Method for preparing wire from difficult-to-deform cobalt-based high-temperature alloy
By using air hammer forging and hot pulling and cold drawing in the preparation of cobalt-based high-temperature alloys, the poor plasticity and deformation problems of cobalt-based high-temperature alloys are overcome, and efficient and low-cost silk preparation is achieved, and the current solution is solved. There are problems of low processing efficiency and high cost in the technology, which is suitable for large-scale production.
Patent Information
- Application Number
- CN202411142726.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-26
AI Technical Summary
The plasticity of cobalt-based high-temperature alloys is poor, the existing preparation methods are low in processing efficiency and high cost, and the length of the wire is limited, making it difficult to meet the application needs in some fields.
Before rolling, the cobalt-based high-temperature alloy is forged with air hammer, combined with hot and cold drawing processes, and through multiple passes of rotary forging and drawing processing, the required wire size is finally obtained, overcoming the deformation difference and deformation difficulties. question.
Simplified the preparation process, reduced production costs, improved production efficiency, significantly improved the forged blanking material yield, reduced the wire breaking rate, and can prepare wire materials with smaller diameters to meet the requirements of straight wire and disc wire. Good strong plasticity matching.
Smart Images

Figure CN119016535A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the preparation of alloy materials, and in particular to a method for preparing wire materials from a hard-to-deform cobalt-based high-temperature alloy. Background Art
[0002] Cobalt-based superalloy is a high-performance alloy material with excellent high-temperature strength, good corrosion resistance and oxidation resistance. It is widely used in aerospace, petrochemical, power generation and other fields. Among them, cobalt-based alloy wire is an important cobalt-based alloy product. However, the plasticity of cobalt-based superalloy is poor. At present, the preparation method of cobalt-based superalloy wire mainly adopts the powder metallurgy method to make alloy ingots, cuts the required wire size by wire cutting, and then uses centerless grinding to trim the surface. The high-temperature alloy welding wire prepared by this method has low processing efficiency and high cost, and the wire length is greatly limited, which limits its application in some fields. Summary of the invention
[0003] The purpose of the present invention is to provide a method for preparing a cobalt-based high-temperature alloy wire in view of the above-mentioned deficiencies in the prior art. The method uses an air hammer to forge the cobalt-based high-temperature alloy before rolling to cause pre-deformation, and finally obtains the required wire size by combining hot drawing and cold drawing, thereby overcoming the problems of poor shaping and difficult deformation of the cobalt-based high-temperature alloy.
[0004] To achieve the above object, the present invention adopts the following technical solutions:
[0005] The present invention provides a method for preparing a wire material from a hard-to-deform cobalt-based high-temperature alloy, comprising:
[0006] (1) Prepare raw materials according to the element ratio required by the standard:
[0007] (2) placing the raw materials weighed in the above step (1) into a vacuum induction melting furnace to prepare a cobalt-based alloy ingot that meets the composition requirements;
[0008] (3) Forging and blanking the cobalt-based alloy ingot with the required composition;
[0009] (4) The forged blank is surface processed by hot rotary forging with a rotary forging machine, and multiple rotary forgings are performed. After rotary forging, large and small turntable wire drawing is performed respectively, and finally the surface is finished by cold drawing machine and belt grinding machine.
[0010] Furthermore, the method for preparing wire from a difficult-to-deform cobalt-based high-temperature alloy is characterized in that the composition of the difficult-to-deform cobalt-based high-temperature alloy wire includes, by mass percentage, C: 0.05%-0.15%, Mn: ≤0.125%, Si: 0.20%-0.50%, Cr: 20%-24%, Ni: 20%-24%, W: 13%-16%, Fe≤3%, and Co is the balance.
[0011] Furthermore, in (2), the stainless steel ingot mold needs to be baked for more than 30 minutes before pouring, and the baking temperature is greater than 500° C. After the raw materials are completely melted, they are refined at 1520° C.-1650° C. for 3-10 minutes, and then cooled to 1380° C.-1520° C. for pouring.
