Lithium iron phosphate precursor and preparation method thereof, lithium iron phosphate and preparation method and application thereof
By controlling the particle size and component mass ratio of the lithium iron phosphate precursor, the problem of low compaction density of lithium iron phosphate material is solved, and the preparation of lithium iron phosphate with high compaction density and good electrical properties is achieved. It is suitable for lithium-ion batteries The positive electrode material meets the energy density requirements of long battery life.
Patent Information
- Application Number
- CN202411497607.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-10-25
AI Technical Summary
The compaction density of lithium iron phosphate materials is low and the preparation method is complex, making it difficult to achieve stable industrial production with high powder compaction density, and cannot meet the energy density requirements of long range.
By preparing a lithium iron phosphate precursor, the method includes reacting an iron source with a phosphoric acid solution to produce product A and reacting with a mixture of a lithium source and a coating source to produce product B, and obtaining component I and component II by grinding and controlling it The particle size and mass ratio form a high-pressure density lithium iron phosphate precursor, and then spray-dry, sintering and crushing to obtain lithium iron phosphate with high-pressure density and good electrical properties.
The high compaction density and good electrical performance of lithium iron phosphate are achieved. The battery has a small energy loss during charging and discharging, and the preparation method is simple and feasible, which is suitable for industrial production.
Smart Images

Figure CN119018871A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a lithium iron phosphate precursor and a preparation method thereof, lithium iron phosphate and a preparation method and application thereof. Background Art
[0002] Lithium iron phosphate is a positive electrode material for lithium-ion batteries. When used as a power battery, it has the advantages of good cycle performance and high safety. However, its energy density is low and cannot meet the requirements of long battery life.
[0003] In order to solve the problem of battery life anxiety, existing research technology currently uses lithium manganese iron phosphate as the next generation of lithium iron phosphate material. However, lithium manganese iron phosphate has lower electrical conductivity and poor cycle performance due to the Jiang Tailer effect.
[0004] In the prior art, although the energy density of lithium iron phosphate batteries can be increased by increasing the compaction density of lithium iron phosphate powder, the maximum compaction density of industrial lithium iron phosphate products currently shipped in large quantities on the market is 2.60g / cm 3 However, these preparation methods are complicated and the industrial production is unstable, making it difficult to achieve stable industrial production of high powder compaction density iron phosphate. Summary of the invention
[0005] The present invention mainly aims to overcome the defects of low compaction density and complicated preparation method of lithium iron phosphate materials in the prior art, and provides a lithium iron phosphate precursor and a preparation method thereof, lithium iron phosphate and a preparation method and application thereof. The lithium iron phosphate prepared by the present invention has high compaction density and good electrical properties.
[0006] In order to overcome the above technical problems, the present invention provides the following technical solutions.
[0007] The present invention provides a method for preparing a lithium iron phosphate precursor, which comprises the following steps:
[0008] S1. reacting a mixture I including an iron source and a phosphoric acid solution, and grinding after the reaction to obtain a product A;
[0009] reacting a mixture II including a first organic acid solution, a lithium source and a coating source, and obtaining a product B after the reaction is completed; the order of preparing the product A and the product B is not limited;
[0010] S2. Divide the mixture of the product A and the product B into two parts, grind them separately to obtain component I and component II, and then mix component I and component II to obtain a lithium iron phosphate precursor; wherein the average particle size of component I is 800-1600nm; the average particle size of component II is 50-600nm; and the mass ratio of component I to component II is (0.25-9):1.
[0011] In S1, the completion of the reaction means that generally no gas is generated during the reaction, as known to those skilled in the art.
[0012] In S1, the reaction is carried out under stirring, and the stirring speed is preferably 25-50 Hz, such as 30 Hz. The stirring speed will affect the generation of precipitates, thereby affecting the particle size distribution.
[0013] In S1, the iron source does not include iron phosphate. Those skilled in the art know that the present invention is a process for preparing lithium iron phosphate after the step of preparing iron phosphate.
[0014] In S1, the iron source is a compound containing iron and oxygen, more preferably one or more of iron powder, ferric oxide, ferrosoferric oxide and ferric nitrate, and further preferably one or more of iron powder, ferric oxide and ferrosoferric oxide.
[0015] Preferably, the iron content in the iron powder is 95wt% or more, more preferably 99wt% or more, and even more preferably 99.5wt% or more, for example 99.7wt%.
