Pattern forming method

By using metal-containing resist compositions and developer compositions in photoresist, the film thickness is increased after development and contains phosphorus and sulfur elements, the sensitivity of photoresist is reduced and the line edge roughness is solved under extreme ultraviolet exposure. The problem of increased degree achieves better etch resistance and critical dimensional uniformity.

CN119024654APending Publication Date: 2024-11-26SAMSUNG SDI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410424324.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-03-19
Filing Date
2024-04-10
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The sensitivity of existing chemical amplified photoresist is reduced under extreme ultraviolet exposure, the roughness of the line edge increases, and it is difficult to simultaneously improve etch resistance and critical dimension uniformity.

Method used

Using a metal-containing resist composition, a resist pattern is formed by coating the developer composition, the film thickness is increased after development, and phosphorus and sulfur elements are contained on the surface to reduce the interval of the resist pattern to improve the roughness of the line edge.

Benefits of technology

After development, the thickness of the resist film increases, reduces the bridging phenomenon, improves line edge roughness and resolution, and improves the pattern's etch resistance and critical dimension uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119024654A_ABST
    Figure CN119024654A_ABST
Patent Text Reader

Abstract

A method of forming a pattern is provided, the method comprising applying a metal-containing resist composition on a substrate; drying and heating to form a metal-containing resist film on the substrate; exposing the metal-containing resist film using the patterned mask; and applying a developer composition to remove the unexposed region, thereby forming a resist pattern. The thickness of the post-development resist film is increased by about 5% to about 100% compared to the thickness of the pre-development resist film, and the surface of the post-development resist film may include about 5 at% to about 20 at%, based on the total number of atoms, of at least one selected from the group consisting of a phosphorus element and a sulfur element.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority and the benefits of Korean Patent Application No. 10-2023-0066535 filed in the Korean Intellectual Property Office on May 23, 2023, and this application claims priority and the benefits of Korean Patent Application No. 10-2024-0037581 filed in the Korean Intellectual Property Office on March 19, 2024, and all disclosures of the Korean patent applications are incorporated herein by reference. Technical Field

[0003] Embodiments of the present disclosure relate to a method of forming a pattern including developing. Background Art

[0004] In recent years, the semiconductor industry has been experiencing a substantial reduction in critical dimension (CD), and this reduction in dimension will benefit from new (or new types of) high performance photoresist materials and patterning methods that meet the expectations for processing and patterning smaller and smaller features.

[0005] Chemically amplified (CA) photoresists are designed to ensure high sensitivity, but due to their elemental composition (mainly less O, F and S, C) will reduce the absorbance at about 13.5nm wavelength and thus reduce sensitivity, so the photoresist may suffer more difficulties under extreme ultraviolet (EUV) light exposure. CA photoresists may have difficulties due to roughness problems at small feature sizes and partly due to the nature of acid catalyst processes. Experiments have shown that line edge roughness (LER) increases with decreasing photospeed. Due to these shortcomings and problems of CA photoresists, new (or new types) of high-performance photoresists are needed in the semiconductor industry.

[0006] It would be beneficial to develop a photoresist that ensures excellent etching resistance and resolution in a photolithography process while also (eg, simultaneously) improving sensitivity and enhancing critical dimension (CD) uniformity and line edge roughness (LER) characteristics. Summary of the invention

[0007] Some exemplary embodiments of the present disclosure provide a method of forming a pattern including developing, the method including applying a developer composition to form a resist pattern.

[0008] According to some exemplary embodiments, the method of forming a pattern includes: coating a metal-containing resist composition on a substrate; performing a heat treatment including drying and heating to form a metal-containing resist film on the substrate; exposing the metal-containing resist film using a patterned mask; and coating a developer composition to remove unexposed areas to form a resist pattern, wherein the thickness of the metal-containing resist film after development is increased by about 5% to about 100% compared to the thickness of the metal-containing resist film before development, and the surface of the metal-containing resist film after development may include about 5at% to about 20at% of at least one selected from phosphorus and sulfur based on the total number of atoms.

[0009] The developer composition may include an additive and an organic solvent, wherein the additive includes at least one selected from a phosphoric acid compound, a phosphorous acid compound, a hypophosphorous acid compound, and a sulfonic acid compound.

[0010] The additive may be included in an amount of about 0.01 wt % to about 10 wt %.