[0012] Furthermore, in (3), the alloy ingot is kept in a muffle furnace for more than 2 hours to ensure that the temperature of the alloy ingot is uniform. The temperature is kept at 1160°C-1250°C. The alloy ingot with uniform temperature is forged to a size of Bars, bar length 400-430mm. Forged bars need to be annealed, annealing temperature 1160℃-1250℃, annealing time 12h-30h.
[0013] Furthermore, in (4), the surface of the annealed bar is machined to The processed bars are visually inspected and the surface is required to completely remove the oxide scale, slag inclusions and forging cracks produced by forging.
[0014] Furthermore, in said (4), the rolling temperature is 1160°C-1250°C, and the holding time is 10-40 minutes. The alloy rod is put into the continuous rolling equipment, and the processing die sequence is: 21mm-9.4mm.
[0015] Further, in (4), the rotary forging temperature is 1160℃-1250℃, and the processing die sequence is 9.4±0.1mm-9.0±0.1mm. The rotary forging temperature is 1100℃-1200℃, and the processing die sequence (material diameter sequence change size): 9.0±0.1mm±0.1mm-8.3±0.1mm-7.8±0.1mm-7.3±0.1mmmm-6.8±0.1mm-6.5±0.1mm. The rotary forging temperature is 960℃-1110℃, and the combined rotary forging allows a temperature fluctuation range of ±20℃; the processing die sequence (material diameter sequence change size): 6.5±0.1mm-5.9±0.1mm-5.3±0.1mm-4.8±0.1mm-4.4±0.1mm-4.0±0.1mm-3.70±0.1mm.
[0016] Furthermore, in (4), the large turntable wire drawing: the wire drawing temperature is 1100℃-950℃, and the temperature fluctuation range is ±20℃; the processing sequence (the material diameter changes in sequence): 3.70±0.1mm-3.5±0.1mm-3.2±0.05mm-2.9±0.05mm-2.5±0.05mm-2.3±0.05mm-2.1±0.05mm-1.9±0.05mm-1.78±0.05mm-1.6±0.05mm-1.5±0.05mm. Wire drawing on the rotating disk: the wire drawing temperature is 1150℃-1000℃, and the temperature fluctuation range is ±20℃; processing sequence (material diameter change sequence): 1.5±0.05mm-1.4±0.01mm-1.3±0.01mm-1.2±0.01mm-1.1±0.01mm-1.0±0.01mm-0.9±0.01mm.
[0017] Furthermore, in (4), if the final die size is larger than the diameter size by 0.02 mm, a cold drawing machine is used to reduce the diameter, and surface grinding and finishing are performed; if the final die size is smaller than the diameter size by 0.02 mm, a belt grinding machine is used to grind and finish the surface.
[0018] The present invention forges the cobalt-based high-temperature alloy with an air hammer before rolling to pre-deform it, and finally obtains the required wire size by combining hot drawing and cold drawing, thereby overcoming the problems of poor shaping and difficult deformation of the cobalt-based high-temperature alloy.
[0019] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:
[0020] (1) The present invention provides a method for preparing a cobalt-based high-temperature alloy wire, which has a simple preparation process route, low cost, and is suitable for large-scale production. Compared with the complex preparation process in the prior art, the preparation process of the present invention greatly reduces production costs, improves production efficiency, and is conducive to promotion and application.
[0021] (2) The present invention uses an air hammer to forge the cobalt-based high-temperature alloy before rolling to cause it to undergo pre-deformation. This method can significantly improve the forging yield rate.
[0022] (3) The present invention strictly controls the deformation of each section during the wire drawing stage to reduce the wire breakage rate. Cold drawing and belt sanding machine processing can ensure the size and surface quality of the wire.
