Packaging sheet and preparation method and application thereof

By setting up a UV adhesive layer on the surface of the unetched substrate to form a concave protective cover, the surface unevenness and water-oxygen transmission problems caused by the etching process in PMOLED package are solved, and the strength and aesthetics are improved. for transparent display applications.

CN119031790AInactive Publication Date: 2024-11-26SUZHOU QUINGYUE OPTOELECTRONICS TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411138497.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In PMOLED packaging, the surface of the packaging sheet caused by the etching process is uneven, and the scene is distorted and line distorted after perspective. The traditional packaging method is insensitive to water and oxygen transmission, making it difficult to meet the special application needs of transparent displays.

Method used

The UV adhesive layer is arranged on the surface of the substrate that has not been etched. The UV adhesive layer is formed through screen printing and ultraviolet lamp curing to form a concave protective cover to isolate water and oxygen, and ensure the strength and adhesion of the packaging sheet, avoiding the Bad phenomena in the etching process.

Benefits of technology

The packaging sheet without etching is realized, the original transmittance and flatness of the glass is maintained, the strength and aesthetics of the packaging sheet are enhanced, the distortion after perspective and line distortion are avoided, and the waste liquid is discharged in an environmentally friendly manner.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119031790A_ABST
    Figure CN119031790A_ABST
Patent Text Reader

Abstract

The invention provides a packaging sheet and a preparation method and application thereof, and the preparation method comprises the following steps: arranging a UV glue layer on the surface of a substrate, and carrying out curing to obtain the packaging sheet, the base material is a base material which is not subjected to etching treatment; the UV adhesive layer is arranged on the periphery of the base material. According to the invention, on the premise of ensuring the original transmittance and flatness of the base material, the packaging sheet obtained by the preparation method has equivalent or even better strength and function than a packaging sheet obtained by an etching process, can replace the packaging sheet obtained by the etching process, has a good visual effect of appearance, is more convenient to use, does not discharge waste liquid in the preparation process, and is suitable for industrial production. The environment is protected.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of packaging materials, and in particular relates to a packaging sheet and a preparation method and application thereof. Background Art

[0002] The manufacturing process of passive organic light-emitting diode (PMOLED) involves the evaporation of organic materials and active metals, which are very sensitive to water and oxygen and need to prevent water and oxygen from penetrating. Therefore, PMOLED packaging is performed. The main function of PMOLED packaging is to isolate the light-emitting device from the external environment to prevent the intrusion of moisture, oxygen, impurities, etc. into the screen, thereby stabilizing the various parameters of the device. It also plays a protective role to prevent external forces from damaging the device, thereby increasing the service life of the PMOLED screen.

[0003] Usually, PMOLED packaging mainly adopts the method of adding a glass cover plate to the surface of the EL substrate, attaching a desiccant to the inside of the cover plate, and then adhering the substrate and the cover plate to each other through a sealant, and then performing negative pressure pressing and UV curing. The cover plate packaging method can form a concave protective cover between the EL substrate and the glass packaging sheet, thereby effectively isolating the PMOLED functional layers and the cathode from contact with water, oxygen and other components in the air, and can also play a role in reinforcement and protection.

[0004] However, in special application scenarios such as transparent displays (such as magnifying glasses, sights, etc.), it is necessary to see through the display device and magnify the scene. However, the encapsulation sheet prepared by etching process will produce etching lines in the corresponding display area after etching, that is, the surface is uneven after etching, and the scene will be distorted and the lines will be twisted after perspective.

[0005] Therefore, developing a method for preparing an encapsulation sheet that does not require etching and can both ensure the strength and reinforced protection of the encapsulation sheet and avoid distortion of the scene and line distortion after perspective viewing is an urgent problem to be solved in this field. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention aims to provide a packaging sheet and a preparation method and application thereof. The packaging sheet obtained by the preparation method has the same or even better strength and function as the packaging sheet obtained by the etching process while ensuring the original transmittance and flatness of the glass, and can replace the packaging sheet obtained by the etching process, and has a good visual effect and is more convenient to use, which is comparable to frameless products.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a method for preparing an encapsulation sheet, the method comprising the following steps:

[0009] A UV adhesive layer is arranged on the surface of a substrate and cured to obtain the encapsulation sheet; the substrate is a substrate that has not been etched; and the UV adhesive layer is arranged around the substrate.