[0011] The phosphorous acid compound can be at least one of the following: phosphonic acid, methylphosphonic acid, ethylphosphonic acid, butylphosphonic acid, hexylphosphonic acid, n-octylphosphonic acid, tetradecylphosphonic acid, octadecylphosphonic acid, phenylphosphonic acid, vinylphosphonic acid, aminomethylphosphonic acid, methylenediaminetetramethylenephosphonic acid, ethylenediaminetetramethylenephosphonic acid, 1-amino-1-phosphonooctylphosphonic acid, hydroxyethylphosphonic acid, 2-aminoethylphosphonic acid, 3-aminopropylphosphonic acid, 4-methylphenylphosphonic acid, 3-methylphenylphosphonic acid, 2-methyl 1H,1H,2H,2H-perfluorooctanephosphonic acid, cyclohexylmethylphosphonic acid, 2-thienylmethylphosphonic acid, 4-fluorophenylphosphonic acid, benzylphosphonic acid, or a combination thereof.

[0012] The phosphorous acid compound may be at least one of the following: diphenylphosphinic acid, bis(4-methoxyphenyl)phosphinic acid, phosphinic acid, bis(hydroxymethyl)phosphinic acid, phenylphosphinic acid, p-(3-aminopropyl)-p-butylphosphinic acid, or a combination thereof.

[0013] The sulfonic acid compound may be at least one of the following: p-toluenesulfonic acid, benzenesulfonic acid, p-dodecylbenzenesulfonic acid, 1,4-naphthalene disulfonic acid, methanesulfonic acid, phenylmethanesulfonic acid, 1-octanesulfonic acid, 4-vinylbenzenesulfonic acid, 2-methylbenzenesulfonic acid, ethanesulfonic acid, 2,5-dimethylbenzenesulfonic acid, 2,4-dimethylbenzenesulfonic acid, allylsulfonic acid, 1-butanesulfonic acid, 1-propanesulfonic acid, 2-propanesulfonic acid, vinylbenzenesulfonic acid, hexanesulfonic acid, heptanesulfonic acid or a combination thereof.

[0014] The metal compound included in the metal-containing resist composition may include at least one selected from the group consisting of an organic oxygen group-containing tin compound and an organic carbonyl oxygen group-containing tin compound.

[0015] The metal compound can be represented by Chemical Formula 1.

[0016] [Chemical formula 1]

[0017]

[0018] In Chemical Formula 1,

[0019] R 1 is selected from substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, substituted or unsubstituted C7 to C30 arylalkyl, and L a -OR a (Where L a is a substituted or unsubstituted C1 to C20 alkylene group, and R a is a substituted or unsubstituted C1 to C20 alkyl),

[0020] R 2 To R 4 each independently represents a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, a substituted or unsubstituted C7 to C30 aralkyl group, -OR b or -OC(=O)R c ,

[0021] R 2 to R 4 At least one of them is independently selected from -OR b or -OC(=O)R c ,

[0022] R bis a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof, and

[0023] R c is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof.

[0024] The method of forming a pattern according to some example embodiments may realize a fine pattern in which the width (thickness) of the resist pattern is relatively increased by reducing the interval between the resist patterns while reducing a bridge and improving LER characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The drawings, together with the specification, illustrate embodiments of the presently disclosed subject matter, and, together with the description, serve to explain principles of the embodiments of the presently disclosed subject matter.

[0026] Figures 1 to 3 2 is a cross-sectional view showing a process sequence to explain a method of forming a pattern according to an embodiment of the present disclosure.

[0027] Figure 4 is a set of scanning electron micrograph images comparing the thickness of the resist film after development.

[0028] Figure 5 It is a graph showing the results of X-ray photoelectron spectroscopy (XPS) analysis of the resist film after development.

[0029] Figure 6 is a set of scanning electron micrograph images showing the resist pattern after development.

[0030] [Explanation of Symbols]

[0031] 100: substrate;

[0032] 110: feature layer;

[0033] 110P: characteristic pattern;

[0034] 130P: photoresist pattern;

[0035] OP: Open your mouth. DETAILED DESCRIPTION

[0036] Hereinafter, embodiments of the present disclosure are described in more detail with reference to the accompanying drawings. In the following description of the subject matter of the present disclosure, well-known functions or configurations may not be described for the purpose of clarifying the description of the embodiments of the present disclosure.

[0037] In order to clearly illustrate the embodiments of the present disclosure, some descriptions and relationships may be omitted, and throughout the present disclosure, the same or similar configuration elements are represented by the same reference numerals. In addition, since the size and thickness of each configuration shown in the drawings can be arbitrarily shown for better understanding and ease of description, the present disclosure is not necessarily limited thereto.