[0023] (4) The present invention is divided into large and small turntable wire drawing in the wire drawing stage. This method can prepare wires with smaller diameters (less than 1 mm) and can meet the requirements of straight wires and coiled wires at the same time. It has a high yield rate and good strength-plasticity matching. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The alloy wire material with a diameter of Φ0.9 mm prepared in Example 1;
[0025] Figure 2 The alloy wire material with a diameter of Φ0.9 mm prepared in Example 1;
[0026] Figure 3 This is the cracking during the preparation of the alloy wire in Comparative Example 1. DETAILED DESCRIPTION
[0027] In order to make the invention purpose, technical solution and beneficial technical effects of the present invention clearer, the present invention is further described in detail below in conjunction with specific implementation methods;
[0028] Embodiment 1:
[0029] This example provides a method for preparing wire from a hard-to-deform cobalt-based high-temperature alloy. The composition of the hard-to-deform cobalt-based high-temperature alloy wire includes, by mass percentage, C: 0.08%, Mn: 0.09%, Si: 0.30%, Cr: 22%, Ni: 22%, W: 15%, Fe: 2%, and Co is the balance.
[0030] A method for preparing wire from a difficult-to-deform cobalt-based high-temperature alloy is as follows:
[0031] (1) Prepare raw materials according to the element ratio required by the standard.
[0032] (2) The raw materials are melted in a vacuum induction melting furnace. The stainless steel ingot mold needs to be baked for more than 30 minutes before pouring. The baking temperature is greater than 500°C. After the raw materials are completely melted, they are refined at 1600°C for 8 minutes. Then the temperature is cooled to 1450°C and poured into the stainless steel ingot mold. The alloy ingot has a diameter of 80 mm and a length of 200 mm.
[0033] (3) Use an air hammer to forge the ingot and keep the alloy ingot in a muffle furnace for more than 2 hours to ensure that the overall temperature of the alloy ingot is uniform. The holding temperature is 1180℃ and the final forging temperature is 1070℃. Forge to a diameter of Round bar, bar length 420mm. Forged bar needs to be annealed at 1200℃ for 20h.
[0034] (4) The surface of the annealed bar is machined to the diameter size The processed bars are visually inspected and the surface is required to completely remove the oxide scale, slag inclusions and forging cracks produced by forging.
[0035] The rolling temperature is 1200℃, and the holding time before rolling is 20min. The alloy rod is put into the continuous rolling equipment, and the processing sequence is: the diameter of the round rod is processed from 21mm to 9.4mm.
[0036] (5) Use a rotary forging machine for continuous forging. The forging must be carried out strictly in accordance with the processing die sequence and diameter reduction range of each rotary forging machine.
[0037] a. Put the alloy rod into the rotary forging equipment, the rotary forging temperature is 1200℃, and the processing sequence is: the diameter of the round rod is processed from 9.4mm to 9.0mm.
[0038] b. Place the alloy rod into the rotary forging equipment, the rotary forging temperature is 1150℃, and the processing die sequence (the diameter of the round rod changes in sequence): 9.0mm-8.3mm-7.8mm-7.3mm-6.8mm-6.5mm.
[0039] c. Place the alloy rod into the rotary forging equipment, the rotary forging temperature is 1100℃, and the allowable temperature fluctuation range of rotary forging is ±20℃; processing mold sequence (the diameter of the round rod changes in sequence): 6.5mm-5.9mm-5.3mm-4.8mm-4.4mm-4.0mm-3.70mm.
[0040] (6) Large turntable wire drawing (wire diameter 3.7mm-1.5mm): the wire drawing temperature is 1100℃, and the temperature fluctuation range is ±20℃; processing sequence (material diameter change sequence): 3.70mm-3.5mm-3.2mm-2.9mm-2.5mm-2.3mm-2.1mm-1.9mm-1.78mm-1.6mm-1.5mm.
[0041] Wire drawing on a rotating disk (wire diameter 1.5mm-0.8mm): wire drawing temperature is 1150°C, temperature fluctuation range is ±20°C; processing sequence (material diameter changes in sequence): 1.5mm-1.4mm-1.3mm-1.2mm-1.1mm-1.0mm-0.9mm.
