Method for preparing fiber electrode by utilizing magnet to induce Fe3O4-coated GO to carry out directional arrangement
By using Fe3O4@GO liquid crystal solution in fiber electrodes for magnet-induced rotary spinning technology, the shortcomings in mechanical and electrochemical properties of fiber electrodes are solved, and high energy density and stability are achieved. It is suitable for flexible supercapacitors and lithium ions Battery.
Patent Information
- Application Number
- CN202411135033.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-19
AI Technical Summary
The existing fiber electrodes have shortcomings in mechanical and electrochemical properties, and it is difficult to take into account high energy density and stability. Especially in flexible supercapacitors, traditional surface coating methods cause the active material to detach and affect the energy output.
By dispersing Fe3O4 nanoparticles in graphene oxide suspension, ethylenediamine regulates the distribution to form Fe3O4@GO liquid crystal solution, and bidirectional orientation arrangement is performed through magnet-induced rotary spinning technology to form Fe3O4@GO gel fiber wire , and finally dry, stretch and wind the fiber electrodes.
The prepared fiber electrode has high tensile strength and excellent electrochemical properties, significantly improved volume-specific capacitance and energy density, and has a high retention rate under mechanical bending. It is suitable for flexible supercapacitors and lithium-ion batteries.
Smart Images

Figure CN119020885A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a fiber electrode by directional arrangement of Fe3O4@GO induced by a magnet, belonging to the technical field of functional materials. Background Art
[0002] In recent years, the demand for multifunctional structural composite materials has been growing steadily, especially structural energy storage composite materials, which have attracted attention because they can withstand heavy loads and have electrical energy storage functions (such as batteries, supercapacitors, etc.). The potential application scenarios of flexible supercapacitors usually require thinness, strong deformation ability, and high deformation cycle stability, which puts forward new requirements for the electromechanical properties of supercapacitors, such as capacity retention rate, voltage output stability, structural cycle stability, and electrical properties. In this context, one-dimensional fiber supercapacitors can perfectly fill the gap and provide diverse possibilities for the field of flexible wearable electronics.
[0003] To date, the fabrication of fiber lithium-ion battery electrodes has achieved tremendous innovations, from the optimized design of active materials to device configurations. The traditional preparation method of fiber electrodes is to select a suitable linear substrate or current collector, such as metal wire, polymer-based fiber, carbon fiber, and carbon nanotube / graphene-based fiber as a supporting backbone to coat or deposit active materials. A variety of active materials (such as MnO2, MoS, Fe2O3, etc.) have been incorporated into fiber electrodes to obtain high specific capacities. At the same time, novel coaxial / twisted structures are adopted to enhance electrochemical performance, but the improvement in energy density is still far from satisfactory. In general, fiber electrodes fabricated by such surface coating methods have two major disadvantages: the additional substrate weight reduces the effective mass loading of active materials, which severely limits their overall energy density; and the interfacial adhesion between the active layer and the fiber substrate is loose, which easily leads to the detachment of active materials under deformation, resulting in unstable energy output. Therefore, fiber electrodes with both excellent flexibility and high linear / volume specific capacity have become a rarely achieved but urgently needed attribute for flexible fiber supercapacitors.
[0004] Graphene is mainly used as anode material in energy storage devices due to its two-dimensional structure and excellent physical and chemical properties, especially in lithium-ion batteries. Due to its high conductivity, extremely high specific surface area and good lithium compatibility, it greatly improves the battery's charging speed, cycle stability and energy storage capacity; its ability to promote the rapid transmission of electrons and lithium ions significantly enhances the battery's power density and cycle life. The versatility and wide application prospects of graphene show its importance as an anode and potential cathode material in the field of supercapacitor technology, depending on specific battery technology and design requirements. Therefore, it is necessary to design a fiber electrode material with a directional morphology based on graphene fibers to solve the above technical problems. Summary of the invention
[0005] [Technical issues]
[0006] The mechanical and electrochemical properties of general structural energy storage composite materials are poor;
[0007] Conventional composite materials cannot take into account both electrochemical and mechanical properties.
