 hours under normal pressure, let it stand for 10 hours, centrifuge it, wash it three times with deionized water, and place the obtained precipitate in an oven at 60°C to dry it for 12 hours to obtain manganese-modified defective carbon nitride (Mn-d-CN -180 ).
[0084] Test Case
[0085] Under normal pressure, using 100 ml of CO2 and 5 ml of H2O as raw materials, 100 mg of carbon nitride materials prepared in Examples 1-4 and Comparative Examples 1-3 were used as catalysts, and visible light was used to catalyze the reduction of CO2. The CO generation yield is shown in Table 1.
[0086] Table 1 Test results
[0087]
[0088] It can be seen from the results in Table 1 that the modified defective carbon nitride materials prepared in Examples 1-4 of the present invention have better catalytic performance due to the dual modification effect, and can greatly improve the yield of CO under the same reaction conditions. Among them, the catalytic performance of the defective carbon nitride material modified with Mn is more outstanding (as shown in Examples 1 and 4).
[0089] In addition, it can be seen from the results in Table 1 that when defective carbon nitride undergoes a hydrothermal reaction in an ionic solution of a modified metal, a reaction temperature that is too high or too low cannot achieve a good modification effect (as shown in Comparative Example 2, when the hydrothermal reaction temperature is too low, the modified metal can only be physically adsorbed on the surface of the defective carbon nitride material and cannot achieve the purpose of modification; as shown in Comparative Example 3, when the hydrothermal reaction temperature is too high, the corresponding modification effect cannot be achieved either).
[0090] Unless otherwise defined, the terms used in the present invention have the meanings commonly understood by those skilled in the art.
[0091] The embodiments described in the present invention are for illustrative purposes only and are not intended to limit the scope of protection of the present invention. Those skilled in the art may make various other substitutions, changes and improvements within the scope of the present invention. Therefore, the present invention is not limited to the above embodiments, but is only limited by the claims.
Claims
1. A modified defective carbon nitride, It is characterized in that The modified carbon nitride is composed of defective carbon nitride and modified metal, wherein the modified metal is selected from one or more of Mn, Cu and Co, and the content of the modified carbon nitride is 1-10% of the modified defective carbon nitride by mass percentage.
2. The modified defective carbon nitride according to claim 1, It is characterized in that The modified metal is selected from Mn; and / or The content of the modified metal is 1.5-6.5% by mass of the modified defective carbon nitride, preferably 3-5% by mass.
3. The method for preparing the modified defective carbon nitride according to claim 1 or 2, It is characterized in that The following steps are involved: S1: Preparation of defective carbon nitride using thiourea and carbon nitride precursor materials; as well as S2: dispersing the defective carbon nitride in a solution containing modified metal ions, performing a hydrothermal reaction at 100-150° C. under normal pressure, and separating and drying the obtained product after the reaction to obtain the modified defective carbon nitride; Wherein, the carbon nitride precursor material is selected from one or more of urea, cyanamide, and dicyandiamide, and the modified metal ion is selected from Mn 2+ , Cu 2+ 、Co 2+ One or more of .
4. The preparation method according to claim 3, It is characterized in that The step S1 further comprises the following steps: S101: preparing 0.1-0.5 g / ml thiourea aqueous solution and carbon nitride precursor material aqueous solution respectively, mixing equal volumes, and drying to obtain an intermediate; and S102: calcining the intermediate at 400-700° C. to obtain the defective carbon nitride.
5. The preparation method according to claim 4, It is characterized in that In the step S101, the drying temperature is 50-80° C. and the drying time is 10-30 hours; and / or In the step S102, the calcination time is 2 to 6 hours.
6. The preparation method according to any one of claims 3 to 5, It is characterized in that In the step S2, the solution containing modified metal ions is a soluble salt solution of modified metal ions, preferably nitrate, wherein the concentration of the modified metal ions is 10 to 50 mmol / l.
7. The preparation method according to any one of claims 3 to 6, It is characterized in that In the step S2, the mass ratio of the defective carbon nitride to the modified metal ion is 5:1 to 40:
1.
8. The preparation method according to any one of claims 3 to 7, It is characterized in that The step S2 further includes the following process: The defective carbon nitride is dispersed in a solution containing modified metal ions, and subjected to a hydrothermal reaction at 100 to 150° C. at normal pressure for 4 to 15 hours. After the reaction is completed, the product is allowed to stand for 6 to 20 hours, and the product is separated, washed with water, and dried at 50 to 80° C. for 10 to 30 hours to obtain the modified defective carbon nitride.
9. Use of the modified defective carbon nitride according to claim 1 or 2 or the modified defective carbon nitride prepared by the preparation method according to any one of claims 3 to 8 as a photocatalyst; Preferably, the photocatalyst is used to reduce CO 2 Preparation of CO and CH 4 of photocatalyst.
10. A photocatalytic reduction of CO 2 Preparation of CO and CH 4 A method, wherein the method uses the modified defective carbon nitride according to claim 1 or 2 or the modified defective carbon nitride prepared by the preparation method according to any one of claims 3 to 8 as a photocatalyst.
Citation Information
Cited By
Photocatalyst based on g-C3N4 surface defect anchoring Ni / Mn Janus diatomic sites as well as preparation method and application
CN120984336A
A photocatalyst based on g-c3n4 surface defect anchoring ni / mn janus diatomic site, and a preparation method and application thereof