[0010] In the present invention, the substrate is not subjected to etching treatment, the substrate surface has high flatness, and has no etching lines, dents, scratches, etc., which is beneficial to improving the transmittance of the encapsulation sheet, avoiding distortion and line twisting after perspective, and ensuring aesthetics. At the same time, no etching liquid is required, and no waste liquid is discharged during the preparation process, which is environmentally friendly. A UV adhesive layer is arranged on the surface of the substrate, so that the encapsulation sheet can form a concave protective cover, isolating the device functional layer and the cathode from contact with water, oxygen and other components in the air, and can also ensure the strength and adhesion of the encapsulation sheet.

[0011] Preferably, the substrate comprises glass.

[0012] In the present invention, the glass includes white glass.

[0013] In the present invention, the thickness of the substrate is 0.2-0.5 mm, for example, 0.2 mm, 0.25 mm, 0.3 mm, 0.35 mm, 0.4 mm, 0.45 mm, 0.5 mm, etc.

[0014] Preferably, the UV adhesive layer is arranged in a strip shape around the substrate.

[0015] Preferably, the outer side of the UV adhesive layer is flush with the side edge of the substrate.

[0016] Preferably, the length of the UV adhesive layer is the same as the length of the substrate, and the width of the UV adhesive layer is 1 / 10 to 1 / 5 of the width of the substrate, for example, it can be 1 / 10, 1 / 9, 1 / 8, 1 / 7, 1 / 6, 1 / 5, etc. Preferably, the thickness of the UV adhesive layer is 0.05 to 0.15 mm, for example, it can be 0.05 mm, 0.06 mm, 0.07 mm, 0.08 mm, 0.09 mm, 0.1 mm, 0.11 mm, 0.12 mm, 0.13 mm, 0.14 mm, 0.15 mm, etc.; preferably 0.05 to 0.1 mm.

[0017] In the present invention, the thickness of the UV adhesive layer is within the above-defined range, which can not only ensure the adhesion of the packaging sheet, but also ensure that the color of the packaging sheet is close to transparent, making the packaging sheet beautiful and convenient for analyzing the abnormalities of the metal routing in the packaging area; if the thickness is too low, the adhesion is low and it cannot be used; if the thickness is too high, the color is green.

[0018] Preferably, the method of providing the UV adhesive layer comprises screen printing.

[0019] Preferably, after the UV adhesive layer is provided by screen printing, the method further includes a step of removing the mold.

[0020] In the present invention, the mold refers to a mold used for screen printing.

[0021] Preferably, the material of the UV glue layer includes UV glue.

[0022] Preferably, the UV glue includes at least one of acrylate glue, polyurethane glue or epoxy resin glue.

[0023] Preferably, the curing method comprises irradiating with ultraviolet light.

[0024] Preferably, the curing includes a first curing and a second curing.

[0025] Preferably, the first curing time is 20 to 30 seconds, for example, it can be 20 seconds, 21 seconds, 22 seconds, 23 seconds, 24 seconds, 25 seconds, 26 seconds, 27 seconds, 28 seconds, 29 seconds, 30 seconds, etc.

[0026] In the present invention, ultraviolet light is used for irradiation for 20 to 30 seconds, and pre-curing is performed first, so that the obtained packaging sheet has better adhesion performance; wherein, if screen printing UV glue is used, the first curing time is too long, which will cause the screen and the packaging sheet to adhere, and cause the UV glue layer to deform.

[0027] Preferably, the second curing time is 150 to 270 s, for example, it can be 150s, 155s, 160s, 165s, 170s, 175s, 180s, 185s, 190s, 195s, 200s, 205s, 210s, 215s, 220s, 225s, 230s, 235s, 240s, 245s, 250s, 255s, 260s, 265s, 270s, etc.; more preferably, it is 180 to 260 s.

[0028] In the present invention, when the second curing time is within a specific range, the curing strength and adhesion of the encapsulation sheet are better; if the curing time is too short, the curing strength and adhesion are low; if the curing time is too long, the UV adhesive layer becomes brittle, which also leads to reduced adhesion.