[0008] [Technical solution]
[0009] In order to solve the above problems, the present invention first disperses Fe3O4 nanoparticles in a GO (graphene oxide) suspension, and adjusts the distribution of Fe3O4 nanoparticles on the surface of GO nanosheets by adding ethylenediamine (EDA) to form a Fe3O4-modified graphene oxide (Fe3O4@GO) liquid crystal solution; then, the Fe3O4-modified graphene oxide (Fe3O4@GO) liquid crystal solution is extruded into a coagulation bath through a spinneret of a spinning device, and at the same time, a magnet is used to rotate above the spinneret to drive Fe3O4@GO to rotate and unfold in the solution for bidirectional directional arrangement, forming Fe3O4@GO gel fiber filaments; finally, drying, stretching, and winding to obtain a fiber electrode. The fiber electrode prepared by the present invention can take into account both electrochemical properties and mechanical properties, and can be used to prepare batteries, supercapacitors, etc.
[0010] The first object of the present invention is to provide a method for preparing a fiber electrode by directional arrangement of Fe3O4@GO induced by a magnet, comprising the following steps:
[0011] (1) Fe3O4 nanoparticles are dispersed in GO (graphene oxide) suspension, and the distribution of Fe3O4 nanoparticles on the surface of GO nanosheets is regulated by adding ethylenediamine (EDA), and the mixture is mixed evenly to form Fe3O4-modified graphene oxide (Fe3O4@GO) liquid crystal solution;
[0012] (2) extruding a Fe3O4-modified graphene oxide (Fe3O4@GO) liquid crystal solution into a coagulation bath through a spinneret of a spinning device, and before spinning, using a magnet to rotate above the spinneret to drive the Fe3O4@GO to rotate and expand in the solution for bidirectional orientation to form Fe3O4@GO gel fiber filaments; wherein the rotation speed of the magnet is 0.5-10 rpm;
[0013] (3) drying, stretching, and winding the Fe3O4@GO gel fiber to obtain fibers;
[0014] (4) The fibers are reduced and calcined to obtain fiber electrodes.
[0015] In one embodiment of the present invention, in step (1), GO (graphene oxide) is prepared by using a modified Hummers method.
[0016] In one embodiment of the present invention, the Fe3O4 nanoparticles in step (1) are prepared by a hydrothermal method.
[0017] In one embodiment of the present invention, the particle size of GO (graphene oxide) in step (1) is 0.5 to 50 μm.
[0018] In one embodiment of the present invention, the average particle size of the Fe3O4 nanoparticles in step (1) is 220 nm.
[0019] In one embodiment of the present invention, the concentration of the GO (graphene oxide) suspension in step (1) is 10-20 mg / mL, and the solvent is water.
[0020] In one embodiment of the present invention, the concentration of Fe3O4 nanoparticles in the GO (graphene oxide) suspension in step (1) is 1-30wt%, further optimized to 5-20wt%.
[0021] In one embodiment of the present invention, the volume ratio of GO (graphene oxide) suspension and ethylenediamine (EDA) in step (1) is 10 mL: 40-100 μL.
[0022] In one embodiment of the present invention, the uniform mixing in step (1) is achieved by vigorous stirring, specifically stirring at 800 rpm for 100-150 min.
[0023] In one embodiment of the present invention, the Fe3O4-modified graphene oxide (Fe3O4@GO) liquid crystal solution in step (2) needs to be degassed before spinning, and the degassing is performed by centrifugation at 200-4000 rpm for 5-15 minutes.
[0024] In one embodiment of the present invention, the coagulation bath in step (2) is a mixture of ethanol, water and CaCl2 or pure ethyl acetate; wherein the volume ratio of ethanol to water in the mixture is 3:1, and the concentration of CaCl2 is 5wt%.
[0025] In one embodiment of the present invention, the magnet in step (2) is a ring-shaped perforated neodymium magnet with an outer diameter of 20 mm, an inner diameter of 18 mm, and a ring thickness of 2 mm.
