High-brightness hanging nickel plating solution and chemical nickel plating method
By adding softener, main light agent, wetting agent and brightening additive to the nickel plating solution to adjust the pH value, the problem of insufficient brightness and flatness of the nickel plating solution is solved, and the high brightness and stability of the plating layer is improved. Suitable for high demand nickel-plated workpieces.
Patent Information
- Application Number
- CN202411121317.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
AI Technical Summary
The existing nickel plating solution is difficult to meet the needs of high brightness and flatness, the coating is hard and difficult to process, and it lacks tolerance for impurities.
Adopt the formula of high-gloss hanging nickel plating liquid, including nickel sulfate, nickel chloride, boric acid, softener, main light agent and wetting agent, and adjust within the appropriate pH range, and add brightening additives such as N-methyl-2 -Pyridone and sodium dihydrogen phosphate, citric acid to improve the brightness and stability of the coating.
Significantly improve the brightness, flatness and adhesion stability of the plating layer, increase the tolerance of the plating solution to impurities, extend the service life of the nickel liquid, and form a more uniform and smooth plating layer.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present application relates to the field of electroplating technology, and in particular to a high-brightness rack nickel plating solution and a chemical nickel plating method. Background Art
[0002] Chemical nickel plating technology is a surface treatment process in which a layer of nickel is plated on the surface of a workpiece. The nickel plating layer has high stability in the air, and because the metal nickel has a strong passivation ability, a very thin passivation film can be quickly formed on the surface, which can resist corrosion from the atmosphere, alkali and some acids. Since the nickel plating layer has a relatively high hardness and high chemical stability, it is often used in the printing industry to increase the hardness of the surface of the workpiece, and a thicker nickel plating layer is also plated on the surface of some chemical equipment to reduce corrosion damage to the surface of the equipment. In addition, the nickel plating layer can also be used as a protective decorative coating. It is applied to the surface of steel, zinc die castings, aluminum alloys and copper alloys to protect the base material from corrosion or to provide a bright decorative effect.
[0003] Bright nickel plating for decorative purposes requires the surface of the plating to have a mirror-like glossy appearance, and at the same time requires the surface of the plating to be overall flat, without scratches and gaps. In the prior art, nickel plating liquid usually uses nickel sulfate, boric acid, etc. as the main components of the rack nickel plating liquid, but the brightness of the rack nickel plating layer is not very high, which is difficult to meet the needs of products with special requirements, and the plating layer is relatively hard, which is difficult to meet the needs of workpieces that need post-plating processing. Summary of the invention
[0004] In view of the above technical problems, the present application provides a high-brightness rack nickel plating solution and a chemical nickel plating method. In the first aspect, the present application provides a high-brightness rack nickel plating solution, which adopts the following technical solution: A high-brightness rack nickel plating solution comprises the following components in concentrations: 220-270 g / L of nickel sulfate, 45-55 g / L of nickel chloride, 45-60 g / L of boric acid, 8-15 ml / L of softener, 0.3-0.7 ml / L of primary brightener, and 1-3 ml / L of wetting agent.
[0005] By adopting the above technical scheme, nickel sulfate and nickel chloride are used as the main materials of the nickel plating solution, and a certain amount of softener, main brightener and wetting agent are added thereto. The addition of the main brightener can control the brightness and filling degree of the coating, so that the nickel coating has a higher brightness and filling effect; the addition of the softener can reduce the internal stress of the coating, while increasing the ductility of the coating and the covering ability in the low current density area. At the same time, the softener can also improve the tolerance of the plating solution to impurities to a certain extent, and improve the performance of the coating. The wetting agent is mainly used as a surfactant, which can improve the wetting performance of the nickel liquid on the surface of the workpiece and prevent pinholes from appearing on the coating. The amount of the main brightener added should not be too high, otherwise it will cause pinholes to be relatively easy to form on the coating, and it is easy to leak plating and blacken in some areas; and the appropriate increase in the amount of softener added can further improve the tolerance of the plating solution to impurities.