[0042] (7) The final die diameter error is greater than 0.02 mm (the diameter is 0.93 mm), and the cold drawing machine is used to reduce the diameter (the diameter is 0.91 mm), and the surface is ground and finished until the surface presents a metallic luster, with no oxidation color or cracks on the surface;
[0043] If the final mold diameter size error is less than 0.02mm, directly use a belt grinder to grind and finish the surface until the surface presents a metallic luster, without oxidation color and cracks.
[0044] The macroscopic picture of the finished wire material of this embodiment is as follows: Figure 1 As shown, in this embodiment, the finished wire can be made into a round straight strip, the wire diameter is 0.9 mm, the length is 220 cm, the wire surface is bright, without oxide scale and cracks.
[0045] Embodiment 2:
[0046] This example provides a method for preparing wire from a hard-to-deform cobalt-based high-temperature alloy. The composition of the hard-to-deform cobalt-based high-temperature alloy wire includes, by mass percentage, C: 0.15%, Mn: 0.10%, Si: 0.40%, Cr: 23%, Ni: 21%, W: 14%, Fe: 1.5%, and Co is the balance.
[0047] A method for preparing wire from a difficult-to-deform cobalt-based high-temperature alloy is as follows:
[0048] (1) Prepare raw materials according to the element ratio required by the standard:
[0049] (2) The raw materials are melted in a vacuum induction melting furnace. The stainless steel ingot mold needs to be baked for more than 30 minutes before pouring. The baking temperature is greater than 500°C. After the raw materials are completely melted, they are refined at 1580°C for 10 minutes, and then cooled to 1450°C and poured into the stainless steel ingot mold. The alloy ingot has a diameter of 80 mm and a length of 200 mm.
[0050] (3) Use an air hammer to forge the ingot and keep the alloy ingot in a muffle furnace for more than 2 hours to ensure that the overall temperature of the alloy ingot is uniform. The holding temperature is 1180℃ and the final forging temperature is 1070℃. Forge to a diameter of Round bar, bar length 420mm. Forged bar needs to be annealed at 1150℃ and 25h.
[0051] (4) The surface of the annealed bar is machined to the diameter size The processed bars are visually inspected and the surface is required to completely remove the oxide scale, slag inclusions and forging cracks produced by forging.
[0052] The rolling temperature is 1180℃, and the holding time before rolling is 25min. The alloy rod is put into the continuous rolling equipment, and the processing sequence is: the diameter of the round rod is from 21±2mm to 9.4±0.1mm.
[0053] (5) Use a rotary forging machine for continuous forging. The forging must be carried out strictly in accordance with the processing die sequence and diameter reduction range of each rotary forging machine.
[0054] a. Put the alloy rod into the rotary forging equipment, the rotary forging temperature is 1200℃, and the processing sequence is: the diameter of the round rod is processed from 9.4mm to 9.0mm.
[0055] b. Place the alloy rod into the rotary forging equipment, the rotary forging temperature is 1160℃, and the processing sequence is: (the diameter of the round rod changes in sequence): 9.0mm-8.3mm-7.7mm-7.3mm-6.8mm-6.5mm.
[0056] c. Place the alloy rod into the rotary forging equipment, the rotary forging temperature is 1110℃, and the allowable temperature fluctuation range of rotary forging is ±20℃; processing mold sequence: (round rod diameter changes in sequence): 6.5mm-5.9mm-5.3mm-4.8mm-4.4mm-4.0mm-3.70mm.
[0057] (6) Large turntable wire drawing (wire diameter 3.7mm-1.5mm): wire drawing temperature is 1100℃, temperature fluctuation range is ±20℃; processing mode: 3.7mm-3.5mm-3.2mm-2.9mm-2.5mm-2.3mm-2.1mm-1.9mm-1.78mm-1.6mm-1.5mm. Medium turntable wire drawing (wire diameter 1.5mm-0.8mm): wire drawing temperature is 1150℃, temperature fluctuation range is ±20℃; processing mode: 1.5mm-1.4mm-1.3mm-1.2mm-1.1mm-1.0mm-0.91mm.