[0029] Preferably, the preparation method comprises the following steps:

[0030] UV glue with a thickness of 0.05 to 0.15 mm is screen-printed around the unetched glass surface, and after irradiating with ultraviolet light for 20 to 30 seconds, the mold is removed, and the ultraviolet light is continuously irradiated for 150 to 270 seconds to obtain the packaging sheet.

[0031] In a second aspect, the present invention provides an encapsulation sheet, which is prepared according to the preparation method described in the first aspect.

[0032] In a third aspect, the present invention provides a use of a packaging sheet prepared according to the preparation method described in the first aspect or a packaging sheet described in the second aspect in a passive organic light emitting diode packaging.

[0033] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] The preparation method of the encapsulation sheet provided by the present invention does not perform etching treatment on the substrate, thereby ensuring that the substrate has high transmittance and high flatness, has no bad marks such as dots or lines, and has no etching marks, avoids the residual liquid medicine and water stains caused by the etching process, avoids distortion and line twisting after perspective, and ensures aesthetics; a UV adhesive layer is arranged on the surface of the substrate, so that the encapsulation sheet can form a concave protective cover, isolates the device functional layer and the cathode from contact with water, oxygen and other components in the air, and can also ensure the strength and adhesion of the encapsulation sheet, and the UV adhesive layer is not easy to deform; in addition, no waste liquid is discharged during the preparation process, which is environmentally friendly and pollution-free. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is an appearance diagram of a packaging sheet obtained by the preparation method provided in Example 1 of the present invention;

[0037] Figure 2 This is an appearance diagram of a packaging sheet obtained by the preparation method provided in Example 2 of the present invention;

[0038] Figure 3 This is an appearance diagram of the encapsulation sheet obtained by the preparation method provided in Example 3 of the present invention;

[0039] Figure 4 This is an appearance diagram of a packaging sheet obtained by the preparation method provided in Example 4 of the present invention;

[0040] Figure 5 This is an appearance diagram of a packaging sheet obtained by the preparation method provided in Example 5 of the present invention;

[0041] Figure 6 A schematic diagram of the cross-sectional structure of a PMOLED containing only a substrate and a packaging sheet after the packaging sheet provided by the present invention is used for PMOLED packaging;

[0042] Among them, 1-substrate; 2-encapsulation sheet; 21-unetched white glass; 22-UV adhesive layer;

[0043] Figure 7A schematic diagram of the cross-sectional structure of a PMOLED comprising a substrate, a functional layer, a drying material and a packaging sheet after the packaging sheet provided by the present invention is used for PMOLED packaging;

[0044] Among them, 100-substrate; 101-indium tin oxide conductive glass (ITO); 102-anode; 103-hole injection layer; 104-hole transport layer; 105-light-emitting layer; 106-electron transport layer; 107-electron injection layer; 108-cathode; 109-cathode modification layer; 110-encapsulation sheet; 210-unetched white glass; 220-UV adhesive layer; 310-drying material. DETAILED DESCRIPTION

[0045] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0046] The materials used in the present invention can be purchased from the market or prepared by conventional methods; unless otherwise specified, the materials used in the present invention are as follows:

[0047] UV glue: Three-bond epoxy resin UV glue TB3114;

[0048] White glass: Liguang alkaline substrate; thickness is 0.3mm.

[0049] Example 1

[0050] This embodiment provides a method for preparing a packaging sheet, which specifically includes the following steps:

[0051] UV glue with a thickness of 0.05 mm is screen-printed around the unetched white glass surface to form a UV glue wall frame (i.e., UV glue layer), and the outer side of the UV glue layer is flush with the side of the white glass; the length of the UV glue layer is the same as that of the white glass, and the width of a single side is 1 / 8 of the white glass; after the first curing is performed by ultraviolet light irradiation for 25 seconds, the screen is removed, and the ultraviolet light is continued to be irradiated for 200 seconds for the second curing to obtain the packaging sheet.

[0052] Example 2

[0053] This embodiment provides a method for preparing a packaging sheet, which is different from Embodiment 1 only in that UV glue with a thickness of 0.1 mm is screen-printed, and other steps are the same as those of Embodiment 1.