[0006] Optionally, the softener is one or both of saccharin and sodium allyl sulfonate.
[0007] Optionally, the primary light agent is one or both of 1,4-butynediol and benzyl acetone.
[0008] Optionally, the wetting agent is one or more combinations of sodium dodecyl sulfate, polyethylene glycol, and sodium isooctyl sulfate.
[0009] Optionally, the pH value of the high-brightness nickel plating solution is 3.5-4.5.
[0010] By adopting the above technical solution and adjusting the pH value of the nickel plating solution to the above range, the nickel solution can have better stability, the precipitation of impurities and precipitates in the nickel plating solution can be reduced, and the nickel layer has better film-forming properties within this pH range, and the formed coating is more uniform and stable.
[0011] Optionally, the high-brightness rack nickel plating solution further includes a brightening additive with a concentration of 0.5-1.5 g / L, and the brightening additive includes one or more combinations of N-methyl-2-pyridone, diethanolamine and sodium dihydrogen phosphate.
[0012] Optionally, the brightening additive includes N-methyl-2-pyridone, diethanolamine and sodium dihydrogen phosphate, and the mass ratio of N-methyl-2-pyridone, diethanolamine and sodium dihydrogen phosphate is (0.1-1):(1-5):(1-3).
[0013] By adopting the above technical scheme, the addition of brightening additives can further improve the brightness of the coating, make the nickel coating brighter, and achieve a better appearance effect. As an organic additive, N-methyl-2-pyridone can promote the reaction of nickel ions in nickel solution, improve the brightness and reflectivity of the electroplated layer; at the same time, N-methyl-2-pyridone has a certain antioxidant effect, which can reduce the oxidation reaction of nickel solution and extend the service life and stability of nickel solution. Diethanolamine can adjust the pH of nickel solution, keep the pH of the plating solution within a suitable range, stabilize the properties of nickel solution, stabilize nickel ions and other impurity ions in nickel solution, and prevent them from precipitation or precipitation; in addition, diethanolamine can also reduce the surface tension of the liquid, make the plating solution easier to wet the surface of the workpiece, and improve the adhesion and uniformity of the coating. The combined use of sodium dihydrogen phosphate and diethanolamine can further improve the stability of nickel solution and nickel plating efficiency, and ensure the long-term stability of nickel solution and electroplating quality.
[0014] Optionally, the high-brightness rack nickel plating solution also includes citric acid, and the concentration of the citric acid is 1-3 g / L.
[0015] More preferably, the mass ratio of citric acid to N-methyl-2-pyridone is (8-12):1.
[0016] By adopting the above technical solution, citric acid can be used as a buffer in the nickel solution to adjust the pH value of the nickel solution, so that it is kept within an appropriate range, and the pH of the electroplating solution is prevented from being too high or too low, thereby affecting the stability of the nickel solution. Citric acid can form a complex with nickel ions in the plating solution, thereby improving the stability and activity of nickel ions in the nickel solution, promoting the formation and deposition of the coating, improving the brightness and uniformity of the coating, inhibiting the sawtooth effect that occurs during the nickel plating process, making the coating smoother, and improving the quality of the coating. N-methyl-2-pyridone can promote the effect of citric acid in inhibiting sawtooth, further improving the smoothness of the coating.
[0017] In a second aspect, the present application provides a chemical nickel plating method, which adopts the following technical solution: A chemical nickel plating method comprises the following steps: S1. According to the ratio, nickel chloride, boric acid and sulfuric acid are added to hot pure water in sequence and dispersed evenly, then activated carbon powder is added and filtered, and then softener, primary brightener and wetting agent are added to prepare a nickel plating solution; S2, after the workpiece is hung, it is subjected to degreasing, water washing and pickling in sequence to remove stains and oxides on the surface of the workpiece; S3, activating and pre-treating the cleaned workpiece, and then sending it into a working tank filled with nickel plating solution for electroplating; S4. The nickel plating process is completed after the electroplated parts are polished, passivated and dried.
[0018] Optionally, in step S3, the temperature of the nickel plating solution is 55-65°C.