[0058] (7) The final die size error is greater than 0.02 mm (diameter is 1.13 mm), and the cold drawing machine is used to reduce the diameter (diameter is 1.11 mm), and the surface is ground and finished;
[0059] If the final mold diameter size error is less than 0.02mm, directly use a belt grinder to grind and finish the surface until the surface presents a metallic luster, with no oxidation color or cracks.
[0060] The macroscopic picture of the finished wire material of this embodiment is as follows: Figure 2 As shown, in this embodiment, the finished wire material has a diameter of 1.1 mm and can be made into coiled wire, and the surface of the wire material is bright, without oxide scale or cracks.
[0061] Embodiment 3:
[0062] This example provides a method for preparing wire from a hard-to-deform cobalt-based high-temperature alloy. The composition of the hard-to-deform cobalt-based high-temperature alloy wire includes, by mass percentage, C: 0.15%, Mn: 0.12%, Si: 0.40%, Cr: 24%, Ni: 24%, W: 14%, Fe: 2.5%, and Co is the balance.
[0063] A method for preparing wire from a difficult-to-deform cobalt-based high-temperature alloy is as follows:
[0064] (1) Prepare raw materials according to the element ratio required by the standard:
[0065] (2) The raw materials are melted in a vacuum induction melting furnace. The stainless steel ingot mold needs to be baked for more than 30 minutes before pouring. The baking temperature is greater than 500°C. After the raw materials are completely melted, they are refined at 1600°C for 10 minutes. Then the temperature is lowered to 1500°C and poured into the stainless steel ingot mold. The alloy ingot has a diameter of 80 mm and a length of 200 mm.
[0066] (3) Use an air hammer to forge the ingot and keep the alloy ingot in a muffle furnace for more than 2 hours to ensure that the overall temperature of the alloy ingot is uniform. The holding temperature is 1200℃ and the final forging temperature is 1070℃. Forge to a diameter of Round bar, bar length 430mm. Forged bar needs to be annealed at 1200℃ for 30h.
[0067] (4) The surface of the annealed bar is machined to the diameter size The processed bars are visually inspected and the surface is required to completely remove the oxide scale, slag inclusions and forging cracks produced by forging.
[0068] The rolling temperature is 1180℃, and the holding time before rolling is 25min. The alloy rod is put into the continuous rolling equipment, and the processing sequence is: the diameter of the round rod is from 21±2mm to 9.4±0.1mm.
[0069] (5) Use a rotary forging machine for continuous forging. The forging must be carried out strictly in accordance with the processing die sequence and diameter reduction range of each rotary forging machine.
[0070] a. Put the alloy rod into the rotary forging equipment, the rotary forging temperature is 1200℃, and the processing sequence is: the round rod is processed from 9.4mm to 9.0mm.
[0071] b. Place the alloy rod into the rotary forging equipment, the rotary forging temperature is 1160℃, and the processing sequence (the diameter of the round rod changes in sequence): 9.0mm-8.3mm-7.8mm-7.3mm-6.8mm-6.5mm.
[0072] c. Place the alloy rod into the rotary forging equipment. The rotary forging temperature is 1100°C. The allowable temperature fluctuation range of rotary forging is ±20°C. Processing sequence (round rod diameter changes in sequence): 6.5mm-5.9mm-5.3mm-4.8mm-4.4mm-4.0mm-3.70mm.
[0073] (6) Large turntable wire drawing (wire diameter 3.7mm-1.5mm): wire drawing temperature is 1100℃, temperature fluctuation range is ±20℃; processing mode (material diameter changes in sequence): 3.70mm-3.5mm-3.2mm-2.9mm-2.5mm-2.3mm-2.1mm-1.9mm-1.78mm-1.6mm-1.5mm. Medium turntable wire drawing (wire diameter 1.5mm-0.8mm): wire drawing temperature is 1150℃, temperature fluctuation range is ±20℃; processing mode (material diameter changes in sequence): 1.5mm-1.4mm-1.3mm-1.2mm-1.1mm-1.0mm-0.9mm.