[0016] Preferably, the iron powder is one or more of primary reduced iron powder, secondary reduced iron powder, carbonyl reduced iron powder and electrolytic iron powder.
[0017] Preferably, the purity of the ferric oxide is 95wt% or more, more preferably 99wt% or more, and even more preferably 99.5wt% or more.
[0018] Preferably, the purity of the ferrosoferric oxide is 95 wt % or more, more preferably 99 wt % or more, and even more preferably 99.5 wt % or more.
[0019] In S1, the mesh size of the iron source may be 100-1000 meshes, more preferably 200-500 meshes, for example 250 meshes or 300 meshes.
[0020] In S1, the phosphoric acid solution generally refers to an aqueous phosphoric acid solution, and the mass percentage concentration of phosphoric acid in the phosphoric acid solution is preferably 20-85%, for example, 49%, 59% or 62%.
[0021] In S1, the phosphoric acid in the phosphoric acid solution may be conventional phosphoric acid in the art, such as industrial grade phosphoric acid, food grade phosphoric acid, electrical grade phosphoric acid or electronic grade phosphoric acid.
[0022] Wherein, the electrical grade phosphoric acid can be purchased from Guangxi Qinzhou Chengxing Chemical Technology Co., Ltd.
[0023] In S1, the reaction temperature of the mixture I may be 20-95°C, preferably 30-90°C, for example 35°C, 45°C, 55°C or 85°C.
[0024] In S1, the mixture I can be prepared by adding an iron source into a phosphoric acid solution under stirring.
[0025] In S1, in the mixture I, the molar ratio of iron element to phosphoric acid may be (0.94-1.05):1, preferably (0.96-1.0):1, for example, 0.98:1 or 0.995:1.
[0026] In S1, the mixture I may further include a catalyst. The catalyst has a catalytic effect during the reaction and can be used as a doping element to improve the conductivity of the lithium iron phosphate product after the reaction.
[0027] The catalyst is preferably a titanium-based catalyst.
[0028] The molar ratio of the titanium element in the catalyst to the iron element in the iron source is preferably (0.5-1):100, for example 1.15:100.
[0029] The catalyst is preferably added by first mixing the catalyst with the phosphoric acid solution and then adding the iron source.
[0030] In S1, the grinding operation and conditions may be conventional grinding operations, such as sand milling or ball milling.
[0031] Preferably, the grinding is performed using a sand mill.
[0032] The sand mill is preferably a vertical sand mill, a horizontal sand mill, a basket sand mill or a double-cone rod sand mill; the horizontal sand mill is preferably a nano-scale horizontal sand mill.
[0033] The particle size of the grinding beads used in the sand mill is preferably 0.1-3.0 mm, for example 0.3 mm or 0.4 mm.
[0034] The grinding beads used in the sand mill are preferably zirconia beads.
[0035] In S1, the viscosity of the product A may be 8000-20000 cps, preferably 10000-20000 cps, for example 15000 cps.
[0036] In S1, the first organic acid solution generally refers to an aqueous solution of a first organic acid, and the mass percentage concentration of the first organic acid in the first organic acid solution is preferably 5-98%, for example, 30%, 55%, 62% or 72%.
[0037] In S1, the first organic acid in the first organic acid solution is one or more of a carboxylic acid compound, ascorbic acid and a polymer acid, and the carboxylic acid compound is preferably one or more of formic acid, acetic acid, oxalic acid, citric acid, tartaric acid and malic acid.
[0038] The polymer acid refers to a high molecular weight polymer obtained by copolymerizing unsaturated olefins containing carboxylic acid through free radical polymerization, preferably polyacrylic acid or polymethacrylic acid.
[0039] In S1, the amount of the first organic acid in the first organic acid solution may be 20%-40%, for example, 32%, where the percentage is the mass of the first organic acid relative to the mass of phosphoric acid.
[0040] In some specific embodiments, the organic acid is one or more of citric acid, oxalic acid, malic acid, tartaric acid and polyacrylic acid.
[0041] In S1, the lithium source is a lithium-containing compound conventionally used in the art, preferably one or more of lithium hydroxide monohydrate, lithium carbonate, lithium dihydrogen phosphate, lithium phosphate and lithium acetate, for example, lithium hydroxide monohydrate and / or lithium carbonate; the lithium carbonate is preferably industrial grade lithium carbonate or battery grade lithium carbonate.