[0019] In summary, the present application includes at least one of the following beneficial technical effects: 1. In the technical solution of the present application, a softener, a main brightener and a wetting agent are added to nickel sulfate, nickel chloride and boric acid, and the addition ratio of the softener is increased to a certain extent, which can significantly improve the brightness and filling degree of the coating. In addition, when the addition ratio of the softener is increased, the tolerance of the plating solution to impurities can be improved, and the adhesion stability and uniformity of the coating on the surface can be improved.
[0020] 2. Further add brightening additives. The addition of brightening additives can further improve the brightness of the coating, make the nickel coating brighter, and achieve better aesthetic effects. N-methyl-2-pyridone, as an organic additive, can promote the reaction of nickel ions in nickel solution, improve the brightness and reflectivity of the electroplated layer; at the same time, N-methyl-2-pyridone has a certain antioxidant effect, which can reduce the oxidation reaction of nickel solution and extend the service life and stability of nickel solution. Diethanolamine can adjust the pH of nickel solution, keep the pH of the plating solution within a suitable range, stabilize the properties of nickel solution, stabilize nickel ions and other impurity ions in nickel solution, and prevent them from precipitation or precipitation; in addition, diethanolamine can also reduce the surface tension of the liquid, make the plating solution easier to wet the surface of the workpiece, and improve the adhesion and uniformity of the coating. The combined use of sodium dihydrogen phosphate and diethanolamine can further improve the stability of nickel solution and nickel plating efficiency, and ensure the long-term stability of nickel solution and electroplating quality.
[0021] 3. Further add citric acid. Citric acid can be used as a buffer in nickel solution to adjust the pH value of nickel solution, keep it within an appropriate range, and prevent the pH of the electroplating solution from being too high or too low, which affects the stability of the nickel solution. Citric acid can form a complex with nickel ions in the plating solution, thereby improving the stability and activity of nickel ions in the nickel solution, promoting the formation and deposition of the coating, improving the brightness and uniformity of the coating, inhibiting the sawtooth effect during the nickel plating process, making the coating smoother, and improving the quality of the coating. N-methyl-2-pyridone can promote the effect of citric acid in inhibiting sawtooth, further improving the smoothness of the coating. DETAILED DESCRIPTION
[0022] The present application is further described in detail below in conjunction with specific examples. It should be noted that, if no specific conditions are specified in the following examples, all are carried out under conventional conditions or conditions recommended by the manufacturer; the raw materials used in the following examples can be obtained from common commercial sources unless otherwise specified.
[0023] Example 1 A high-brightness rack nickel plating solution comprises components with the following concentrations: 220 g / L nickel sulfate, 55 g / L nickel chloride, 45 g / L boric acid, 8 ml / L softener, 0.7 ml / L main brightener, and 1 ml / L wetting agent.
[0024] Among them, the softener is sodium allyl sulfonate, the main brightener is 1,4-butynediol, and the wetting agent is sodium dodecyl sulfate.
[0025] Example 2 A high-brightness rack nickel plating solution comprises components with the following concentrations: 270 g / L nickel sulfate, 45 g / L nickel chloride, 60 g / L boric acid, 15 ml / L softener, 0.3 ml / L main brightener, and 3 ml / L wetting agent.
[0026] Among them, the softener is sodium allyl sulfonate, the main brightener is 1,4-butynediol, and the wetting agent is sodium dodecyl sulfate.
[0027] Example 3 A high-brightness rack nickel plating solution comprises components with the following concentrations: 270 g / L nickel sulfate, 50 g / L nickel chloride, 45 g / L boric acid, 10 ml / L softener, 0.4 ml / L primary brightener, and 2 ml / L wetting agent.
[0028] Among them, the softener is sodium allyl sulfonate, the main brightener is 1,4-butynediol, and the wetting agent is sodium dodecyl sulfate.
[0029] Example 4 A high-brightness rack nickel plating solution comprises components with the following concentrations: 245 g / L nickel sulfate, 55 g / L nickel chloride, 50 g / L boric acid, 12 ml / L softener, 0.6 ml / L main brightener, and 2 ml / L wetting agent.