[0074] (7) The final die size error is greater than 0.02 mm (diameter is 1.03 mm), and the cold drawing machine is used to reduce the diameter (diameter is 1.01 mm) and the surface is ground and finished;
[0075] If the final mold size error is less than 0.02mm, the surface is directly polished by belt grinding machine.
[0076] In this embodiment, the finished wire material has a diameter of 1.0 mm and can be made into coiled wire. The surface of the wire material is bright and has no oxide scale or cracks.
[0077] Comparative Example 1
[0078] The composition of the difficult-to-deform cobalt-based high-temperature alloy gold wire in this comparative example includes, by mass percentage, C: 0.08%, Mn: 0.09%, Si: 0.30%, Cr: 22%, Ni: 22%, W: 15%, Fe: 2%, and Co as the balance.
[0079] In this comparative example, the hard-to-deform cobalt-based high-temperature alloy gold wire material is prepared by a hot drawing process. The process comprises four steps: smelting (the process and conditions of this step are the same as those of step 2 in Example 1) - continuous rolling (the process and conditions of this step are the same as those of step 4 in Example 1) - rotary forging (the process and conditions of this step are the same as those of step 5 in Example 1) - hot drawing (the process and conditions of this step are the same as those of step 6 in Example 1), and the difference from Example 1 is that high-temperature forging is not performed before hot rolling.
[0080] The vacuum induction melting furnace is used for smelting. The stainless steel ingot mold needs to be baked for more than 30 minutes before pouring. The baking temperature is greater than 500°C. After the raw materials are completely melted, they are refined at 1600°C for 10 minutes, and then cooled to 1500°C for pouring. The ingot diameter is 80mm.
[0081] Since the alloy was not pre-deformed before continuous rolling due to the lack of high-temperature forging before hot rolling, the grain size inside the structure was coarse. Therefore, the alloy was deformed too much during continuous rolling, and it was difficult for the alloy to deform during continuous rolling. The deformation exceeded the plastic capacity during the hot rolling stage, and cracking occurred in the alloy rod during the continuous rolling process. The macroscopic image of the cracking is as follows: Figure 3 As shown in the macroscopic picture, it can be seen that the alloy rod is broken through in the longitudinal direction and cannot be deformed by drawing. Even if no complete cracking occurs in the continuous rolling stage, tiny microcracks will appear at the tail of the strip. Due to the existence of these microcracks, there are structural defects in some areas of the wire during the subsequent rotary forging process. Due to the existence of such defects, the quality of the wire is unstable during the hot drawing process, and wire breakage occurs.
[0082] Comparative Example 2
[0083] The composition of the difficult-to-deform cobalt-based high-temperature alloy gold wire in this comparative example includes, by mass percentage, C: 0.08%, Mn: 0.09%, Si: 0.30%, Cr: 22%, Ni: 22%, W: 15%, Fe: 2%, and Co as the balance.
[0084] In this comparative example, the hard-to-deform cobalt-based high-temperature alloy gold wire material is prepared by a hot drawing process. The process comprises five steps: smelting (the process and conditions of this step are the same as those of step 2 in Example 1) - blanking (the process and conditions of this step are the same as those of step 3 in Example 1) - continuous rolling (the process and conditions of this step are the same as those of step 4 in Example 1) - rotary forging (the process and conditions of this step are the same as those of step 5 in Example 1) - hot drawing (the process and conditions of this step are the same as those of step 6 in Example 1), and the difference from Example 1 is that no cold drawing and grinding treatment is performed.
[0085] The vacuum induction melting furnace is used for smelting. The stainless steel ingot mold needs to be baked for more than 30 minutes before pouring. The baking temperature is greater than 500°C. After the raw materials are completely melted, they are refined at 1600°C for 10 minutes, and then cooled to 1500°C for pouring. The ingot diameter is 80mm.
[0086] During the hot drawing process, in order to increase the lubricity of the wire, graphite emulsion is added during the drawing process. Under the action of high temperature, the surface of the sample is oxidized and turns black. Since no cold drawing and grinding treatment is performed after hot drawing to remove the surface oxide layer, the surface of the sample does not show metallic luster and the color is darker. At the same time, since no grinding process is performed, the sample becomes uneven in size and irregular in cross-sectional roundness during the drawing process.