[0054] Example 3

[0055] This embodiment provides a method for preparing a packaging sheet, which is different from Embodiment 1 only in that UV glue with a thickness of 0.15 mm is screen-printed, and other steps are the same as those in Embodiment 1.

[0056] Example 4

[0057] This embodiment provides a method for preparing a packaging sheet, which is different from Embodiment 1 only in that UV glue with a thickness of 0.2 mm is screen-printed, and other steps are the same as those in Embodiment 1.

[0058] Example 5

[0059] This embodiment provides a method for preparing a packaging sheet, which is different from Embodiment 1 only in that UV glue with a thickness of 0.25 mm is screen-printed, and other steps are the same as those in Embodiment 1.

[0060] Example 6

[0061] This embodiment provides a method for preparing a packaging sheet, which is different from Embodiment 1 only in that the second curing time is 260 seconds, and the other steps are the same as those in Embodiment 1.

[0062] Example 7

[0063] This embodiment provides a method for preparing a packaging sheet, which is different from the first embodiment only in that the second curing time is 320 seconds, and the other steps are the same as the first embodiment.

[0064] Example 8

[0065] This embodiment provides a method for preparing a packaging sheet, which is different from Embodiment 1 only in that the second curing time is 120 seconds, and the other steps are the same as those in Embodiment 1.

[0066] Example 9

[0067] This embodiment provides a method for preparing a packaging sheet, which is different from the first embodiment only in that the second curing time is 60 seconds, and the other steps are the same as those in the first embodiment.

[0068] Application Examples

[0069] This application example provides an application of an encapsulation sheet obtained by the preparation method provided in Examples 1 to 9 in PMOLED encapsulation; the structural schematic diagram of the PMOLED cross section after encapsulation is as follows: Figure 6 As shown; comprising a PMOLED substrate 1 and a packaging sheet 2; the packaging sheet 2 comprises an unetched white glass 21 and a UV adhesive layer 22; different functional layers can be set on the surface of the substrate 1; the surface of the unetched white glass 21 can be provided with a dry material.

[0070] The cross-sectional structure diagram of the packaged PMOLED after different functional layers are arranged on the substrate surface and dry materials are arranged on the unetched white glass surface is shown in FIG. Figure 7 As shown; it includes a substrate 100, an ITO conductive glass 101, an anode 102, a hole injection layer 103, a hole transport layer 104, a light-emitting layer 105, an electron transport layer 106, an electron injection layer 107, a cathode 108, a cathode modification layer 109 and a packaging sheet 110; the packaging sheet includes unetched white glass 210 and a UV glue layer 220; the surface of the unetched white glass 210 is provided with a drying material 310.

[0071] Performance Testing

[0072] (1) Appearance: Observe the color and transparency of the encapsulation sheet visually. The whiter and more transparent the encapsulation sheet is, the better the performance of the encapsulation sheet is.

[0073] The appearance of the encapsulation sheet obtained by the preparation method provided in Example 1 is as follows: Figure 1 As shown; the appearance of the encapsulation sheet obtained by the preparation method provided in Example 2 is as shown Figure 2 The appearance of the encapsulation sheet obtained by the preparation method provided in Example 3 is shown in Figure 3 The appearance of the encapsulation sheet obtained by the preparation method provided in Example 4 is shown in Figure 4 The appearance of the encapsulation sheet obtained by the preparation method provided in Example 5 is shown in Figure 5 As shown;

[0074] Depend on Figure 1 to Figure 5 It can be seen that when the thickness of the UV adhesive layer is within a specific range, the color of the packaging sheet is whiter and more transparent; when the thickness is too high, the packaging sheet will gradually turn green, which is aesthetically pleasing and also makes it inconvenient to analyze abnormalities of metal traces in the packaging area.