[0038] In the drawings, the thickness of a layer, film, panel, region, etc. may be exaggerated for clarity. In the drawings, the thickness of a portion of a layer or region may be exaggerated for clarity. It should be understood that if an element (such as a layer, film, region, or substrate) is referred to as being "on" another element, the element may be directly on the other element or intervening elements may also be present.

[0039] In the present disclosure, "substituted" means that a hydrogen atom is replaced by a deuterium, a halogen group, a hydroxyl group, an amino group, a substituted or unsubstituted C1 to C30 amine group, a nitro group, a substituted or unsubstituted C1 to C40 silyl group, a C1 to C30 alkyl group, a C1 to C10 haloalkyl group, a C1 to C10 alkylsilyl group, a C3 to C30 cycloalkyl group, a C6 to C30 aryl group, a C1 to C20 alkoxy group, or a cyano group. "Unsubstituted" means that a hydrogen atom remains a hydrogen atom without being replaced by another substituent.

[0040] In the present disclosure, unless otherwise defined, the term "alkyl" refers to a straight or branched aliphatic hydrocarbon group. The alkyl group may be a "saturated alkyl group" not containing any double or triple bonds.

[0041] The alkyl group may be a C1 to C20 alkyl group. For example, the alkyl group may be a C1 to C10 alkyl group or a C1 to C6 alkyl group. For example, a C1 to C4 alkyl group means that the alkyl chain contains 1 to 4 carbon atoms and may be selected from methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl and tert-butyl.

[0042] Examples of alkyl groups include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, hexyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, and the like.

[0043] In the present disclosure, if no definition is otherwise provided, the term "cycloalkyl group" refers to a monovalent cyclic aliphatic hydrocarbon group.

[0044] In the present disclosure, if a definition is not otherwise provided, the term "alkenyl group" is a straight or branched aliphatic hydrocarbon group, and refers to an aliphatic unsaturated alkenyl group containing one or more double bonds.

[0045] In the present disclosure, if a definition is not otherwise provided, the term "alkynyl group" is a straight or branched aliphatic hydrocarbon group, and refers to an unsaturated alkynyl group containing one or more triple bonds.

[0046] In the present disclosure, "aryl" refers to a substituent in which all elements of the cyclic substituent have p-orbitals, and these p-orbitals form conjugation, and may include monocyclic, polycyclic or fused ring (e.g., rings that share adjacent pairs of carbon atoms) functional groups.

[0047] Hereinafter, methods of forming patterns according to some example embodiments will be described in more detail with reference to the accompanying drawings.

[0048] According to some exemplary embodiments, the method of forming a pattern includes: coating a metal-containing resist composition on a substrate; performing drying and heating to form a metal-containing resist film on the substrate; exposing the metal-containing resist film using a patterned mask; and coating a developer composition to remove unexposed areas, thereby forming a resist pattern.

[0049] wherein the thickness of the resist film after development increases by about 5% to about 100% compared to the thickness of the resist film before development, and

[0050] The surface of the developed resist film may include about 5 at % to about 20 at % of at least one selected from phosphorus and sulfur, based on the total number of atoms.

[0051] In order to reduce the space gap of the resist, the gap between the mask patterns may be narrowed, but there is a problem of generating bridges between lines due to diffraction of light during exposure, and thus causing an increase in LER.

[0052] If a developer having high solubility is used, the pitch interval may become widened even at the same energy, but conversely, if a developer having low solubility is used, bridges may also be generated between lines because undissolved components remain in some of the pitches.

[0053] However, the resist pattern formed according to the embodiment of the method for forming a pattern disclosed herein can achieve the effect of reducing the spacing interval without (or substantially without) bridging, and thus improve the LER characteristics, because the resist film contains about 5at% to about 20at% of at least one selected from phosphorus and sulfur on the surface after development, and thus the thickness after development is increased by about 5% to about 100% relative to before development.

[0054] The P component and the S component among the developer components are adsorbed onto the resist surface to increase the thickness of the pattern and maintain the shape of the pattern, and thus reduce the pitch interval.

[0055] In some embodiments, the method of forming a pattern using a metal-containing resist composition may include coating the metal-containing resist composition on a substrate having a thin film formed thereon by spin coating, slit coating, inkjet printing and / or the like, and drying it to form a resist film. The metal-containing resist composition may include a tin compound, for example, the tin compound may include at least one selected from a tin compound containing an organic oxygen group and a tin compound containing an organic carbonyl oxygen group.

[0056] For example, the metal compound included in the metal-containing resist composition may be represented by Chemical Formula 1.