[0087] Comparative Example 3
[0088] The composition of the difficult-to-deform cobalt-based high-temperature alloy gold wire in this comparative example includes, by mass percentage, C: 0.08%, Mn: 0.09%, Si: 0.30%, Cr: 22%, Ni: 22%, W: 15%, Fe: 2%, and Co as the balance.
[0089] In this comparative example, the hard-to-deform cobalt-based high-temperature alloy gold wire material is prepared by a hot drawing process. The process comprises five steps: smelting (the process and conditions of this step are the same as those of step 2 in Example 1) - blanking (the process and conditions of this step are the same as those of step 3 in Example 1, except that no annealing treatment is performed after blanking) - continuous rolling (the process and conditions of this step are the same as those of step 4 in Example 1) - rotary forging (the process and conditions of this step are the same as those of step 5 in Example 1) - hot drawing (the process and conditions of this step are the same as those of step 6 in Example 1).
[0090] The vacuum induction melting furnace is used for smelting. The stainless steel ingot mold needs to be baked for more than 30 minutes before pouring. The baking temperature is greater than 500°C. After the raw materials are completely melted, they are refined at 1600°C for 10 minutes, and then cooled to 1500°C for pouring. The ingot diameter is 80mm.
[0091] After the blanking, the sample was not annealed, the internal stress was large, and cracking occurred during the hot rolling stage. The annealing process can not only release the internal stress generated during the blanking process, but also homogenize the structure and eliminate the segregation generated during the casting process.
[0092] The comparison results of Examples 1-3 and Comparative Examples 1-3 show that the preparation method of the present invention adopts vacuum melting, air hammer forging, annealing, continuous rolling, multi-stage rotary forging and wire drawing and other processes, and by precisely controlling the specific details of each process step, it can effectively prepare difficult-to-deform alloy fine wires while achieving good surface quality, and is suitable for continuous precision welding.
Claims
1. A method for preparing wire from a hard-to-deform cobalt-based high-temperature alloy, It is characterized in that The method comprises the following steps: (1) Prepare raw materials according to the element ratio required by the standard: (2) placing the raw materials weighed in the above step (1) into a vacuum induction melting furnace to prepare a cobalt-based alloy ingot that meets the composition requirements; (3) Forging and blanking the cobalt-based alloy ingots that meet the composition requirements; forging into round bars with a diameter of φ25±2 mm; the forged bars need to be annealed; (4) The forged billet is surface processed to a round bar with a diameter of φ21±2 mm; After rolling, the hot rotary forging is carried out by a rotary forging machine, and multiple rotary forgings are carried out. After rotary forging, large and small turntable wire drawing is carried out respectively, and finally the surface is ground and finished by a cold drawing machine / or a belt grinder.
2. The method according to claim 1, It is characterized in that The components of the hard-to-deform cobalt-based high-temperature alloy wire include, by mass percentage, C: 0.05%-0.15%, Mn: ≤0.125%, Si: 0.20%-0.50%, Cr: 20%-24%, Ni: 20%-24%, W: 13%-16%, Fe≤3%, and Co as the balance.
3. The method according to claim 1, It is characterized in that In the step (2), the stainless steel ingot mold used needs to be baked for more than 30 minutes before casting, and the baking temperature is greater than 500°C; After the raw materials are completely melted, they are refined at 1520°C-1650°C for 3-10 minutes, then cooled to 1380°C-1520°C and poured into a stainless steel ingot mold to obtain an alloy ingot with a diameter of 80-85mm and a length of 200-230mm.