[0030] Among them, the softener is sodium allyl sulfonate, the main brightener is 1,4-butynediol, and the wetting agent is sodium dodecyl sulfate.
[0031] Comparative Example 1 A high-brightness rack nickel plating solution comprises components with the following concentrations: 245 g / L nickel sulfate, 55 g / L nickel chloride, 50 g / L boric acid, 5 ml / L softener, 0.6 ml / L primary brightener, and 2 ml / L wetting agent.
[0032] Among them, the softener is sodium allyl sulfonate, the main brightener is 1,4-butynediol, and the wetting agent is sodium dodecyl sulfate.
[0033] Comparative Example 2 A high-brightness rack nickel plating solution comprises components with the following concentrations: 245 g / L nickel sulfate, 55 g / L nickel chloride, 50 g / L boric acid, 12 ml / L softener, 1 ml / L main brightener, and 2 ml / L wetting agent.
[0034] Among them, the softener is sodium allyl sulfonate, the main brightener is 1,4-butynediol, and the wetting agent is sodium dodecyl sulfate.
[0035] Performance testing The high-brightness nickel plating solution provided in the above embodiment and comparative example was subjected to chemical nickel plating, and then the performance parameters of the plating layer were detected, as follows: According to the ratio, take nickel chloride and slowly add it into 50℃ hot pure water, stir until completely dissolved, then slowly add boric acid while stirring, continue stirring until completely dissolved; continue to add nickel sulfate and stir until completely dissolved. Then add 3g / L activated carbon powder, stir for 30min, filter out the precipitate after standing and settling, then add softener, primary brightener, wetting agent in turn, and add 10% (v / v) dilute sulfuric acid to adjust the pH of the mixed solution to 3.5-4.5, stir and mix evenly to obtain nickel plating solution.
[0036] The specific nickel plating process is as follows: S1. Place the workpiece to be plated in a solution containing a degreasing agent, and use ultrasonic vibration to treat the oil stains on the surface of the workpiece to be plated; the degreasing agent is an acidic degreasing agent H-111, and the volume fraction of the solution is 50ml / L (the solvent is water); and the treatment is carried out at a temperature of 60°C for 10 minutes; S2, pickling and activating the degreased parts to be plated, the pickling agent includes hydrochloric acid and nitric acid, the concentration of hydrochloric acid is 100ml / L, the concentration of nitric acid is 10ml / L, the pickling activation temperature is 25°C, and the time is 10min; S3, putting the plated parts activated by pickling into an ultrasonic cleaning machine and cleaning them with pure water to remove the acid solution remaining on the surface; S4, hanging the workpiece to be plated in a plating tank containing nickel plating solution, wherein the temperature of the nickel plating solution in the plating tank is 60±5° C., performing rack nickel plating, and depositing nickel ions on the surface of the workpiece to be plated to form a uniform plating layer; S4, after the coating deposition is completed, the plated part is taken out from the plating tank and the chemical plating solution remaining on the surface is cleaned and removed; S5. After cleaning, the plated parts are placed in an oven for drying to remove surface moisture; S6. Performing surface treatment such as polishing and grinding on the coating to obtain a plated part.
[0037] Among them, the workpiece to be plated is an aluminum alloy workpiece.
[0038] The plated parts obtained above were subjected to performance testing, wherein the brightness was measured using a gloss meter; the bonding strength was tested by a bending test, where the plated parts were bent at 90° to observe whether the nickel plating layer had cracks, shedding, etc. The performance test results of Examples 1-4 and Comparative Examples 1-2 are shown in Table 1 below.