[0026] In one embodiment of the present invention, the spinneret in step (2) is a 22G hole spinneret with a needle inner diameter of 0.4 mm and an outer diameter of 0.7 mm.
[0027] In one embodiment of the present invention, the magnet in step (2) improves the sheet order of the fiber cross section through the rotational shear flow, thereby significantly promoting the lateral fiber arrangement.
[0028] In one embodiment of the present invention, in step (2), the Fe3O4@GO fluid is transformed into gel fibers by double diffusion between water (water in GO (graphene oxide) suspension) and a coagulation bath.
[0029] In one embodiment of the present invention, the drying in step (3) is carried out at 60-80° C. for 24 hours.
[0030] In one embodiment of the present invention, the stretching ratio in step (3) is 1.5-2.5 times.
[0031] In one embodiment of the present invention, the diameter of the fiber in step (3) is 40-70 microns.
[0032] In one embodiment of the present invention, the reduction in step (4) is to place the fiber in a straight state and reduce it in a 47 wt % hydroiodic acid (HI) aqueous solution at 90° C. for 360-480 min.
[0033] In one embodiment of the present invention, the calcination in step (4) is to heat the reduced fiber from room temperature to 450°C at a rate of 5°C / min, and then maintain it at 800°C and 1200°C for 1 hour at a rate of 10°C / min in an argon flow.
[0034] In one embodiment of the present invention, the diameter of the fiber electrode in step (4) is 40-70 microns.
[0035] The second object of the present invention is the fiber electrode prepared by the method of the present invention.
[0036] The third object of the present invention is to provide an electrode material, which is obtained by weaving the fiber electrode described in the present invention.
[0037] The fourth object of the present invention is the application of the fiber electrode or electrode material described in the present invention in the electrical field.
[0038] A fifth object of the present invention is to provide a lithium electronic battery, which uses the fiber electrode or electrode material described in the present invention.
[0039] A sixth object of the present invention is to provide a supercapacitor, which uses the fiber electrode or electrode material described in the present invention.
[0040] The seventh object of the present invention is to provide a method for simultaneously improving the electrochemical properties and mechanical properties of electrode materials, which uses the fiber electrode or electrode material described in the present invention.
[0041] The eighth object of the present invention is to provide a structural energy storage composite material, which uses the fiber electrode or electrode material described in the present invention.
[0042] [Beneficial Effects]
[0043] (1) The tensile strength of the fiber electrode prepared by the present invention can reach above 225 MPa and can be as high as 928.8 MPa.
[0044] (2) The volumetric specific capacitance of the fiber supercapacitor electrode prepared by the present invention is 2 mV s -1 Up to 1237.0Fcm -3 The assembled fiber supercapacitor has a power of 30.1 mW cm -3 40.0 mWh cm -3 The energy density of the device was 2.37 W, and it exhibited almost 100% capacitance retention under mechanical bending at different angles.
[0045] (3) The volumetric capacity of the flexible fiber-shaped lithium-ion battery prepared by the present invention is 2 mV s -1 Up to 162mAhcm -3 The assembled fiber supercapacitor has a power of 625.3 mW cm -3 32mWh cm -3 The energy density of the battery is 2.5W, and it exhibits almost 100% capacity retention under mechanical bending at different angles.
[0046] (4) By modifying the graphene fiber to make it magnetic, it has the concept of bidirectionally promoting the assembly order during the spinning process, so that the graphene fiber can achieve synergistically improved mechanical and electrochemical properties. The concentric arrangement of graphene oxide sheets on the cross section and along the fiber axis are achieved through multiple shear flow fields. This bidirectional promotion promotes the directional arrangement of graphene sheets in the prepared macroscopic graphene fiber, resulting in a dense and crystalline graphite structure and improving its performance. The development of new functional fibers with good energy storage performance, high conductivity and strong mechanical properties, as well as the assembly of supercapacitors, provides feasibility for solving these problems. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 : TEM image of graphene oxide (GO).
[0048] Figure 2 :Actual picture of the fiber bundle after preliminary spinning.
[0049] Figure 3 : SEM of fibers with bidirectional orientation, where (a) is 500 μm and (b) is 3 μm.
[0050] Figure 4 : Stress-strain curves of fiber electrodes prepared with different contents of Fe3O4.
[0051] Figure 5: Tensile strength results of fiber electrodes prepared at different rotation speeds.
[0052] Figure 6 :(a) Fiber supercapacitor at 2mV s -1 CV curves of (a) fiber supercapacitor at 2 mV s -1 CV curves of fiber-shaped lithium-ion battery at different bending angles (c) at 2 mV s -1 CV curves of lithium-ion batteries at 2 mV s -1 The CV curves at different bending angles are shown below.
[0053] Figure 7 : Cyclic charge-discharge performance of flexible fiber supercapacitors prepared using fiber electrodes. DETAILED DESCRIPTION
[0054] The preferred embodiments of the present invention are described below. It should be understood that the embodiments are for better explaining the present invention and are not used to limit the present invention.
[0055] Test method:
[0056] 1. Test of diameter and cross-sectional area:
[0057] The diameter and cross-sectional area of the prepared fiber were measured according to the GB / T 29762-2013 standard for the determination of carbon fiber fiber diameter and cross-sectional area.
[0058] 2. Stress-strain curve test:
[0059] The tensile properties test was carried out according to the GB / T 31290-2022 carbon fiber monofilament tensile properties determination standard, and the stress-strain curve was plotted according to the load-displacement curve.
[0060] The raw materials used in the examples are:
[0061] GO (graphene oxide) is prepared by a modified Hummers method as follows:
[0062] Add 400mL of sulfuric acid and phosphoric acid with a volume ratio of 9:1 to the beaker, stir and mix them evenly at 100rpm; slowly add 21g of expandable graphite and potassium permanganate with a mass ratio of 1:6 in batches, and the reaction system will release a small amount of heat; move the beaker into a constant temperature water bath at 50℃, and react for 12h at 200rpm and 50℃; after the reaction is completed, wait for the reaction liquid to cool to room temperature, slowly add 200mL of ice cubes and 20mL of 30% hydrogen peroxide solution to prevent its temperature from rising until no bubbles are generated, then use ice cubes to cool it outside, and ultrasonicate for 1h; then centrifuge it at 1000rpm for 6min, take the upper clear night, and then centrifuge it at 8000rpm for 6min to take the precipitate. Finally, wash it three times with 30% HCl solution, anhydrous ethanol, and deionized water, respectively, to obtain graphene oxide (GO).
[0063] Ferroferric oxide (Fe3O4) nanoparticles were prepared by hydrothermal method as follows:
[0064] Under continuous stirring (500rpm), 0.07M FeCl3·4H2O and 0.14M FeCl·6H2O were dissolved in deionized water to form a homogeneous solution; an appropriate amount of ammonia solution (30%) was added dropwise to 80mL of the homogeneous solution, and the pH value of the solution was measured using a pH meter to be 9, and the solution was kept at 80℃ for 1h under constant stirring (500rpm); after the reaction was completed, a black precipitate was formed. The obtained precipitate was washed 3 times with distilled water and calcined at 300℃ for 3 hours; the prepared sample was collected as Fe3O4 nanoparticles.
[0065] Graphene oxide (GO): specifications are 0.5 to 50 μm;
[0066] Fe3O4 nanoparticles: The specification is an average particle size of 220nm.
[0067] Example 1
[0068] A method for preparing a fiber electrode by using a magnet to induce the directional arrangement of Fe3O4@GO comprises the following steps:
[0069] (1) Dispersing Fe3O4 nanoparticles in 10 mL of 10 mg / mL GO (graphene oxide) suspension, using 50 μL of ethylenediamine (EDA) in an ultrasonic cleaner to adjust the distribution of Fe3O4 nanoparticles on the surface of GO nanosheets, and reacting at 40 W for 30 min; after the reaction is completed, stirring the solution vigorously at 1000 rpm for 120 min to make it completely uniform, forming a Fe3O4-modified graphene oxide (Fe3O4@GO) liquid crystal solution; wherein the concentration of Fe3O4 nanoparticles in the GO (graphene oxide) suspension is 20 wt%;
[0070] (2) The Fe3O4-modified graphene oxide (Fe3O4@GO) liquid crystal solution was degassed by centrifugation at 1500 rpm for 10 minutes, and then placed in a spinning device, and extruded into a coagulation bath (pure ethyl acetate) through a spinneret (22G hole spinneret, needle inner diameter 0.4 mm, outer diameter 0.7 mm) of the spinning device at an extrusion speed of 0.2 mL / min. Before spinning, a magnet (specification: annular neodymium magnet with holes, outer diameter 20 mm, inner diameter 18 mm, ring thickness 2 mm) was used to rotate above the spinneret (speed of 8 rpm) to drive the Fe3O4@GO to rotate and expand in the solution for bidirectional directional arrangement. The Fe3O4@GO fluid was double diffused between water and the coagulation bath to become gel fiber filaments, and the fiber filaments were pulled out of the coagulation bath to form Fe3O4@GO gel fiber filaments (diameter 200-300 μm);
[0071] (3) The Fe3O4@GO gel fiber was dried at 60 °C for 24 h and directed onto a polytetrafluoroethylene roller (with the same size and rotation speed), and the fiber was stretched (stretching ratio of 1.2 times) by adjusting the latter roller to a higher speed; subsequently, the fiber was further stretched (stretching ratio of 1.5 times) and finally collected on a drum for winding to obtain the fiber;
[0072] (4) The fiber was straightened and reduced in a 47 wt% hydroiodic acid (HI) aqueous solution at 90°C for 360 min. After the reduction was completed, the fiber was taken out and heated from room temperature to 450°C at a rate of 5°C / min, and then maintained at 800°C and 1200°C for 1 h in an argon gas flow at a rate of 10°C / min. A fiber electrode (with a diameter of 40-70 μm) was obtained.
[0073] Example 2
[0074] The concentration of Fe3O4 nanoparticles in the GO (graphene oxide) suspension in step (1) of Example 1 was adjusted to 0, 5, 10, 15, 20, 25, and 30 wt%; at the same time, the rotation speed of the magnet in step (2) was adjusted to 5 rpm; the rest was kept consistent with Example 1 to obtain a fiber electrode.
[0075] The obtained fiber electrode performance was tested, and the test results are as follows:
[0076] Figure 4 The stress-strain curves of fiber electrodes prepared with different contents of Fe3O4. Figure 4It can be seen that the tensile strength of pure graphene fiber is 106.8MPa. After adding different amounts of magnetic materials and promoting bidirectional arrangement, its tensile strength is increased several times. Among them, the tensile strength of Fe3O4@GO mixed fibers with 5, 10, 15, 20, and 25wt% contents are 328.4, 747.9, 855.7, 928.8, and 722.7MPa, respectively. After adding 25wt% of Fe3O4, there are too many magnetic materials, which makes the mixture uneven, causing the orientation of the fiber to decrease, resulting in a decrease in tensile strength. Therefore, after adding 20wt% of Fe3O4, the mixed fiber can achieve the maximum mechanical properties.
[0077] Example 3
[0078] The rotation speed of the magnet in step (2) of Example 1 is adjusted to 0.5, 1, 2, 5, 8, 10, and 15 rpm; at the same time, the concentration of Fe3O4 nanoparticles in the GO (graphene oxide) suspension in step (1) is 20 wt %, and the rest is consistent with Example 1 to obtain a fiber electrode.
[0079] The obtained fiber electrode performance was tested, and the test results are as follows:
[0080] Figure 5 The tensile strength results of the fiber electrodes prepared at different rotation speeds. Figure 5 It can be seen that: the higher or lower rotation speed of the magnet ring leads to the formation of disordered or random arrangement of Fe3O4@GO sheets, resulting in poor orientation order and smaller crystallite size. The tensile strength of the composite graphene fiber is 225.3, 291.2, 559.6, 929.8, 1104.4, 886.3, 562.3Mpa when the rotation speed is 0.5, 1, 2, 5, 8, 10, 15rpm / s, respectively. It can be seen that the appropriate rotation speed can increase the orderly arrangement of graphene sheets. When the magnet ring rotates too fast, the force on the sheets may be uneven, causing large sheets of graphene to break into small sheets, resulting in a decrease in mechanical properties.
[0081] Example 4
[0082] A flexible fiber supercapacitor is prepared using the fiber electrode of Example 3 (the rotation speed of the magnet is 5 rpm, and the concentration of Fe3O4 nanoparticles in GO (graphene oxide) suspension is 20 wt%);
[0083] The preparation method is as follows:
[0084] 1 g of polyvinyl alcohol (PVA) powder was added to 10 mL of deionized water and then vigorously stirred at 90 °C for 30 min until a clear solution was obtained to obtain a mixture;
[0085] When the temperature of the mixture drops to ambient temperature, 1 g of H3PO4 is added to the mixture and mixed well to obtain a PVA / H3PO4 gel electrolyte;
[0086] A flexible fiber supercapacitor was assembled using two fiber electrodes of Example 3 and PVA / H3PO4 gel electrolyte.
[0087] The fiber electrode was immersed in PVA / H3PO4 gel electrolyte for 1 hour, taken out, and dried in air for 8 hours;
[0088] Two fiber electrodes coated with electrolyte are placed in parallel on a flexible PET substrate, and the electrolyte is re-coated until the fiber surface is completely wrapped with the electrolyte, and then a flexible fiber supercapacitor is made.
[0089] The obtained flexible fiber supercapacitor was tested by measuring the electrochemical properties using an electrochemical workstation (CHI 660D), including cyclic voltammetry (CV) and other tests;
[0090] The test results are as follows:
[0091] from Figure 6 It can be seen from (a) and (b) that the volumetric capacitance of the fiber supercapacitor electrode is 2mV s -1 Up to 1237.0F cm -3 The assembled fiber supercapacitor has a power of 30.1 mW cm -3 40.0 mWh cm -3 The energy density of the device was 2.37 W, and it exhibited almost 100% capacitance retention under mechanical bending at different angles.
[0092] Figure 7 The cyclic charge-discharge performance of flexible fiber supercapacitors prepared using fiber electrodes. Figure 7 It can be seen that the fiber electrode exhibits excellent electrochemical performance as well as excellent flexibility and stability.
[0093] It can be seen that the flexible fiber supercapacitor prepared by using the fiber electrode of the present invention can have excellent electrochemical performance and cycle performance. The fiber supercapacitor not only has the characteristics of large capacitance, high power density, and long cycle life, but also has the advantages of small size, light weight, good flexibility, and strong deformation ability. Therefore, the fiber supercapacitor can meet the high flexibility, weavability, and wearability requirements of flexible devices such as wearable smart devices, making it an ideal choice for the energy storage system of wearable smart devices.
[0094] Example 5
[0095] A flexible fiber lithium-ion battery is prepared using the fiber electrode of Example 3 (the rotation speed of the magnet is 5 rpm, and the concentration of Fe3O4 nanoparticles in the GO (graphene oxide) suspension is 20 wt%):
[0096] The details are as follows:
[0097] First, polyvinylidene fluoride-co-hexafluoropropylene (PVDF-HFP) was added to N-methylpyrrolidone (NMP) solution to prepare a mixed solution with a mass fraction of 15 wt%, and magnetic stirring was carried out overnight to obtain a PVDF-HFP / NMP solution;
[0098] Then, lithium iron phosphate, carbon black and PVDF-HFP were dispersed into the PVDF-HFP / NMP solution in a mass ratio of 7:2:1, and stirred for 1 hour using a high-speed disperser to obtain a uniformly dispersed mixed liquid; wherein the concentration of lithium iron phosphate in the PVDF-HFP / NMP solution was 70wt%;
[0099] The mixed liquid was extruded at a high speed of 8 mm / s and immersed in an ethanol coagulation bath;
[0100] After thorough solvent exchange, the fiber electrode was placed in an open container and dried naturally at room temperature to obtain a lithium iron phosphate fiber electrode.
[0101] The preparation of fiber-shaped lithium-ion batteries is as follows:
[0102] The lithium iron phosphate fiber and graphene fiber electrodes were immersed in PVDF-HFP acetone solution (0.5wt%) for three times, a layer of PVDF-HFP separation membrane was evenly coated on the surface, and then they were twisted to serve as cathode and anode respectively;
[0103] The potential window of the fiber-type full cell is 1-2.5V;
[0104] A current collector (aluminum foil for cathode electrode and copper foil for anode electrode) was attached to the end of each fiber electrode, and then the injection and packaging process of ethylene carbonate (EC) liquid electrolyte containing 1M lithium hexafluorophosphate (LiPF6) was completed in a glove box.
[0105] The test results are as follows:
[0106] from Figure 6 It can be seen from (c) and (d) that the results show that the volumetric capacity of the fiber supercapacitor electrode is 2mVs -1 Up to 162mAh cm -3 The assembled fiber supercapacitor has a power of 625.3 mW cm -3 32mWh cm -3The energy density of the prepared fiber electrode is 100%, and the capacity retention rate is almost 100% under mechanical bending at different angles. The prepared fiber electrode exhibits excellent electrochemical performance as well as excellent flexibility and stability.
[0107] It can be seen that the flexible fiber-shaped lithium-ion battery prepared by using the fiber electrode of the present invention can have excellent electrochemical performance and cycle performance. The fiber-shaped lithium-ion battery not only has the characteristics of large capacity, high power density, and long cycle life, but also has the advantages of small size, light weight, good flexibility, and strong deformation ability. Therefore, the fiber-shaped lithium-ion battery can also meet the high flexibility, weavability, and wearability requirements of flexible devices such as wearable smart devices, making it an ideal choice for the energy storage system of wearable smart devices.
[0108] Comparative Example 1
[0109] The magnet in step (2) of Example 1 is omitted, and the rest is kept the same as Example 1 to obtain a fiber electrode.
[0110] The results show that the mechanical properties of the prepared fiber electrode are reduced by about 85% compared with those of Example 1. At the same time, the electrical conductivity is also reduced by 32%.
[0111] Comparative Example 2
[0112] The fiber electrode of comparative example 1 was used to prepare a fiber supercapacitor according to example 4.
[0113] The results show that compared with the fiber supercapacitor prepared in Example 4, its electrochemical performance decreased by about 42%. At the same time, when the electrochemical performance was tested at different angles, the fiber supercapacitor short-circuited when bent to 120°. It can be determined that rotating the graphene mixed solution at different rates in the magnetic field during the spinning process can not only increase the mechanical properties of the prepared fiber electrode material, but also improve its electrochemical performance.
[0114] Comparative Example 3
[0115] The fiber electrode of Comparative Example 1 was used to prepare a fiber-shaped lithium-ion battery according to Example 5.
[0116] The results show that compared with the fiber-shaped lithium-ion battery prepared in Example 5, its specific capacity is 64 mAh cm -3 , compared with the fiber-shaped lithium-ion battery prepared in Example 5, its specific capacity is reduced by nearly 60%. Although no short circuit occurs in the bending state, its specific capacity gradually decreases with the increase of the bending angle. Similarly, through this comparative example, it can be determined that by rotating the graphene mixed solution at different rates in the magnetic field during the spinning process, not only the mechanical properties of the prepared fiber electrode material can be increased, but also its electrochemical properties can be improved.