[0042] In S1, the molar ratio of the lithium element in the lithium source to the phosphoric acid in the phosphoric acid solution may be (0.98-1.05):1, for example, 0.98:1, 1.02:1, 1.03:1 or 1.04:1.
[0043] In S1, the coating source may be one or more of a carbon material, a metal compound and a conductive polymer. The coating source can complex the metal ions, which helps to achieve a special structure of lithium iron phosphate.
[0044] Among them, the carbon material is preferably glucose, glucose derivatives, second organic acids, organic acid derivatives, phenolic resins, polyethylene, polyethylene glycol, polyvinyl alcohol, polyvinyl alcohol derivatives, polyacrylic acid, polyacrylic acid derivatives, heterocyclic polymers or condensation polymers with N or O elements.
[0045] The glucose derivative preferably includes at least one of sucrose, starch and cyclodextrin.
[0046] The second organic acid preferably includes at least one of formic acid, acetic acid, oxalic acid, citric acid, tartaric acid and malic acid.
[0047] The polyacrylic acid derivative preferably includes polyacrylate.
[0048] The heterocyclic polymer having N or O elements preferably includes polyvinyl pyrrolidone.
[0049] Wherein, the metal compound preferably includes aluminum oxide and / or zinc stannate.
[0050] Wherein, the conductive polymer preferably includes one or more of polyaniline, polystyrene thiol, polyacetylene, lithium carbonate and polycarbonate.
[0051] In some embodiments, the coating source is polyethylene glycol.
[0052] In some embodiments, the coating source is sucrose.
[0053] In some embodiments, the coating source is citric acid and polyacrylic acid.
[0054] In some embodiments, the coating source is lithium carbonate, sucrose and polyvinyl pyrrolidone.
[0055] In some embodiments, the coating source is a mixture of polyvinyl alcohol, cyclodextrin and polyethylene glycol.
[0056] In S1, the amount of the coating source can be 1%-60%, preferably 5%-50%, more preferably 10%-40%, for example 15%, where the percentage refers to the mass percentage of the coating source to the mass percentage of the phosphoric acid.
[0057] In S1, the reaction temperature of the mixture II may be 20-95°C, preferably 30-90°C, for example 35°C, 40°C, 45°C or 55°C.
[0058] In S1, the mixture II can be prepared by adding a lithium source and a coating source into a stirring organic acid solution.
[0059] In S2, the mixture of the product A and the product B is generally prepared by mixing the product A and the product B.
[0060] In S2, the grinding operation and conditions may be conventional grinding operations, such as sand milling or ball milling.
[0061] Preferably, the grinding is performed using a sand mill.
[0062] The sand mill is preferably a vertical sand mill, a horizontal sand mill, a basket sand mill or a double-cone rod sand mill; the horizontal sand mill is preferably a nano-scale horizontal sand mill.
[0063] The particle size of the grinding beads used in the sand mill is preferably 0.1-3.0 mm, for example 0.3 mm or 0.4 mm.
[0064] The grinding beads used in the sand mill are preferably zirconia beads.
[0065] In S2, the grinding time can be conventional in the art and will be affected by factors such as the size of the zirconium beads, the feed rate, and the wear of the zirconium beads. Specifically, the average particle size of each component is controlled, and the sanding is stopped when the sanding reaches the target particle size. The corresponding time is not fixed, for example, 6-10 hours.
[0066] In S2, the average particle size of component I may be 1000-1500 nm, for example 1200 nm.
[0067] In S2, the average particle size of component II may be 100-300 nm, for example, 150 nm.
[0068] In S2, the mass ratio of the component I to the component II may be (0.25-9):1, preferably (1-5):1, for example 7:3.
[0069] The present invention provides a lithium iron phosphate precursor, which is prepared by the preparation method as described above.
[0070] In the present invention, the lithium iron phosphate precursor is an amorphous material formed by the accumulation of precipitates or an iron salt, a lithium salt and a mixture thereof with low crystallinity. Controlling the particle size of the lithium iron phosphate precursor is only to change the average size of the accumulation.