[0057] [Chemical formula 1]

[0058]

[0059] In Chemical Formula 1,

[0060] R 1 is selected from substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, substituted or unsubstituted C7 to C30 arylalkyl, and -L a -OR a (Where L a is a substituted or unsubstituted C1 to C20 alkylene group, and R a is a substituted or unsubstituted C1 to C20 alkyl),

[0061] R 2 To R 4 each independently represents a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, a substituted or unsubstituted C7 to C30 aralkyl group, -OR b or -OC(=O)R c ,

[0062] R 2 to R 4 At least one of them is independently -OR b or -OC(=O)R c ,

[0063] R bis a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof, and

[0064] R c is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof.

[0065] R b and R c Each independently may be a substituted or unsubstituted C1 to C20 alkyl group.

[0066] Next, a first heat treatment process of heating the substrate on which the metal-containing photoresist film is formed is performed. The first heat treatment process may be performed at a temperature of about 80° C. to about 120° C. In an embodiment of the process, the solvent is evaporated and the metal-containing photoresist film may be more firmly bonded to the substrate.

[0067] Then, the photoresist film is selectively exposed using the patterned mask.

[0068] In some embodiments, examples of light that can be used in the exposure process may include not only light with a short wavelength, such as i-line (wavelength 365nm), KrF excimer laser (wavelength 248nm), ArF excimer laser (wavelength 193nm), but also light with a high-energy wavelength, such as EUV (extreme ultraviolet light, wavelength 13.5nm), electron beam (electron beam, E-Beam), etc.

[0069] In some embodiments, the light used for exposure according to some exemplary embodiments may be light having a short wavelength in the range of about 5 nm to about 150 nm, but also light having a high-energy wavelength, such as EUV (extreme ultraviolet light; wavelength: about 13.5 nm), electron beam (E-Beam) and / or the like.

[0070] In the formation of the photoresist pattern, a negative type pattern may be formed.

[0071] The exposed region of the photoresist film has a solubility different from that of the unexposed region of the photoresist film because the polymer is formed by a cross-linking reaction such as condensation between organic metal compounds.

[0072] Then, a second heat treatment process is performed on the substrate. The second heat treatment process may be performed at a temperature of about 90° C. to about 200° C. By performing the second heat treatment process, the exposed area of ​​the photoresist film becomes difficult to dissolve in the developer solution.

[0073] Then, development using a developer composition may be carried out.

[0074] In some embodiments, a photoresist pattern corresponding to a negative tone image may be completed by applying a developer composition to dissolve the photoresist film corresponding to an unexposed area and then removing the photoresist film.

[0075] Figures 1 to 3 are cross-sectional views showing a process sequence to explain an embodiment of a method of forming a pattern.

[0076] Reference Figure 1 , on the substrate 100, the exposed photoresist film is developed to form a photoresist pattern 130P.

[0077] In some example embodiments, the exposed photoresist film may be developed to remove unexposed regions of the photoresist film, and a photoresist pattern 130P including the exposed regions of the photoresist film may be formed. The photoresist pattern 130P may include a plurality of openings OP.

[0078] In some exemplary embodiments, the development of the photoresist film may be performed by a negative-tone development (NTD) process. In some embodiments, the metal-containing photoresist developer composition according to the embodiments may be used as a developer composition.

[0079] Reference Figure 2 , using photoresist pattern 130P to Figure 1 The resulting feature layer 110 is shown processed.

[0080] For example, the feature layer 110 is processed by various suitable processes: etching the feature layer 110 exposed through the opening OP of the photoresist pattern 130P, implanting impurity ions into the feature layer 110, forming an additional film on the feature layer 110 through the opening OP, deforming a portion of the feature layer 110 through the opening OP, and / or the like. Figure 2 An exemplary process of processing the feature pattern 110P by etching the feature layer 110 exposed through the opening OP is shown.

[0081] Reference Figure 3 ,exist Figure 2In the resultant shown, the photoresist pattern 130P remaining on the feature pattern 110P is removed. To remove the photoresist pattern 130P, an ashing process and / or a stripping process may be used.

[0082] According to some example embodiments, the thickness of the resist film after development may increase by 5% to 100% compared to the thickness of the resist film before development.

[0083] The thickness of the resist film after development can be increased by including at least one selected from phosphorus element and sulfur element on the surface of the resist pattern.

[0084] For example, at least one selected from the phosphorus element and the sulfur element may be included in an amount of about 5 at % to about 20 at % based on the total number of atoms.

[0085] For example, the developer composition may include an additive and an organic solvent, wherein the additive includes at least one selected from a phosphoric acid compound, a phosphorous acid compound, a hypophosphorous acid compound, and a sulfonic acid compound.