[0117] Comparative Example 4
[0118] The magnet in Example 1 was replaced with a thin rod for stirring in the capillary to prepare Fe3O4@GO fibers;
[0119] The details are as follows:
[0120] First, the graphene solution was injected into a capillary with a diameter of 300 mm, and a thin stainless steel strip with a diameter of 100 mm was inserted into the middle of the capillary for uniform rotation at a rotation speed of 8 rpm / s. After continuous rotation for 60 min, the stainless steel strip was taken out. At this time, the graphene solution in the capillary had a certain horizontal arrangement after the rotation of the stainless steel, and then one end of the capillary was inserted into the spinning device used in Example 1, and the graphene solution in the capillary was extruded at the same speed. The other conditions were the same as in Example 1 to obtain Fe3O4@GO fibers.
[0121] The tensile strength of the fiber was tested for its mechanical properties and the results showed that its tensile strength was only 428 MPa, which was about 77% lower than the 1104.4 MPa of Fe3O4@GO fiber prepared by magnet rotation under the same conditions.
[0122] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A method for preparing fiber electrodes by using a magnet to induce Fe3O4@GO to arrange in a directional manner, characterized in that: The steps include: (1) Fe3O4 nanoparticles are dispersed in GO (graphene oxide) suspension, and the distribution of Fe3O4 nanoparticles on the surface of GO nanosheets is regulated by adding ethylenediamine (EDA), and the mixture is mixed evenly to form Fe3O4-modified graphene oxide (Fe3O4@GO) liquid crystal solution; (2) extruding a Fe3O4-modified graphene oxide (Fe3O4@GO) liquid crystal solution into a coagulation bath through a spinneret of a spinning device, and before spinning, using a magnet to rotate above the spinneret to drive the Fe3O4@GO to rotate and expand in the solution for bidirectional orientation to form Fe3O4@GO gel fiber filaments; wherein the rotation speed of the magnet is 0.5-10 rpm; (3) drying, stretching, and winding the Fe3O4@GO gel fiber to obtain fibers; (4) The fibers are reduced and calcined to obtain fiber electrodes.
2. The method according to claim 1, characterized in that: In step (1), the concentration of Fe3O4 nanoparticles in the GO (graphene oxide) suspension is 1-30wt%.
3. The method according to claim 1, characterized in that In step (2), the coagulation bath is a mixture of ethanol, water and CaCl2 or pure ethyl acetate; wherein the volume ratio of ethanol to water in the mixture is 3:1, and the concentration of CaCl2 is 5wt%.
4. The fiber electrode prepared by the method according to any one of claims 1 to 3.
5. An electrode material, characterized in that: The fiber electrode according to claim 4 is woven into the fiber electrode.
6. Use of the fiber electrode according to claim 4 or the electrode material according to claim 5 in the field of electricity.
7. A lithium-ion battery, characterized in that: The fiber electrode according to claim 4 or the electrode material according to claim 5 is used.
8. A supercapacitor, characterized in that: The fiber electrode according to claim 4 or the electrode material according to claim 5 is used.
9. A method for simultaneously improving the electrochemical properties and mechanical properties of an electrode material, characterized in that: The fiber electrode according to claim 4 or the electrode material according to claim 5 is used.
10. A structural energy storage composite material, characterized in that: The fiber electrode according to claim 4 or the electrode material according to claim 5 is used.
Citation Information
Patent Citations
Method for preparing graphene / polymer orderly micro-nanometer composite fiber through magnetic spinning
CN104862799A
Graphene enhanced conductive rubber film and preparation method thereof
CN109306083A
Electrospinning device, oriented Fe3O4 / Gr / PAN composite conductive nanofiber and preparation method thereof
CN109468701A
Graphene oxide magnetic directional dispersion reinforced cement-based composite material and preparation method thereof
CN114573284A
Magnetic orientation graphene / carbon composite material and preparation method thereof
CN118993050A
Cited By
Two-dimensional nano material electrode, preparation method and application
CN120581537A