4. The method according to claim 1, It is characterized in that In the step (3), the alloy ingot is kept warm in the muffle furnace for more than 2 hours, preferably in the range of 2-4 hours, to ensure that the overall temperature of the alloy ingot is uniform; the holding temperature is 1160°C-1250°C; the alloy ingot with uniform temperature is forged (preferably using an air hammer to forge the ingot into a blank), and forged into a rod with a diameter size of φ (23-27mm, preferably 24-26mm) and a rod length of 400-430mm; the forged rod needs to be annealed, the annealing temperature is 1160°C-1250°C, and the annealing time is 12h-30h.
5. The method according to claim 1, It is characterized in that In the step (4), the surface of the rod after annealing in the step (3) is turned to a diameter of φ21±2 mm (preferably 21±1 mm); the processed rod is visually inspected to completely remove the oxide scale, slag inclusions and forging cracks generated by forging.
6. The method according to claim 1, It is characterized in that In the step (4), the rolling is carried out using a Y-type continuous rolling equipment. Before rolling, the alloy rod needs to be heated to a rolling temperature and kept warm. The rolling temperature is 1160°C-1250°C and the holding time is 10-40 minutes. The alloy rod is placed in the continuous rolling equipment and the processing sequence is: from a diameter of 21±2mm to a diameter of 9.4±0.1mm.
7. The method according to claim 1, It is characterized in that The hot rotary forging process in step (4) is as follows: the alloy rod is placed in a rotary forging device and subjected to multiple passes of rotary forging: Step 1: The rotary forging temperature is 1160℃-1250℃, and the processing die sequence (material diameter sequence change size): 9.4±0.1mm-9.0±0.1mm; Step 2: The rotary forging temperature is 1100℃-1200℃, and the processing die sequence (material diameter sequence change size): 9.0±0.1mm±0.1mm-8.3±0.1mm-7.8±0.1mm-7.3±0.1mm mm-6.8±0.1mm-6.5±0.1mm; Step 3: The rotary forging temperature is 960℃-1110℃, and the combined rotary forging allows a temperature fluctuation range of ±20℃; processing sequence (material diameter sequence change size): 6.5±0.1mm-5.9±0.1mm-5.3±0.1mm-4.8±0.1mm-4.4±0.1mm-4.0±0.1mm-3.70±0.1mm.
8. The method according to claim 1, It is characterized in that In the step (4), the large turntable wire drawing: the wire drawing temperature is 1100°C-950°C, the temperature fluctuation range is ±20°C; the processing mold sequence (the material diameter sequence changes): 3.70±0.1mm-3.5±0.1mm-3.2±0.05mm-2.9±0.05mm-2.5±0.05mm-2.3±0.05mm-2.1±0.05mm-1.9±0.05mm-1.78±0.05mm-1.6±0.05mm-1.5±0.05mm; Wire drawing on the rotating disk: the wire drawing temperature is 1150℃-1000℃, and the temperature fluctuation range is ±20℃; processing sequence (material diameter change sequence): 1.5±0.05mm-1.4±0.01mm-1.3±0.01mm-1.2±0.01mm-1.1±0.01mm-1.0±0.01mm-0.9±0.01mm.
9. The method according to claim 1, It is characterized in that In the step (4), the surface is finished, and the error range of the final mold diameter size is greater than 0.02 mm. A cold drawing machine is used to reduce the diameter, and the surface is ground and finished until the surface presents a metallic luster, and the surface has no oxidation color and no cracks. If the error range of the final mold diameter size is less than 0.02 mm, a belt grinding machine is used to grind and finish the surface until the surface presents a metallic luster, and the surface has no oxidation color and no cracks.
Citation Information
Patent Citations
Co-based alloy used for combustion chamber components, and preparation method thereof
CN106756404A
Co-Fe alloy wire with high magnetic induced torsion performance and preparing method of Co-Fe alloy wire
CN106868347A
Preparation method of hot-working-state cobalt-based alloy rod wire
CN111575539A
Preparation method of high-temperature-resistant and wear-resistant cobalt-based alloy wire
CN113210455A
Preparation method of high-performance tungsten-rhenium thermocouple wire
CN113604719A
Cited By
Preparation method of high-strength cobalt-based alloy wire
CN119733750A
Method for reducing inclusion content in high-temperature alloy powder and application