[0086] The phosphorus element and the sulfur element contained in the surface of the resist film after development may be derived from the additive in the developer composition.

[0087] The additive may be included in an amount of about 0.01 wt % to about 10 wt % based on the total 100 wt % of the developer composition. In some embodiments, the additive may be included in an amount of about 0.01 wt % to about 7 wt %, about 0.01 wt % to about 5 wt %, about 0.01 wt % to about 3 wt %, or about 0.01 wt % to about 1 wt %.

[0088] For example, the phosphorous acid compound can be at least one of the following: phosphonic acid, methylphosphonic acid, ethylphosphonic acid, butylphosphonic acid, hexylphosphonic acid, n-octylphosphonic acid, tetradecylphosphonic acid, octadecylphosphonic acid, phenylphosphonic acid, vinylphosphonic acid, aminomethylphosphonic acid, methylenediaminetetramethylenephosphonic acid, ethylenediaminetetramethylenephosphonic acid, 1-amino-1-phosphonooctylphosphonic acid, hydroxyethylphosphonic acid, 2-aminoethylphosphonic acid, 3-aminopropylphosphonic acid, 4-methylphenylphosphonic acid, 3-methylphenylphosphonic acid, 1H,1H,2H,2H-perfluorooctanephosphonic acid, cyclohexylmethylphosphonic acid, 2-thienylmethylphosphonic acid, 4-fluorophenylphosphonic acid, benzylphosphonic acid or a combination thereof.

[0089] For example, the hypophosphorous acid compound may be at least one of the following: diphenylphosphinic acid, bis(4-methoxyphenyl)phosphinic acid, phosphinic acid, bis(hydroxymethyl)phosphinic acid, phenylphosphinic acid, p-(3-aminopropyl)-p-butylphosphinic acid, or a combination thereof.

[0090] For example, the sulfonic acid compound may be at least one of the following: p-toluenesulfonic acid, benzenesulfonic acid, p-dodecylbenzenesulfonic acid, 1,4-naphthalene disulfonic acid, methanesulfonic acid, phenylmethanesulfonic acid, 1-octanesulfonic acid, 4-vinylbenzenesulfonic acid, 2-methylbenzenesulfonic acid, ethanesulfonic acid, 2,5-dimethylbenzenesulfonic acid, 2,4-dimethylbenzenesulfonic acid, allylsulfonic acid, 1-butanesulfonic acid, 1-propanesulfonic acid, 2-propanesulfonic acid, vinylbenzenesulfonic acid, hexanesulfonic acid, heptanesulfonic acid or a combination thereof.

[0091] Examples of the organic solvent included in the metal-containing photoresist developer composition according to the embodiment may include at least one selected from ethers, alcohols, glycol ethers, aromatic hydrocarbon compounds, ketones, and esters, but are not limited thereto. For example, the organic solvent may include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl celulose acetate, ethyl celulose acetate, diethylene glycol methyl ether, diethylene glycol ethyl ether, propylene glycol, propylene glycol methyl ether (PGME), propylene glycol methyl ether acetate (PGMEA), propylene glycol ethyl ether, propylene glycol ethyl ether acetate, propylene glycol propyl ether acetate, propylene glycol butyl ether, propylene glycol butyl ether acetate, ethanol, propanol, isopropyl alcohol, isobutyl alcohol, 4-methyl-2-pentenol (also referred to as methyl isobutyl carbinol) carbinol, MIBC)), hexanol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, ethylene glycol, propylene glycol, heptanone, propylene carbonate, butylene carbonate, toluene, xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-hydroxyethyl propionate, 2-hydroxy-2-methylethyl propionate, ethyl ethoxyacetate, ethyl hydroxyacetate, 2-hydroxy-3-methylmethyl butyrate, 3-methoxymethyl propionate, 3-methoxyethyl propionate, 3-ethoxyethyl propionate, 3-ethoxymethyl propionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, γ-butyrolactone, methyl 2-hydroxyisobutyrate, methoxybenzene, n-butyl acetate, 1-methoxy-2-propyl acetate, methoxyethoxypropionate, ethoxyethoxypropionate or a combination thereof, but are not limited thereto.

[0092] If other additives are included as will be further described herein below, a balance of organic solvents may be included in addition to the components.

[0093] The developer composition may further include at least one other additive selected from a surfactant, a dispersant, a moisture absorbent, and a coupling agent.