[0075] (2) Adhesion: The adhesion of the encapsulation sheet obtained by the preparation method provided in Examples 1, 6 to 9 was tested. The specific testing method includes: preparing one AB glue and one AB glue (Kangda New Materials High-Performance AB Glue WD1001), mixing A glue and B glue at a mass ratio of 1:1, and evenly applying the mixture on the iron plate. The AB glue should not be applied to the side and screw holes of the iron plate. Then, the screen to be tested (PMOLED device encapsulated by the encapsulation sheet) is placed with the substrate facing upward, the cut edge of the step area is aligned with the edge of the iron plate, and the encapsulation surface is adhered to the iron plate coated with the AB glue with the encapsulation surface facing downward, and pressed with fingers for about 5 seconds. Be careful not to let the AB glue overflow onto the step area and the substrate surface when pressing; leave the glued screen to be tested for more than 12 hours to allow the AB glue to dry and solidify; then turn on the power of the adhesion tester, rotate the pressure gauge pointer to the value of 0.4Mpa, open the upper cover of the tester, use nuts to fix the iron plate to the screw holes at both ends, cover the upper cover of the tester, press the green button on the left (up button), and the black top block rises until the screen is pushed open; record the corresponding value on the digital display when the screen is pushed open, this value is the corresponding adhesion size of the screen (converted to the equivalent gravity size, so its unit is kg).

[0076] The specific test results of adhesion are shown in Table 1:

[0077] Table 1

[0078]

[0079]

[0080] As shown in Table 1, the preparation method provided by the present invention has a second curing time within a specific range, a high curing strength, a high adhesion, and meets the 3 kg adhesion requirement. As shown in Examples 1, 6, and 7, the encapsulation sheet can reach 3.25 to 6.56 N; as shown in Examples 8 and 9, the second curing time is too short, the curing strength is low, and the 3 kg adhesion requirement is not met.

[0081] In summary, the preparation method provided by the present invention, by setting a UV adhesive layer on the surface of the substrate, does not need to be etched on the substrate, and can also form a concave protective cover to isolate the device functional layer and the cathode from contact with water, oxygen and other components in the air, and can also ensure the strength and adhesion of the packaging sheet. The UV adhesive layer is not easy to deform, avoiding the distortion and line distortion after perspective caused by the etching process, and also avoiding the residual liquid and water stains caused by the etching process. The preparation process is environmentally friendly and pollution-free.

[0082] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a packaging sheet, characterized in that: The preparation method comprises the following steps: Arranging a UV adhesive layer on the surface of the substrate and curing it to obtain the encapsulation sheet; The substrate is a substrate that has not been etched; the UV adhesive layer is arranged around the substrate.

2. The preparation method according to claim 1, characterized in that: The substrate includes glass.

3. The preparation method according to claim 1 or 2, characterized in that: The UV adhesive layer is arranged in a strip shape around the substrate; Preferably, the outer side of the UV adhesive layer is flush with the side edge of the substrate; Preferably, the length of the UV adhesive layer is the same as the length of the substrate, and the width of the UV adhesive layer is 1 / 10 to 1 / 5 of the width of the substrate.

4. The preparation method according to any one of claims 1 to 3, characterized in that: The thickness of the UV adhesive layer is 0.05-0.15 mm, preferably 0.05-0.1 mm.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The method of setting the UV adhesive layer includes screen printing; Preferably, after the UV adhesive layer is provided by screen printing, the step of removing the mold is also included; Preferably, the material of the UV adhesive layer includes UV glue; Preferably, the UV glue includes at least one of acrylate glue, polyurethane glue or epoxy resin glue.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The curing method includes irradiation with ultraviolet light; Preferably, the curing includes a first curing and a second curing.

7. The preparation method according to claim 6, characterized in that: The first curing time is 20 to 30 seconds; Preferably, the second curing time is 150 to 270 seconds, more preferably 180 to 260 seconds.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: UV glue with a thickness of 0.05 to 0.15 mm is screen-printed around the unetched glass surface, and after irradiating with ultraviolet light for 20 to 30 seconds, the mold is removed, and the ultraviolet light is continuously irradiated for 150 to 270 seconds to obtain the packaging sheet.

9. A packaging sheet, characterized in that: The encapsulation sheet is prepared according to the preparation method according to any one of claims 1 to 8.

10. Use of a packaging sheet prepared by the preparation method according to any one of claims 1 to 8 or a packaging sheet according to claim 9 in passive organic light emitting diode packaging.

Citation Information

Cited By

  • Encapsulation sheet, preparation method therefor and application thereof

    WO2026040371A1