[0071] The inventor accidentally discovered through research that by controlling the particle size of the lithium iron phosphate precursor, a lithium iron phosphate product with a secondary particle structure in the shape of a flower cluster can be formed through a subsequent preparation process. When the particle size of the lithium iron phosphate precursor is small, the secondary particle structure is more easily destroyed in the subsequent crushing process. On the contrary, when the particle size of the lithium iron phosphate precursor is large, subsequent crushing and other treatments will not easily and completely destroy its secondary particle structure.
[0072] The present invention provides a method for preparing lithium iron phosphate, which comprises the following steps: spray drying, sintering and crushing the lithium iron phosphate precursor as described above in sequence to obtain the lithium iron phosphate;
[0073] The crushing includes screening the sintered material to obtain an upper screened material and a lower screened material, and then crushing the upper screened material and the lower screened material respectively, and then mixing them to obtain the lithium iron phosphate;
[0074] The particle size of the upper screening material after crushing satisfies: 1.1 μm ≤ D50 ≤ 1.80 μm;
[0075] The particle size of the lower layer screening material after crushing satisfies: 0.8 μm≤D50≤1.45 μm.
[0076] In the present invention, the D50 particle size of the upper screened material after crushing may be 1.1-1.6 nm, for example, 1.59 nm, 1.53 nm, 1.52 nm, 1.49 nm, 1.47 nm, 1.41 nm, 1.38 nm, 1.34 nm, 1.32 nm, 1.31 nm, 1.27 nm or 1.13 nm.
[0077] In the present invention, the D50 particle size of the lower layer screened material after crushing can be: 0.8-1.4 nm, for example, 1.34 nm, 1.24 nm, 1.21 nm, 1.16 nm, 1.13 nm, 1.12 nm, 1.1 nm, 1.09 nm, 1.09 nm, 1.02 nm, 0.99 nm, 0.98 nm or 0.82 nm.
[0078] In the present invention, in the lithium iron phosphate, the mass percentage of the particles after the lower layer of screened material is crushed is 10wt%-40wt%, for example, 40wt%, 38wt%, 35wt%, 34wt%, 33wt%, 32wt%, 31wt%, 29wt%, 28wt%, 27wt%, 26wt%, 25wt%, 24wt%, 21wt% or 10wt%.
[0079] In the present invention, the particle size of the upper screening material after crushing can satisfy: D10≤0.54μm.
[0080] In the present invention, the particle size of the upper screening material after crushing can satisfy: D99≤12.5μm.
[0081] In the present invention, the particle size of the upper screening material after crushing can satisfy: Dmax≤18μm.
[0082] In the present invention, the particle size of the lower layer screening material after crushing can satisfy: D10≤0.47μm.
[0083] In the present invention, the particle size of the lower layer screening material after crushing can satisfy: D99≤5.05μm.
[0084] In the present invention, the particle size of the lower layer screening material after crushing can satisfy: Dmax≤6.02μm.
[0085] In the present invention, the air inlet temperature of the spray drying can be 280°C.
[0086] In the present invention, the outlet temperature of the spray drying can be 130°C.
[0087] In the present invention, the sintering temperature may be 730°C-800°C, for example, 730°C, 760°C or 800°C.
[0088] In the present invention, the heating rate of the sintering may be 3-8°C / min, for example 5°C / min.
[0089] In the present invention, the sintering time may be 5 h-20 h, for example 12 h.
[0090] In the present invention, the sintering may be performed under an inert atmosphere, such as nitrogen, and the purity of the nitrogen is preferably 99.999%.
[0091] In the present invention, the mesh size of the sieve used for the screening may be 150-400 meshes, for example, 300 meshes.
[0092] In the present invention, during the crushing process of the upper screened material, the air flow crushing frequency may be 100 HZ-140 HZ, such as 100 HZ, 120 HZ or 140 HZ.
[0093] In the present invention, during the crushing process of the lower layer screening material, the air flow crushing frequency is 140HZ-180HZ, such as 140HZ, 160 or 180HZ.
[0094] The present invention provides a lithium iron phosphate, which is prepared by the preparation method as described above.
[0095] The present invention provides the use of the lithium iron phosphate as described above in a positive electrode material for a lithium ion battery.
[0096] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0097] The reagents and raw materials used in the present invention are commercially available.
[0098] The positive and progressive effects of the present invention are:
[0099] The lithium iron phosphate obtained by the subsequent steps of the lithium iron phosphate precursor provided by the present invention has a high compaction density and good electrical properties. When it is applied to a battery, the battery's charge specific capacity and discharge specific capacity are close at the same rate, indicating that the battery has a small energy loss during the charge and discharge process and has good battery performance. In addition, the preparation method provided by the present invention is simple and can achieve stable industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0100] Figure 1 This is a SEM image of the lithium iron phosphate prepared in Example 1.
[0101] Figure 2 This is the SEM image of the lithium iron phosphate prepared in Comparative Example 4. DETAILED DESCRIPTION
[0102] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0103] Preparation methods of embodiments and comparative examples
[0104] (1) A 62% phosphoric acid solution and titanium dioxide are mixed, and reduced iron powder is added, and the mixture is stirred at 85° C. to react. Gas is generated during the reaction, and the material is then put into a sand mill for sand grinding. The grinding beads in the sand mill are 0.3 mm zirconium oxide beads to obtain product A, wherein the molar ratio of iron element to phosphoric acid is 0.995:1; wherein the molar ratio of titanium element to iron element is 1.15:100;
[0105] (2) A 30% malic acid solution, lithium carbonate and polyethylene glycol are mixed and reacted at 55° C. until no gas is generated to obtain a product B; wherein the molar ratio of lithium element to phosphoric acid is 1.03:1; the mass of polyethylene glycol is 15%, and the percentage is the mass of polyethylene glycol to the mass of phosphoric acid; the amount of malic acid added is 32%, and the percentage is the mass of malic acid to the mass of phosphoric acid;
[0106] (3) mixing the above product A with the product B, and then dividing the mixture into two parts, respectively grinding them to obtain component I and component II, and then mixing component I with component II to obtain a lithium iron phosphate precursor;
[0107] (4) The lithium iron phosphate precursor is spray-dried and sintered in sequence, and then the sintered material is sieved using a 300-mesh sieve to obtain an upper sieved material and a lower sieved material, and then the upper sieved material and the lower sieved material are crushed separately and then mixed to obtain lithium iron phosphate.
[0108] Embodiment 14
[0109] The difference from Example 1 is that no catalyst titanium dioxide is added.
[0110] Embodiment 15
[0111] The difference from Example 1 is that the reduced iron powder in step (1) is replaced by ferric oxide.
[0112] Example 16
[0113] The difference from Example 1 is that the molar ratio of iron element to phosphoric acid in step (1) is replaced with 0.98:1.
[0114] Embodiment 17
[0115] The difference from Example 1 is that the malic acid solution in step (2) is replaced by polyacrylic acid.
[0116] Embodiment 18
[0117] The difference from Example 1 is that the lithium carbonate in step (2) is replaced by lithium hydroxide monohydrate.
[0118] Embodiment 19
[0119] The difference from Example 1 is that the polyethylene glycol in step (2) is replaced by sucrose.
[0120] Embodiment 20
[0121] The difference from Example 1 is that the molar ratio of lithium element to phosphoric acid in step (2) is replaced with 1.01:1.
[0122] Other specific process parameters are shown in Table 1.
[0123] Effect Example 1
[0124] 1. Particle size
[0125] The particle size was tested using a laser particle size analyzer with a refractive index of 1.8%. The equipment model was Malvern 3000. The test results are shown in Table 2.
[0126] 2. Resistivity
[0127] The resistivity of the lithium iron phosphate powder obtained in all the embodiments and comparative examples was tested using a powder resistivity tester (model: ST2742B). The test method was a four-probe test, the test pressure was 8 MPa, and the test results are shown in Table 2.
[0128] 3. Carbon content
[0129] Refer to the national standard: GBT 223.86-2009 Determination of total carbon content of steel and alloys - Infrared absorption method after induction furnace combustion. (Equipment manufacturer, Keguo Instrument, model: HCS-500), the test results are shown in Table 2.
[0130] 4. Compacted density
[0131] The compaction density of lithium iron phosphate powder was tested by an electronic pressure testing machine (model UTM7305Z09) with pressure parameters of 10 kN, 20 kN and 30 kN. The compaction density of the powder under a pressure of 30 kN was taken as the test result. The test results are shown in Table 2.