[0039] Table 1: Performance test results of Examples 1-4 and Comparative Examples 1-3 It can be seen from the data in Table 1 that by adding a softener, a main light agent and a wetting agent to the nickel solution, and controlling the addition amount of the softener and the main light agent within a suitable range, the brightness of the coating, the adhesion strength of the coating and the stability are significantly improved. Specifically, within the scope defined by the technical solution of the present application, the uniformity of the coating thickness is high, the thickness variation range is small, and the bonding force between the coating and the substrate surface is strong. After reducing the addition amount of the softener, the uniformity and adhesion performance of the coating will deteriorate, and impurity points will appear on its surface. This may be due to the decrease in the tolerance of the nickel solution to impurities, and impurities are more likely to appear on the surface of the coating. After increasing the addition amount of the main light agent, the glossiness of the coating is improved to a certain extent, but pinholes will appear on the surface of the coating, and blackening will occur locally.
[0040] Example 5 A high-brightness rack nickel plating solution comprises components with the following concentrations: 245 g / L nickel sulfate, 55 g / L nickel chloride, 50 g / L boric acid, 5 ml / L softener, 0.6 ml / L main brightener, 2 ml / L wetting agent, and 1.0 g / L brightening additive.
[0041] Among them, the brightening additive is N-methyl-2-pyridone, the softener is sodium allyl sulfonate, the main brightener is 1,4-butynediol, and the wetting agent is sodium dodecyl sulfate.
[0042] Example 6 A high-brightness rack nickel plating solution comprises components with the following concentrations: 245 g / L nickel sulfate, 55 g / L nickel chloride, 50 g / L boric acid, 5 ml / L softener, 0.6 ml / L main brightener, 2 ml / L wetting agent, and 1.0 g / L brightening additive.
[0043] Among them, the brightening additive includes a combination of N-methyl-2-pyridone, diethanolamine and sodium dihydrogen phosphate in a mass ratio of 0.5:2.5:2; the softener is sodium allyl sulfonate, the main brightener is 1,4-butynediol, and the wetting agent is sodium dodecyl sulfate.
[0044] Example 7 A high-brightness rack nickel plating solution comprises components with the following concentrations: 245 g / L nickel sulfate, 55 g / L nickel chloride, 50 g / L boric acid, 5 ml / L softener, 0.6 ml / L main brightener, 2 ml / L wetting agent, and 1.0 g / L brightening additive.
[0045] Among them, the brightening additive includes a combination of N-methyl-2-pyridone, diethanolamine and sodium dihydrogen phosphate in a mass ratio of 1:3:1; the softener is sodium allyl sulfonate, the main brightener is 1,4-butynediol, and the wetting agent is sodium dodecyl sulfate.
[0046] Example 8 A high-brightness rack nickel plating solution comprises components with the following concentrations: 245 g / L nickel sulfate, 55 g / L nickel chloride, 50 g / L boric acid, 5 ml / L softener, 0.6 ml / L main brightener, 2 ml / L wetting agent, and 1.0 g / L brightening additive.
[0047] Among them, the brightening additive includes a combination of N-methyl-2-pyridone, diethanolamine and sodium dihydrogen phosphate in a mass ratio of 1.5:0.5:5; the softener is sodium allyl sulfonate, the main brightener is 1,4-butynediol, and the wetting agent is sodium dodecyl sulfate.
[0048] Example 9 A high-brightness rack nickel plating solution comprises components with the following concentrations: 245 g / L nickel sulfate, 55 g / L nickel chloride, 50 g / L boric acid, 5 ml / L softener, 0.6 ml / L main brightener, 2 ml / L wetting agent, and 1.0 g / L brightening additive.
[0049] Among them, the brightening additive includes a combination of N-methyl-2-pyridone, diethanolamine and sodium dihydrogen phosphate in a mass ratio of 2:0.5:0.5; the softener is sodium allyl sulfonate, the main brightener is 1,4-butynediol, and the wetting agent is sodium dodecyl sulfate.
[0050] Example 10 A high-brightness rack nickel plating solution comprises components with the following concentrations: 245 g / L nickel sulfate, 55 g / L nickel chloride, 50 g / L boric acid, 5 ml / L softener, 0.6 ml / L primary brightener, 2 ml / L wetting agent, 1.0 g / L brightening additive, and 2 g / L citric acid.