[0094] Surfactants can be used to improve coating uniformity and improve the wettability of the photoresist composition. In some exemplary embodiments, the surfactant can be a sulfate, a sulfonate, a phosphate, a soap, an amine salt, a quaternary ammonium salt, a polyethylene glycol, an alkylphenol ethylene oxide adduct, a polyol, a nitrogen-containing vinyl polymer or a combination thereof, but is not limited thereto. For example, the surfactant can include an alkylbenzene sulfonate, an alkylpyridinium salt, a polyethylene glycol and / or a quaternary ammonium salt. If the photoresist composition includes a surfactant, the surfactant can be included in an amount of about 0.001wt% to about 3wt% based on the total weight of the photoresist composition.

[0095] The dispersant can be used to evenly (e.g., substantially evenly) disperse each component constituting the photoresist composition in the photoresist composition. In an embodiment, the dispersant can be an epoxy resin, polyvinyl alcohol, polyvinyl butyral, polyvinyl pyrrolidone, glucose, sodium lauryl sulfate, sodium citrate, oleic acid, linoleic acid, or a combination thereof, but is not limited thereto. If the photoresist composition includes the dispersant, the dispersant can be included in an amount of about 0.001 wt % to about 5 wt % based on the total weight of the photoresist composition.

[0096] The desiccant may be used to prevent or reduce the adverse effects of moisture in the photoresist composition. For example, the desiccant may be used to prevent or reduce oxidation of metals contained in the photoresist composition due to moisture. In an embodiment, the desiccant may be polyoxyethylene nonylphenol ether, polyethylene glycol, polypropylene glycol, polyacrylamide, or a combination thereof, but is not limited thereto. If the photoresist composition includes the desiccant, the desiccant may be included in an amount of about 0.001 wt % to about 10 wt % based on the total weight of the photoresist composition.

[0097] The coupling agent can be used to improve the adhesion to the lower film when the photoresist composition is coated on the lower film. In an embodiment, the coupling agent may include a silane coupling agent. The silane coupling agent may be vinyl trimethoxy silane, vinyl triethoxy silane, vinyl trichlorosilane, vinyl tri (β-methoxyethoxy) silane, 3-methacryloxy propyl trimethoxy silane, 3-acryloxy propyl trimethoxy silane, p-phenylene trimethoxy silane, 3-methacryloxy propyl methyl dimethoxy silane, 3-methacryloxy propyl methyl diethoxy silane and / or trimethoxy [3- (phenylamino) propyl] silane, but is not limited thereto. If the photoresist composition includes a coupling agent, the coupling agent may be included in an amount of about 0.001wt% to about 5wt% based on the total weight of the photoresist composition.

[0098] As described above, a photoresist pattern formed by exposure to light having a short wavelength such as i-line (wavelength 365 nm), KrF excimer laser (wavelength 248 nm), ArF excimer laser (wavelength 193 nm), etc., but also to light having high energy such as EUV (extreme ultraviolet light; wavelength 13.5 nm) or electron beam (E-beam) may have a thickness width of about 5 nm to about 100 nm. For example, the photoresist pattern may be formed to have a thickness width of about 5 nm to about 90 nm, about 5 nm to about 80 nm, about 5 nm to about 70 nm, about 5 nm to about 60 nm, about 5 nm to about 50 nm, about 5 nm to about 40 nm, about 5 nm to about 30 nm, or about 5 nm to about 20 nm.

[0099] In some embodiments, the photoresist pattern may have a pitch with a half-pitch of less than or equal to about 50 nm, such as less than or equal to about 40 nm, such as less than or equal to about 30 nm, such as less than or equal to about 20 nm, such as less than or equal to about 15 nm, and the photoresist pattern may have a line width roughness of less than or equal to about 10 nm, less than or equal to about 5 nm, less than or equal to about 3 nm, or less than or equal to about 2 nm.

[0100] Hereinafter, the embodiments of the present disclosure will be described in more detail by examples related to the preparation of the aforementioned metal-containing photoresist developer composition. However, the technical features of the present disclosure are not limited by the following examples.

[0101] Preparation of metal-containing photoresist developer composition

[0102] The organic solvent and the additive were mixed together in a polypropylene (PP) bottle with each component shown in Table 1, and then shaken at room temperature (25° C.) to completely dissolve them. Subsequently, the obtained solution was filtered through a polytetrafluoroethylene (PTFE) filter having a pore size of 1 μm to obtain a developer composition.

[0103] [Table 1]

[0104]

[0105] Preparation of metal-containing photoresist compositions

[0106] An organic metal compound having a structural unit represented by Chemical Formula C was dissolved in 4-methyl-2-pentanol at a concentration of 1 wt %, and then filtered through a 0.1 μm polytetrafluoroethylene (PTFE) syringe filter to prepare a metal-containing photoresist composition.

