Cr2AlC / MCrAlY composite coating for Ti alloy and TiAl alloy and preparation method
By depositing Cr2AlC diffusion barrier layer and MCrAlY coating on the surface of Ti alloy and TiAl alloy, the problem of oxide film damage caused by Ti element diffusion is solved, and the good oxidation resistance and interface bonding strength of the alloy at high temperature is achieved, and the coating is extended. Service time.
Patent Information
- Application Number
- CN202310607253.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-26
AI Technical Summary
The existing Ti alloy and TiAl alloy high-temperature protective coatings have damaged oxide film due to Ti element diffusion at high temperatures, reducing coating integrity and service time, and the ceramic diffusion barrier layer does not match the thermal expansion coefficient of the alloy, affecting the interface bonding strength.
Cr2AlC is used as a diffusion barrier layer, and Cr-Al-C coating is deposited by DC magnetron sputtering and vacuum heat treatment to form a Cr2AlC film, and then MCrAlY coating is deposited by multi-arc ion plating technology. Cr2AlC has a high thermal expansion coefficient and anti-oxidation properties. Ability to block the diffusion of Ti elements at high temperatures and heat-matching with the substrate and coating.
It effectively improves the high-temperature oxidation resistance of Ti alloys and TiAl alloys, enhances the interface bonding strength, extends the service time of the coating, and maintains good protective performance at high temperatures.
Smart Images

Figure CN119020723A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of high-temperature protective coatings for Ti alloys and TiAl alloys, and in particular to a Cr2AlC / MCrAlY composite coating for Ti alloys and TiAl alloys and a preparation method thereof, which is suitable for high-temperature protection of Ti alloys and TiAl alloys. Background Art
[0002] High-temperature protective coatings such as MCrAlY coatings and improved aluminide coatings will selectively oxidize Al at high temperatures, forming a dense α-Al2O3 oxide film on the surface, which has excellent high-temperature corrosion resistance. When these coatings are applied to TiAl, they can effectively improve the high-temperature oxidation resistance of the alloy. However, due to the high activity of Ti at high temperatures, it can diffuse to the surface of the coating in a short time to form rutile-TiO2. The formation of rutile-TiO2 will destroy the integrity of the α-Al2O3 oxide film, which will aggravate the reduction of Al reserves in the coating and reduce the service life. In addition, O diffuses inward along TiO2, resulting in internal oxidation. The formation of brittle oxides will be detrimental to the integrity of the coating. More O enters the interior, and the coating eventually loses its protective ability and fails.
[0003] Therefore, the diffusion barrier between Ti alloy and TiAl alloy and high temperature protective coating is the key to inhibit the diffusion of Ti in Ti alloy and TiAl alloy and matrix elements that endanger the integrity of oxide film into coating. In addition, the diffusion barrier needs to act as a transition layer to relieve interface stress in order to achieve thermodynamic and kinetic balance between different phases. The material system suitable for diffusion barrier must have the following characteristics: ① stability at high temperature, ② thermal matching with matrix alloy and surface coating, and ③ ability to block and block ions from passing through matrix alloy / coating interface. Ceramic systems, such as TiC, TiN, Ti5Si3, Cr2O3, Al2O3, etc., are the focus of current research due to their good structural stability and antioxidant ability. However, the thermal expansion coefficient of ceramic system is quite different from that of alloy, and the interface bonding force is poor, which seriously affects the bonding strength of surface coating and the integrity during thermal cycle. For this reason, people have proposed the solution of active ceramic diffusion barrier, that is, a non-stoichiometric compound film with good toughness is deposited at the beginning, which is transformed into a stable and dense oxide film (such as Al2O3 and Cr2O3) during service. However, due to the intrinsic brittleness of conventional oxide, carbide, and nitride ceramics, as well as limited interfacial reactions with the matrix alloy and surface coating, such systems usually have an adverse effect on the adhesion of the coating. In summary, the ideal diffusion barrier layer should have a good ability to block the diffusion of matrix elements, while having a high interfacial bonding strength with the substrate and the protective coating, but the two are mutually restrictive. If the barrier layer completely blocks the diffusion of elements, it will affect the formation of a protective film at the interface and the bonding performance of the protective coating with the substrate. In addition, there is also the problem of the formation of harmful precipitate phases in long-term high-temperature diffusion reactions. Therefore, to date, the research progress and practical application of diffusion barriers between Ti alloys and TiAl alloys and high-temperature protective coatings are very limited, and there is an urgent need to develop new material systems. Summary of the invention
[0004] The purpose of the present invention is to provide a Cr2AlC / MCrAlY composite coating for Ti alloy and TiAl alloy and a preparation method thereof, so as to improve the high temperature oxidation resistance of Ti alloy and TiAl alloy, ensure their service performance in high temperature environment, solve the problem of thermal expansion coefficient mismatch between MCrAlY coating and Ti alloy and TiAl alloy, Cr2AlC has good ability to block the diffusion of matrix elements, and has good thermal matching with the matrix and protective coating, and has high interface bonding strength.