[0132] Effect Example 2
[0133] Preparation of button cells
[0134] (1) The lithium iron phosphate material, conductive carbon black and polyvinylidene fluoride of the embodiment and comparative example were dispersed in NMP solution at a mass ratio of 90:5:5, and stirred in a vacuum mixer for 3 hours, and the solid content of the slurry was controlled to be 50% to prepare a positive electrode slurry. The positive electrode slurry was evenly coated on aluminum foil, and then placed in a vacuum drying oven at 120°C for 12 hours. After drying, it was punched into discs with a diameter of 12 mm as positive electrode sheets.
[0135] 2) A metal lithium sheet was used as the negative electrode, a Celgard 2400 microporous membrane was used as the separator, and a 1.0 mol / L LiPF6 solution was used as the electrolyte. The solvent of the electrolyte was prepared by mixing ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) in a volume ratio of 1:1:1. The positive electrode sheet, negative electrode sheet, separator and electrolyte were assembled into a CR2016 button cell in an argon-filled glove box.
[0136] The button cell prepared by the above method was used to test the electrical performance. During the test, the cut-off voltage of the charging process was 3.75V, and the cut-off voltage of the discharging process was 2.0V. Equipment manufacturer: Newwell Electronics Co., Ltd., equipment specification: 5V / 10mA
[0137] Charge at a constant current of 0.1C to a voltage of 3.75V, then switch to constant voltage charging to a current of 0.02C, and discharge at a constant current of 0.1C to a voltage of 2.0V. Record the 0.1C charge specific capacity and 0.1C discharge specific capacity as the test results.
[0138] The battery was charged at a constant current of 1C until the voltage reached 3.75V, then switched to constant voltage charging until the current reached 0.02C, and discharged at a constant current of 1C until the voltage reached 2.0V. The 1C discharge specific capacity was recorded as the test result. The test results are shown in Table 2.
[0139] Table 1
[0140]
[0141] Table 2
[0142]
[0143] It can be seen from Table 2 that the lithium iron phosphate prepared by the preparation method provided by the present invention has low resistivity (6.14-9.14Ω•cm) and high compaction density (2.561-2.696 g / cm 3) advantage, when applied to the battery, the battery's 0.1C charge capacity is 160.1-162.3 mAh / g, and the 0.1C discharge capacity is 157.1-159.4 mAh / g. It can be seen that at 0.1C, the charge capacity and discharge capacity are close, indicating that the battery has less energy loss during the charge and discharge process and the battery performance is better.
[0144] Figure 1 This is a SEM image of the lithium iron phosphate prepared in Example 1. Figure 2 The SEM image of lithium iron phosphate prepared in comparative example 4. Combining the data in Table 1 and Table 2, it can be seen that the large primary particles of lithium iron phosphate are crucial to improve the compaction density of the powder. In the presence of large particles, small particles are evenly distributed in the middle of the gaps between the large particles, thereby effectively improving the compaction density of the powder. It is difficult to effectively grade the sintered material using a one-step crushing process. Due to the constant crushing process, the large primary particles will be crushed by the air flow intensity to form multiple small primary particles. There are many exposed lithium iron phosphate sections in such small primary particles, thereby forming defects. At the same time, this crushing process cannot crush the agglomerated small primary particles. These agglomerated small particles cannot be effectively dispersed to fill the gaps between the large particles, resulting in the inability to improve the compaction density of the powder. When the compaction density of the powder is low, there are a large number of gaps between the primary particles of lithium iron phosphate, the filling rate per unit volume becomes low, and the transmission path of lithium ions and electrons will be lengthened, resulting in a decrease in the electrical properties of the material. Increasing the compaction density of the powder can also improve the electrical properties at the same time, and there will be significant improvements in improving the energy density.
[0145] The difference between Examples 1-5 and Comparative Examples 2-3 is that the particle sizes of component I and component II in the lithium iron phosphate precursor are different. It can be seen that changing the particle sizes of component I and component II will affect the particle sizes of the upper and lower sieved materials obtained in the subsequent steps. Changing the particle sizes of component I and component II will have a certain influence on the compaction density and electrical properties of the lithium iron phosphate powder. However, the technical effects of the present invention can be achieved within the scope of the present invention. If it is not within the scope of the present invention, it will have a greater impact on the compaction density and electrical properties.
[0146] The difference between Examples 1, 6-7 and Comparative Example 1 is that the mass ratios of component I and component II in the lithium iron phosphate precursor are different. Combined with the data in Table 2, it can be seen that the mass ratio has a greater impact on the compaction density of the powder. This may be because the proportion of large particles and small particles directly determines the filling degree of the gaps in the large particles, and it must be within an appropriate range to have a good effect.
[0147] The difference between Examples 1 and 8-9 is the sintering temperature. The sintering temperature will affect the fusion of particles. Within a certain range, increasing the sintering temperature is conducive to the fusion of particles to obtain a lithium iron phosphate product with a large and small particle size.
[0148] The difference between Examples 1, 10-13 and Comparative Examples 6-7 is that the crushing frequency of the upper screening material is different from the crushing frequency of the lower screening material, and the obtained particle sizes after crushing are also different. It can be seen that within the scope of the present invention, the materials obtained by different crushing frequencies are mixed, and their particle sizes meet the requirements of the present invention, and good compaction density and electrical properties can be achieved. If the particle size is not within the scope of the present invention, the compaction density and electrical properties are significantly reduced.
[0149] The difference between Examples 1 and 14-20 is that different types or proportions of raw materials are used, but good compaction density and electrical properties can be obtained.
[0150] The difference between Examples 1 and 21-24 is that in the final lithium iron phosphate product, the proportion of particles after the lower layer screening material is crushed is different, which will also have a certain impact on the effect.
[0151] Comparative Examples 4-5 used the traditional one-step crushing method. As mentioned above, the compaction density and electrical properties of the powder were poor.
[0152] The above-described embodiments are only preferred embodiments of the present invention, which are convenient for those skilled in the art to understand and use the present invention. Obviously, any person skilled in the art can slightly modify or change the present embodiment and apply it to other embodiments without creative work. Therefore, the present invention is not limited to the above-described embodiments, and any equal changes, simple modifications and modifications made within the scope of the present invention still belong to the scope of the present invention.
Claims
1. A method for preparing a lithium iron phosphate precursor, characterized in that: It includes the following steps: S1. reacting a mixture I including an iron source and a phosphoric acid solution, and grinding after the reaction to obtain a product A; reacting a mixture II including a first organic acid solution, a lithium source and a coating source, and obtaining a product B after the reaction is completed; the order of preparing the product A and the product B is not limited; S2. Divide the mixture of the product A and the product B into two parts, grind them separately to obtain component I and component II, and then mix component I and component II to obtain a lithium iron phosphate precursor; wherein the average particle size of component I is 800-1600nm; the average particle size of component II is 50-600nm; and the mass ratio of component I to component II is (0.25-9):
1.
2. The method for preparing a lithium iron phosphate precursor according to claim 1, characterized in that: It satisfies one or more of the following conditions (a)-(h): (a) the average particle size of component I is 1000-1500 nm; (b) the average particle size of component II is 100-300 nm; (c) the mass ratio of the component I to the component II is (0.25-9):1; (d) the reaction temperature of the mixture I is 20-95°C; (e) In the mixture I, the molar ratio of iron element to phosphoric acid is (0.94-1.05):1; (f) the molar ratio of lithium element in the lithium source to phosphoric acid in the phosphoric acid solution is (0.98-1.05):1; (g) the amount of the coating source is 1%-60%, where the percentage refers to the mass percentage of the coating source to the mass percentage of the phosphoric acid; (h) The reaction temperature of the mixture II is 20-95°C.
3. The method for preparing a lithium iron phosphate precursor according to claim 1, characterized in that: It satisfies one or more of the following conditions (a)-(g): (a) the iron source is one or more of iron powder, ferric oxide, ferrosoferric oxide and ferric nitrate; (b) the mesh size of the iron source is 100-1000 mesh; (c) the mass percentage concentration of phosphoric acid in the phosphoric acid solution is 20-85%; (d) the phosphoric acid in the phosphoric acid solution is industrial grade phosphoric acid, food grade phosphoric acid, electrical grade phosphoric acid or electronic grade phosphoric acid; (e) the first organic acid in the first organic acid solution is one or more of a carboxylic acid compound, ascorbic acid and a polymer acid; when the first organic acid includes a carboxylic acid compound, the carboxylic acid compound is one or more of formic acid, acetic acid, oxalic acid, citric acid, tartaric acid and malic acid; when the first organic acid includes a polymer acid, the polymer acid is preferably polyacrylic acid or polymethacrylic acid; (f) the lithium source is one or more of lithium hydroxide monohydrate, lithium carbonate, lithium dihydrogen phosphate, lithium phosphate and lithium acetate; (g) the coating source is one or more of a carbon material, a metal compound and a conductive polymer; Wherein, when the coating source includes a carbon material, the carbon material is glucose, a glucose derivative, a second organic acid, an organic acid derivative, a phenolic resin, polyethylene, polyethylene glycol, polyvinyl alcohol, a polyvinyl alcohol derivative, polyacrylic acid, a polyacrylic acid derivative, a heterocyclic polymer or a condensation polymer containing N or O elements; Wherein, when the coating source comprises a metal compound, the metal compound comprises aluminum oxide and / or zinc stannate; Wherein, when the coating source includes a conductive polymer, the conductive polymer includes one or more of polyaniline, polystyrene thiol, polyacetylene, lithium carbonate and polycarbonate.
4. The method for preparing a lithium iron phosphate precursor according to claim 1, characterized in that: It satisfies one or more of the following conditions (a)-(d): (a) The mixture I may further include a catalyst, wherein the catalyst is a titanium-based catalyst; (b) the mass percentage concentration of the first organic acid in the first organic acid solution is 5-98%; (c) the amount of the coating source is 1%-60%, where the percentage refers to the mass percentage of the coating source to the mass percentage of the phosphoric acid; (d) The grinding method is sand milling or ball milling.
5. A lithium iron phosphate precursor, characterized in that: It is prepared by the preparation method of the lithium iron phosphate precursor as described in any one of claims 1 to 4.
6. A method for preparing lithium iron phosphate, characterized in that: The method comprises the following steps: spray drying, sintering and crushing the lithium iron phosphate precursor as claimed in claim 5 in sequence to obtain the lithium iron phosphate; The crushing includes screening the sintered material to obtain an upper screened material and a lower screened material, and then crushing the upper screened material and the lower screened material respectively, and then mixing them to obtain the lithium iron phosphate; The particle size of the upper screening material after crushing satisfies: 1.1 μm ≤ D50 ≤ 1.80 μm; The particle size of the lower layer screening material after crushing satisfies: 0.8 μm≤D50≤1.45 μm.
7. The method for preparing lithium iron phosphate according to claim 6, characterized in that: It satisfies one or more of the following conditions (a)-(e): (a) The D50 particle size of the upper screening material after crushing is 1.1-1.6 nm; (b) The D50 particle size of the lower layer screening material after crushing is: 0.8-1.4nm; (c) In the lithium iron phosphate, the mass percentage of the particles after the lower layer of screening material is crushed is 10wt%-40wt%; (d) The particle size of the upper screening material after crushing satisfies the following requirements: D10≤0.54μm, D99≤12.5μm, Dmax≤18μm; (e) The particle size of the lower layer screening material after crushing satisfies: D10≤0.47μm; D99≤5.05μm; Dmax≤6.02μm.
8. The method for preparing lithium iron phosphate according to claim 6, characterized in that: It satisfies one or more of the following conditions (a)-(g): (a) the sintering temperature is 730°C-800°C; (b) the heating rate of the sintering is 3-8°C / min; (c) the sintering time is 5h-20h; (d) the sintering is carried out under an inert atmosphere; (e) The mesh size of the sieve used for the screening is 150-400 mesh; (f) During the crushing process of the upper screened material, the air flow crushing frequency is 100HZ-140HZ; (g) During the crushing process of the lower layer screening material, the air flow crushing frequency is 140HZ-180HZ.
9. A lithium iron phosphate, characterized in that It is prepared by the preparation method of lithium iron phosphate as described in any one of claims 6 to 8.
10. Use of the lithium iron phosphate as claimed in claim 9 in positive electrode materials for lithium ion batteries.
Citation Information
Patent Citations
Method for preparing carbon-coated lithium iron silicate composite material
CN103985867A
Lithium iron phosphate material and preparation method thereof
CN113321197A
Novel green lithium iron phosphate precursor as well as preparation method and application thereof
CN113896182A
Lithium iron phosphate precursor, lithium iron phosphate material and preparation method and application thereof
CN117133913A
Lithium iron phosphate material, preparation method and application thereof and lithium ion battery
CN118039883A
Cited By
Lithium iron phosphate positive electrode material, preparation method thereof and lithium battery
CN119890280A
Lithium iron phosphate material as well as preparation method and application thereof
CN120504303A
Lithium iron phosphate material, preparation method and application thereof
CN120504303B