[0107] [Chemical formula C]

[0108]

[0109] Evaluation 1: Pattern thickness measurement and XPS analysis

[0110] After hexamethyldisilazane (HMDS) was spin-coated to form a hydrophobic surface on an 8-inch silicon wafer, the prepared metal-containing photoresist (PR) composition was spin-coated on the treated wafer at 1,500 rpm for 30 seconds and then heat-treated at 160° C. for 60 seconds to produce a coated wafer.

[0111] EUV light (Lawrence Berkeley National Laboratory Micro Exposure Tool, MET) is projected onto the wafer. Here, the pad exposure time is adjusted to apply an increasing EUV dose to each pad.

[0112] Subsequently, the resist and substrate were exposed on a hot plate at 180°C for 90 seconds, and then post-exposure baking (PEB) was performed. The baked film was immersed in each developer according to Examples 1 to 7 and Comparative Examples 1 to 3 for 30 seconds, and was additionally washed with the same developer for 15 seconds to form a negative image, i.e., to remove the unexposed coating area. Finally, another hot plate baking was performed at 240°C for 60 seconds to complete the process.

[0113] The residual resist thickness of the exposed pad of the coated wafer was measured at 70° in the wavelength range of 280 nm to 1,000 nm by using an ellipsometer M2000 manufactured by JA Woolam.

[0114] The thickness measurement results are shown in Table 2 and Figure 4 middle.

[0115] The thickness increase rate was calculated according to the following equation 1:

[0116] [Equation 1]

[0117] {(thickness of the photoresist film after development) - (thickness of the photoresist film before development)} / (thickness of the photoresist film after development)] × 100

[0118] The residual resist was subjected to component analysis by X-ray photoelectron spectroscopy (XPS) (AXIS SUPRA, KRATOS Analytical Ltd.), and the results are shown in Figure 5 The analysis was performed in XPS monochromatic mode by setting the beam size to 700 μm during narrow scan, the source power to 150 W for wide scan and 225 W for narrow scan, and a resolution of 20 eV at 0.1 eV intervals for C1s, O1s, P2p, Sn3d, and S3p, respectively, and The surface thickness is measured under the standard.

[0119] Assessment 2: CD Measurement

[0120] The developer was evaluated by injection in the development process during the coating-exposure-development process for manufacturing the pattern wafer. When the process was completed, the pattern wafer on which the line / space CD pattern (critical dimension) pattern was formed was transferred to a GC-5000 critical dimension-scanning electron microscope (CD-SEM) measuring device manufactured by Hitachi Ltd. to measure the CD (critical dimension) size in the area where the half pitch of the mask pattern was 14 nm, and the minimum value of the spacing CD (distance between lines) is shown in Table 2 and Table 3. Figure 6 middle.

[0121] [Table 2]

[0122]

[0123] (*HP: half pitch reference value)

[0124] Referring to Table 2, compared with the metal-containing photoresist developer compositions according to Comparative Examples 1 to 3, the metal-containing photoresist developer compositions according to Examples 1 to 7 exhibited a small amount of residue and reduced pitch CD in the dissolved pitch area due to the increased thickness of the resist film after development, and thus exhibited excellent resolution and reduced bridging and residue.

[0125] Figure 4 is a scanning electron micrograph comparing the thickness of the resist film after development.

[0126] Reference Figure 4 When a developer composition of a sulfonic acid compound is used (Example 5), the thickness of the photoresist film shows an increase compared to when no developer is used (Comparative Example 1) or when a developer composition to which an organic acid is added is used (Comparative Example 2).

[0127] Figure 5 It is a graph showing the results of XPS analysis of the resist film after development.

[0128] Reference Figure 5 As a result of XPS analysis of the resist film after development, the resist film was confirmed to contain the P component. Therefore, the additive component in the developer composition was adsorbed onto the surface of the resist film.

[0129] Figure 6 is a scanning electron micrograph showing the resist pattern after development.

[0130] Reference Figure 6When P component or S component is included among the additive components, the thickness of the resist pattern increases because the P component and the S component are adsorbed on the surface of the resist film, but a small amount of dissolved residue reduces bridging even at a narrow pitch CD (10.5nm), thereby achieving a pattern with excellent resolution. This effect can minimize or reduce the semiconductor line width by minimizing or reducing the size of the pitch portion of the pattern.

[0131] In the above, some embodiments of the present disclosure have been described and illustrated. However, it is obvious to those skilled in the art that the present disclosure is not limited to the described embodiments, and various modifications and changes can be made without departing from the spirit and scope of the present disclosure. Therefore, the modified or changed embodiments themselves may not be understood separately from the technical ideas and aspects of the present disclosure, and the modified embodiments are within the scope of the claims of the present disclosure.