[0051] Among them, the brightening additive includes a combination of N-methyl-2-pyridone, diethanolamine and sodium dihydrogen phosphate in a mass ratio of 0.5:2.5:2; the softener is sodium allyl sulfonate, the main brightener is 1,4-butynediol, and the wetting agent is sodium dodecyl sulfate.
[0052] Embodiment 11 A high-brightness rack nickel plating solution comprises components with the following concentrations: 245 g / L nickel sulfate, 55 g / L nickel chloride, 50 g / L boric acid, 5 ml / L softener, 0.6 ml / L primary brightener, 2 ml / L wetting agent, 1.0 g / L brightening additive, and 2 g / L citric acid.
[0053] Among them, the brightening additive includes a combination of N-methyl-2-pyridone, diethanolamine and sodium dihydrogen phosphate in a mass ratio of 1:3:1; the softener is sodium allyl sulfonate, the main brightener is 1,4-butynediol, and the wetting agent is sodium dodecyl sulfate.
[0054] The performance test results of Examples 5-11 are shown in Table 2 below.
[0055] Table 2: Performance test results of Examples 5-11 It can be seen from the data in Table 2 that the addition of brightening additives and citric acid improves the brightness of the coating to a certain extent, and it can be seen from the data of Examples 6 and 7 that the addition of the incremental additives according to the preferred proportions of the present application can obtain a better brightening effect, and the bonding strength of the coating is further improved.
[0056] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A high-brightness rack nickel plating solution, characterized in that: The invention comprises components of the following concentrations: nickel sulfate 220-270 g / L, nickel chloride 45-55 g / L, boric acid 45-60 g / L, softener 8-15 ml / L, main brightener 0.3-0.7 ml / L, and wetting agent 1-3 ml / L.
2. A high-brightness rack nickel plating solution according to claim 1, characterized in that: The high-brightness rack nickel plating solution also includes a brightening additive with a concentration of 0.5-1.5 g / L, and the brightening additive includes one or more combinations of N-methyl-2-pyridone, diethanolamine and sodium dihydrogen phosphate.
3. A high-brightness rack nickel plating solution according to claim 2, characterized in that: The brightening additive comprises N-methyl-2-pyridone, diethanolamine and sodium dihydrogen phosphate, and the mass ratio of N-methyl-2-pyridone, diethanolamine and sodium dihydrogen phosphate is (0.1-1): (1-5): (1-3).
4. A high-brightness rack nickel plating solution according to claim 3, characterized in that: The high-brightness rack nickel plating solution also includes citric acid at a concentration of 1-3 g / L.
5. A high-brightness rack nickel plating solution according to claim 4, characterized in that: The mass ratio of citric acid to N-methyl-2-pyridone is (8-12):
1.
6. The high-brightness rack nickel plating solution according to claim 1, characterized in that: The softener is one or both of saccharin and sodium allyl sulfonate.
7. The high-brightness rack nickel plating solution according to claim 1, characterized in that: The primary light agent is one or two of 1,4-butynediol and benzyl acetone.
8. The high-brightness rack nickel plating solution according to claim 1, characterized in that: The wetting agent is one or more combinations of sodium lauryl sulfate, polyethylene glycol, and sodium isooctyl sulfate.
9. A high-brightness rack nickel plating solution according to any one of claims 1 to 8, characterized in that: The pH value of the high-brightness nickel plating solution is 3.5-4.
5.
10. A chemical nickel plating method according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. According to the ratio, nickel chloride, boric acid and sulfuric acid are added to hot pure water in sequence and dispersed evenly, then activated carbon powder is added and filtered, and then softener, primary brightener and wetting agent are added to prepare a nickel plating solution; S2, after the workpiece is hung, it is subjected to degreasing, water washing and pickling in sequence to remove stains and oxides on the surface of the workpiece; S3, activating and pre-treating the cleaned workpiece, and then sending it into a working tank filled with nickel plating solution for electroplating; S4. The nickel-plating process is completed after the nickel-plated parts are polished, passivated and dried.