[0005] The technical solution of the present invention is as follows:
[0006] A Cr2AlC / MCrAlY composite coating for Ti alloy and TiAl alloy, the composite coating comprises a Cr2AlC diffusion barrier layer and an MCrAlY protective coating deposited on a Ti alloy or TiAl alloy substrate, the thickness of the Cr2AlC diffusion barrier layer is 2-20 μm, the thickness of the MCrAlY coating is 10-50 μm, and M is Ni, Co or Ni+Co.
[0007] The Cr2AlC / MCrAlY composite coating for Ti alloy and TiAl alloy selects Cr2AlC phase as the diffusion barrier layer of the Ti alloy and TiAl alloy / high temperature protective coating to improve its service performance.
[0008] The method for preparing the Cr2AlC / MCrAlY composite coating for Ti alloy and TiAl alloy comprises the following steps:
[0009] (1) selecting a target material with an atomic ratio of Cr, Al, and C of 2:1:1, and using DC magnetron sputtering to deposit a Cr-Al-C coating with an atomic ratio of Cr, Al, and C of 2:1:1 on a mechanically ground and cleaned Ti alloy or TiAl alloy;
[0010] (2) vacuum heat treatment at a temperature of 650°C ± 50°C for 1 to 20 hours, so that the main phase of the Cr-Al-C coating is Cr2AlC;
[0011] (3) MCrAlY coating is deposited on Ti alloy or TiAl alloy with Cr2AlC coating by multi-arc ion plating technology.
[0012] The method for preparing the Cr2AlC / MCrAlY composite coating for Ti alloy and TiAl alloy, in step (1), the conditions of DC magnetron sputtering are: the back vacuum pressure is ≤2×10 -4 Pa, Ar gas pressure 0.20~0.40Pa, Ar gas flow rate 10~20SCCM, power 80~120W.
[0013] The method for preparing the Cr2AlC / MCrAlY composite coating for Ti alloy and TiAl alloy obtains a diffusion barrier layer whose main phase is Cr2AlC after the vacuum heat treatment in step (2).
[0014] In the method for preparing the Cr2AlC / MCrAlY composite coating for Ti alloy and TiAl alloy, preferably, in step (2), the thickness of the diffusion barrier layer is 2 to 10 μm.
[0015] The method for preparing the Cr2AlC / MCrAlY composite coating for Ti alloy and TiAl alloy, in step (3), the deposition parameters of the multi-arc ion plating are: arc current 70A, substrate temperature 200-250°C, DC pulse bias -20V, Ar gas partial pressure 0.1-0.2Pa, substrate bias -600V, and duty cycle 20%.
[0016] In the method for preparing the Cr2AlC / MCrAlY composite coating for Ti alloy and TiAl alloy, preferably, in step (3), the thickness of the MCrAlY coating is 20 to 40 μm.
[0017] The design concept of the present invention is:
[0018] Cr2AlC has good toughness and high thermal expansion coefficient (13.3×10 -6 K -1 ), and has excellent antioxidant properties. The Cr-Al bond in Cr2AlC is weak, and the diffusion rate of Al along the basal plane of the Cr2AlC crystal is high. At high temperatures, due to the rapid loss of Al, the Cr2AlC film undergoes a phase transition, namely: Cr2AlC film → Cr-C compound / Cr2AlC film / Cr-C compound → Cr-C compound. Due to the formation of strong covalent Cr-C compounds (mainly Cr7C3), Cr-C compounds react with Ti elements at high temperatures, namely Cr-C+Ti→TiC+Cr. The formation of TiC can not only effectively absorb Ti, but TiC itself can also play a role in blocking the mutual diffusion of elements. Therefore, it can be inferred that the application of Cr2AlC can play a role in blocking the mutual diffusion of elements.
[0019] The advantages and beneficial effects of the present invention are:
[0020] 1. The Cr2AlC of the present invention has excellent anti-oxidation performance. As a diffusion barrier layer, Cr2AlC has the following three advantages:
[0021] (1) Cr2AlC and the Cr-C compounds (Cr7C3, Cr3C2, Cr2C) and TiC produced by phase transformation can effectively prevent the mutual diffusion of elements (Ti, Al, Cr, etc.) between the high-temperature protective coating and the substrate.
[0022] (2) The Cr2AlC and the Cr-C compounds (Cr7C3, Cr3C2, Cr2C) and TiC produced by phase transformation of the present invention have good thermal matching with the NiAl coating on the TiAl alloy substrate, the MCrAlY coating and the improved aluminide coating.
[0023] (3) During the oxidation process, Al in Cr2AlC diffuses into the matrix alloy and the surface coating, strengthening the metallurgical bonding of the alloy matrix / Cr2AlC and Cr2AlC / high-temperature protective coating interfaces and enhancing the interface strength. Therefore, Cr2AlC has potential comprehensive performance advantages as an active diffusion barrier.
[0024] 2. The composite coating involved in the present invention has good high-temperature oxidation performance, good bonding strength and high-temperature stability, and can provide good high-temperature protection for Ti alloys and TiAl alloys. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The XRD spectrum of the Cr2AlC coating on the Ti-45Al-2Mn-2Nb-0.8% vol.% TiB2 alloy (the alloy grade of this embodiment is 45XD) prepared in Example 1 of the present invention shows that Cr2AlC is the main phase in the diffusion barrier layer. In the figure, the horizontal axis 2-Theta (degrees) represents the diffraction angle, and the vertical axis Intensity (au) represents the relative intensity.
[0026] Figure 2 The XRD spectrum of the Cr2AlC coating on the Ti-6Al-4Sn-9Zr-1.21Nb-1.6W-0.3Si alloy (the alloy grade of this embodiment is Ti65) prepared in Example 2 of the present invention shows that Cr2AlC is the main phase in the diffusion barrier layer. In the figure, the horizontal axis 2-Theta (degrees) represents the diffraction angle, and the vertical axis Intensity (au) represents the relative intensity.
[0027] Figure 3 The cross-sectional morphology and element distribution results of the NiCrAlY coating / Cr2AlC diffusion barrier layer / 45XD alloy system prepared in Example 1 of the present invention after oxidation at 900°C / 1000h in air.
[0028] Figure 4 The cross-sectional morphology and element distribution results of the NiCrAlY coating / Cr2AlC diffusion barrier layer / Ti65 alloy) system prepared in Example 2 of the present invention after oxidation at 800°C / 500h in air. DETAILED DESCRIPTION
[0029] In the specific implementation process, the present invention proposes a Cr2AlC / MCrAlY composite coating for Ti alloy and TiAl alloy and a preparation method thereof, and the specific operation steps are as follows:
[0030] 1) Mechanically grind the surface of the metal substrate to make it flat and clean it.
[0031] 2) Using physical vapor deposition technology - magnetron sputtering, a Cr-Al-C coating with a Cr, Al, and C atomic ratio of 2:1:1 was prepared on the substrate. The deposition conditions were: the back vacuum pressure ≤ 2×10 -4 Pa, Ar gas pressure 0.20~0.40Pa, Ar gas flow rate 15SCCM, power 80~120W, and the substrate is not heated during deposition.
[0032] 3) The sample prepared in the previous step is subjected to vacuum heat treatment to crystallize the Cr-Al-C coating into a Cr2AlC diffusion barrier layer.
[0033] 4) MCrAlY coating was deposited on Ti alloy or TiAl alloy with Cr2AlC coating by multi-arc ion plating technology. The main deposition parameters were: arc current 70A, substrate temperature 200-250°C, DC pulse bias -20V, Ar gas partial pressure 0.1-0.2Pa, substrate bias -600V, and duty cycle 20%.
[0034] The present invention is further described in detail below through examples and drawings.
[0035] Embodiment 1:
[0036] In this embodiment, the preparation method of the Cr2AlC / NiCrAlY composite coating is as follows:
[0037] A target material with an atomic ratio of Cr, Al, and C of 2:1:1 was selected, and a Cr-Al-C coating with an atomic ratio of Cr, Al, and C of 2:1:1 and a thickness of 4 μm was deposited on a mechanically ground and cleaned TiAl alloy (the alloy grade of the substrate in this embodiment is TiAl 45XD); the prepared sample was subjected to a vacuum heat treatment at 700°C / 1h, and cooled to 25°C in the furnace to crystallize the Cr-Al-C coating into a Cr2AlC diffusion barrier layer.
[0038] The main deposition parameters of magnetron sputtering Cr-Al-C are: back vacuum pressure 1×10 -4 Pa, Ar gas pressure 0.35Pa, Ar gas flow rate 15SCCM, power 80W, and the substrate is not heated during deposition.
[0039] The main deposition parameters of multi-arc ion plating NiCrAlY coating are: arc current 70A, substrate temperature 210℃, DC pulse bias -20V, Ar gas partial pressure 0.16Pa, substrate bias -600V, duty cycle 20%, and the thickness of NiCrAlY coating is 23μm.
[0040] like Figure 1 As shown, the XRD spectrum of the prepared Cr2AlC barrier layer shows that the main phase is Cr2AlC.
[0041] like Figure 3 As shown, from the cross-sectional morphology and element distribution results of the NiCrAlY coating / Cr2AlC diffusion barrier layer / TiAl alloy (45XD) system prepared in Example 1 after oxidation at 900°C / 100h in air, it can be seen that there is no crack at the interface of the NiCrAlY coating / Cr2AlC diffusion barrier layer / 45XD, and the combination is very good, which can effectively prevent Ti from diffusing from the substrate to the coating, and form a dense α-Al2O3 oxide film on the NiCrAlY coating.
[0042] Embodiment 2:
[0043] In this embodiment, the preparation method of the Cr2AlC / NiCrAlY composite coating is as follows:
[0044] A target material with an atomic ratio of Cr, Al, and C of 2:1:1 was selected, and DC magnetron sputtering was used to deposit a Cr-Al-C coating with an atomic ratio of Cr, Al, and C of 2:1:1 and a thickness of 4 μm on a mechanically ground and cleaned Ti alloy (the alloy grade of the substrate in this embodiment is Ti65); the prepared sample was subjected to a vacuum heat treatment at 620°C / 20h, and cooled to 25°C in the furnace to crystallize the C-Al-C coating into a Cr2AlC diffusion barrier layer.
[0045] The main deposition parameters of magnetron sputtering Cr-Al-C are: back vacuum pressure 1×10 -4 Pa, Ar gas pressure 0.35Pa, Ar gas flow rate 15SCCM, power 80W, and the substrate is not heated during deposition.
[0046] The main deposition parameters of multi-arc ion plating NiCrAlY are: arc current 70A, substrate temperature 220℃, DC pulse bias -20V, Ar gas partial pressure 0.12Pa, substrate bias -600V, duty cycle 20%, and the thickness of NiCrAlY coating is 35μm.
[0047] like Figure 2 As shown, the XRD pattern of the prepared Cr2AlC coating shows that the main phase is Cr2AlC.
[0048] like Figure 4 As shown, from the cross-sectional morphology and element distribution results of the NiCrAlY coating / Cr2AlC diffusion barrier layer / Ti alloy (Ti65) system prepared in Example 2 after 800°C / 100h oxidation in air, it can be seen that there is no crack at the interface of the NiCrAlY coating / Cr2AlC diffusion barrier layer / Ti65 alloy, and the combination is very good, which can effectively prevent the diffusion of Ti elements from the substrate into the coating, and form a dense α-Al2O3 oxide film on the NiCrAlY coating.
[0049] The results of the examples show that Cr2AlC, as a diffusion barrier layer of MCrAlY coating / Ti alloy or TiAl alloy, can effectively prevent Ti in the substrate from diffusing into the coating, thereby improving the high-temperature oxidation resistance. Therefore, the MCrAlY / Cr2AlC composite coating is a high-temperature protective coating with excellent performance.
Claims
1. A Cr for Ti alloy and TiAl alloy 2 AlC / MCrAlY composite coating, It is characterized in that The composite coating comprises Cr deposited on a Ti alloy or TiAl alloy substrate. 2 AlC diffusion barrier layer and MCrAlY protective coating, Cr 2 The thickness of the AlC diffusion barrier layer is 2-20 μm, the thickness of the MCrAlY coating is 10-50 μm, and M is Ni, Co or Ni+Co.
2. The Cr2O3 for Ti alloy and TiAl alloy according to claim 1 2 AlC / MCrAlY composite coating, It is characterized in that Select Cr 2 The AlC phase serves as a diffusion barrier layer for Ti alloy and TiAl alloy / high temperature protective coating to improve its service performance.
3. A Cr for Ti alloy and TiAl alloy according to claim 1 or 2 2 Preparation method of AlC / MCrAlY composite coating, It is characterized in that The steps include: (1) selecting a target material with an atomic ratio of Cr, Al, and C of 2:1:1, and using DC magnetron sputtering to deposit a Cr-Al-C coating with an atomic ratio of Cr, Al, and C of 2:1:1 on a mechanically ground and cleaned Ti alloy or TiAl alloy; (2) Vacuum heat treatment at 650℃±50℃ for 1 to 20h to make the main phase of the Cr-Al-C coating crystallized into Cr 2 AlC; (3) Using multi-arc ion plating technology to apply Cr 2 MCrAlY coating is deposited on AlC coated Ti alloy or TiAl alloy.
4. The Cr2O3 for Ti alloy and TiAl alloy according to claim 3 2 Preparation method of AlC / MCrAlY composite coating, It is characterized in that In step (1), the conditions for DC magnetron sputtering are: the back vacuum pressure is ≤ 2×10 -4 Pa, Ar gas pressure 0.20~0.40Pa, Ar gas flow rate 10~20SCCM, power 80~120W.
5. The Cr2O3 for Ti alloy and TiAl alloy according to claim 3 2 Preparation method of AlC / MCrAlY composite coating, It is characterized in that After vacuum heat treatment in step (2), the main phase is Cr 2 Diffusion barrier of AlC.
6. The Cr2O3 for Ti alloy and TiAl alloy according to claim 5 2 Preparation method of AlC / MCrAlY composite coating, It is characterized in that Preferably, in step (2), the thickness of the diffusion barrier layer is 2 to 10 μm.
7. The Cr2O3 for Ti alloy and TiAl alloy according to claim 3 2 Preparation method of AlC / MCrAlY composite coating, It is characterized in that In step (3), the deposition parameters of multi-arc ion plating are: arc current 70A, substrate temperature 200-250°C, DC pulse bias -20V, Ar gas partial pressure 0.1-0.2Pa, substrate bias -600V, and duty cycle 20%.
8. The Cr2O3 for Ti alloy and TiAl alloy according to claim 7 2 Preparation method of AlC / MCrAlY composite coating, It is characterized in that Preferably, in step (3), the thickness of the MCrAlY coating is 20 to 40 μm.
Citation Information
Cited By
Curved surface type inner surface heterogeneous hierarchical coating and preparation method thereof
CN120866796A