Claims

1. A method for forming a pattern, comprising: coating a metal-containing resist composition on a substrate; performing drying and heating to form a metal-containing resist film on the substrate; exposing the metal-containing resist film using a patterned mask; as well as applying a developer composition to remove the unexposed areas, thereby forming a resist pattern, wherein the thickness of the metal-containing resist film increases by 5% to 100% after development compared to the thickness of the metal-containing resist film before development, The surface of the metal-containing resist film after the development includes 5 at % to 20 at % of at least one selected from phosphorus and sulfur, based on the total number of atoms.

2. The method according to claim 1, wherein: The developer composition comprises an additive and an organic solvent, wherein the additive comprises at least one selected from a phosphoric acid compound, a phosphorous acid compound, a hypophosphorous acid compound and a sulfonic acid compound.

3. The method according to claim 2, wherein: The additive is included in an amount of 0.01 wt % to 10 wt %.

4. The method according to claim 2, wherein: The phosphorous acid compound is at least one of the following: phosphonic acid, methylphosphonic acid, ethylphosphonic acid, butylphosphonic acid, hexylphosphonic acid, n-octylphosphonic acid, tetradecylphosphonic acid, octadecylphosphonic acid, phenylphosphonic acid, vinylphosphonic acid, aminomethylphosphonic acid, methylenediaminetetramethylenephosphonic acid, ethylenediaminetetramethylenephosphonic acid, 1-amino-1-phosphonooctylphosphonic acid, hydroxyethylphosphonic acid, 2-aminoethylphosphonic acid, 3-aminopropylphosphonic acid, 4-methylphenylphosphonic acid, 3-methylphenylphosphonic acid. Acid, 2-methylphenylphosphonic acid, 4-aminophenylphosphonic acid, 3-aminophenylphosphonic acid, 2-aminophenylphosphonic acid, 3-hydroxyphenylphosphonic acid, 4-hydroxyphenylphosphonic acid, 2-hydroxyphenylphosphonic acid, 6-hydroxyhexylphosphonic acid, decylphosphonic acid, diphosphonic acid, methylene diphosphonic acid, nitrilotrimethylene triphosphonic acid, 1H,1H,2H,2H-perfluorooctanephosphonic acid, cyclohexylmethylphosphonic acid, 2-thienylmethylphosphonic acid, 4-fluorophenylphosphonic acid, benzylphosphonic acid or a combination thereof.

5. The method according to claim 2, wherein: The hypophosphorous acid compound is at least one of the following: diphenylphosphinic acid, bis(4-methoxyphenyl)phosphinic acid, phosphinic acid, bis(hydroxymethyl)phosphinic acid, phenylphosphinic acid, p-(3-aminopropyl)-p-butylphosphinic acid or a combination thereof.

6. The method according to claim 2, wherein: The sulfonic acid compound is at least one of the following: p-toluenesulfonic acid, benzenesulfonic acid, p-dodecylbenzenesulfonic acid, 1,4-naphthalene disulfonic acid, methanesulfonic acid, phenylmethanesulfonic acid, 1-octanesulfonic acid, 4-vinylbenzenesulfonic acid, 2-methylbenzenesulfonic acid, ethanesulfonic acid, 2,5-dimethylbenzenesulfonic acid, 2,4-dimethylbenzenesulfonic acid, allylsulfonic acid, 1-butanesulfonic acid, 1-propanesulfonic acid, 2-propanesulfonic acid, vinylbenzenesulfonic acid, hexanesulfonic acid, heptanesulfonic acid or a combination thereof.

7. The method according to claim 1, wherein: The metal compound contained in the metal-containing resist composition includes at least one selected from a tin compound containing an organic oxygen group and a tin compound containing an organic carbonyl oxygen group.

8. The method of claim 1, wherein: The metal compound contained in the metal-containing resist composition is represented by Chemical Formula 1: [Chemical formula 1] Wherein, in Chemical Formula 1, R 1 is selected from substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, substituted or unsubstituted C7 to C30 arylalkyl, and L a -OR a , where L a is a substituted or unsubstituted C1 to C20 alkylene group, and R a is a substituted or unsubstituted C1 to C20 alkyl group, R 2 To R 4 each independently represents a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, a substituted or unsubstituted C7 to C30 aralkyl group, -OR b or -OC(=O)R c , R 2 to R 4 At least one of them is independently selected from -OR b or -OC(=O)R c , R b is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof, and R c is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof.