Copper-manganese composite adsorption material as well as preparation method and application thereof
Through the purification reaction of copper-manganese composite adsorbent material contacting hydrogen at low temperature, the problem of difficulty in dealing with trace sulfides in hydrogen in the prior art is solved, and the sulfide content of hydrogen used in fuel cells is achieved in compliance with the standards, reducing costs and simplifying Craft.
Patent Information
- Application Number
- CN202310617339.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-05-29
AI Technical Summary
The existing desulfurization technology is difficult to effectively treat trace sulfides in hydrogen below 50°C, and the process is complex and costly, which cannot meet the strict sulfide content requirements for hydrogen used in fuel cells.
Using copper-manganese composite adsorbent material, the filtered stock solution mixture of graphite oxide and copper source is prepared by the improved Hummer method for hydrothermal treatment, and the copper-manganese composite adsorbent material is prepared for contacting hydrogen at low temperature for purification reaction, effectively removing hydrogen sulfide in it.
At a temperature of 20 to 50°C, the copper-manganese composite adsorbent material can effectively reduce the sulfide content in hydrogen, meet the standard requirements for hydrogen for fuel cells, reduce the preparation cost, and avoid wastewater pollution.
Smart Images

Figure BDA0004254351110000091 
Figure BDA0004254351110000101
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of hydrogen purification, and specifically relates to a copper-manganese composite adsorption material and a preparation method and application thereof. Background Art
[0002] As an important energy source, one of the uses of hydrogen is to supply hydrogen to fuel cells and generate electricity to realize the utilization of hydrogen energy. However, the electrode catalyst of the fuel cell is sensitive to sulfides. The presence of trace sulfides will cause the fuel cell electrode catalyst to be poisoned, thereby reducing its efficiency. Therefore, strict requirements are placed on the sulfide content of hydrogen used in fuel cells. The international requirement is that the sulfide content calculated as hydrogen sulfide must be less than 4ppb, which is the most stringent requirement for the impurity content in hydrogen used in fuel cells. How to ensure that the sulfide content of hydrogen used in fuel cells is qualified is the technical key to hydrogen used in fuel cells. Existing desulfurization technologies are mostly aimed at conventional sulfides (>0.1%), while there are few treatment methods for trace sulfides (such as less than 100ppm) in hydrogen at temperatures below 50°C, or there are problems such as complex treatment processes and high treatment costs. Summary of the invention
[0003] The purpose of the present disclosure is to provide a copper-manganese composite adsorption material and a preparation method and application thereof. The preparation method of the present invention reduces the preparation cost by mixing a mixture of a copper source and a filtered stock solution of graphite oxide, and using the mixture of the filtered stock solution of graphite oxide as a manganese source. The copper-manganese composite adsorption material prepared by the present invention can effectively remove sulfides from hydrogen raw gas during the hydrogen purification reaction process, and the sulfide content in the purified hydrogen can meet the standard requirements for the sulfide content in hydrogen used in fuel cells.
[0004] In order to achieve the above-mentioned purpose, the first aspect of the present disclosure provides a copper-manganese composite adsorption material, wherein the copper-manganese composite adsorption material includes copper element, manganese element, sulfur element, potassium element and oxygen element. Based on the mass of the copper-manganese composite adsorption material, the copper element content is 1-15 weight %, the manganese element content is 20-60 weight %, the sulfur element content is 1-10 weight %, and the potassium element content is 2-15 weight %.
[0005] Optionally, the copper-manganese composite adsorption material is a black powder with an average particle size of less than 0.28 mm, preferably less than 0.1 mm, and a specific surface area of 180 to 400 m 2 / g, preferably 200 to 300 m 2 / g, the pore volume is 0.3-1.0 ml / g, preferably 0.5-0.8 ml / g, and the most probable pore diameter is 15-50 nm, preferably 20-40 nm.
[0006] A second aspect of the present disclosure provides a method for preparing a copper-manganese composite adsorption material and graphite oxide, the method comprising:
[0007] S1 uses an improved Hummer method to prepare graphite oxide, and the obtained material is subjected to solid-liquid separation, the obtained liquid phase is a mixture of the filtered stock solution, and the obtained solid phase is graphite oxide after drying;
[0008] S2: hydrothermally treating the mixture of the copper source and the filtered stock solution and recovering the solid phase material to obtain a copper-manganese composite adsorption material;
[0009] Wherein, no nitrate and hydrogen peroxide are added during the reaction process of the improved Hummer method;
[0010] The molar ratio of manganese element in the mixture of the copper source and the filtered stock solution is (1-20):100;
[0011] Optionally, the graphite oxide has an oxygen content of 20 to 30% by weight and a carbon content of 70 to 80% by weight.
[0012] Optionally, the molar ratio of manganese element in the mixture of the copper source and the filtered stock solution is (2-10):100;
[0013] Among them, in the mixture of the filtered raw liquid, the manganese content calculated as divalent manganese ions is 2-30 g / L, the potassium content calculated as potassium ions is 1-20 g / L, the sulfur content calculated as sulfate ions is 10-150 g / L, and the carbon content calculated as carbon atoms is 0.5-10 g / L.
[0014] Optionally, step S2 includes:
[0015] (1) mixing a copper source with the mixture of the filtered stock solution and optionally water to obtain a mixed solution;
[0016] (2) subjecting the mixed solution to hydrothermal treatment, taking out a solid product, washing, drying and optionally calcining the solid product to obtain the copper-manganese composite adsorption material.
[0017] Optionally, the valence state of the copper element in the copper source is monovalent or divalent;
[0018] The copper source is one or more of an inorganic copper salt, a copper oxide or an organic copper-containing compound.
[0019] Optionally, the conditions of the hydrothermal treatment include: a temperature of 100 to 200° C. and a time of 1 to 72 h under autogenous pressure;
[0020] The calcination conditions include: temperature of 300-600° C., time of 1-12 hours, pressure of 0.1-0.5 MPa, and calcination atmosphere of nitrogen or air.
[0021] The third aspect of the present disclosure provides a hydrogen purification method, which comprises: contacting hydrogen raw gas with the copper-manganese composite adsorption material described in the first aspect of the present disclosure at a temperature of 20 to 50° C. to perform a purification reaction.
[0022] Optionally, the reaction conditions of the hydrogen purification method include: temperature of 20-50°C, pressure of 0.1-5.0 MPa, and space velocity of 500-500000 h -1 ;
[0023] The mass content of sulfide in the hydrogen raw gas is less than 1000 ppm, and the content of sulfide in the hydrogen raw gas is calculated as hydrogen sulfide.
[0024] Through the above technical scheme, the present invention mixes a mixture of a copper source and a filtered stock solution of graphite oxide, performs a hydrothermal treatment under hydrothermal autogenous pressure and atmosphere, and optionally roasts to obtain a copper-manganese composite adsorption material, and uses the mixture of the filtered stock solution of graphite oxide as a manganese source to reduce the preparation cost. The copper-manganese composite adsorption material prepared by the present invention can effectively remove sulfides from hydrogen raw gas during the hydrogen purification reaction process, and can achieve the removal of sulfides from hydrogen at a temperature below 50°C. The content of sulfides in the purified hydrogen can meet the standard requirements for the content of sulfide impurities in hydrogen used in fuel cells.
[0025] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0026] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.
[0027] A first aspect of the present invention provides a copper-manganese composite adsorption material, wherein the copper-manganese composite adsorption material comprises copper, manganese, sulfur, potassium and oxygen. Based on the mass of the copper-manganese composite adsorption material, the copper content is 1 to 15% by weight, preferably 2 to 10% by weight; the manganese content is 20 to 60% by weight, preferably 25 to 50% by weight; the sulfur content is 1 to 10% by weight, preferably 2 to 5% by weight; the potassium content is 2 to 15% by weight, preferably 4 to 10% by weight; and the balance is O element.
[0028] In a specific embodiment of the present invention, the copper-manganese composite adsorption material is a black powder with an average particle size of less than 0.28 mm, preferably less than 0.1 mm, and a specific surface area of 180 to 400 m 2 / g, preferably 200 to 300 m 2 / g, the pore volume is 0.3-1.0 ml / g, preferably 0.5-0.8 ml / g, and the most probable pore diameter is 15-50 nm, preferably 20-40 nm.
[0029] The preparation method of the present invention mixes a mixture of a copper source and a filtered stock solution of graphite oxide, and uses the mixture of the filtered stock solution of graphite oxide as a manganese source, thereby making full use of the filtered stock solution of graphite oxide and reducing the preparation cost. At the same time, it also avoids the problem of wastewater environmental pollution in the process of preparing graphite oxide alone.
[0030] A second aspect of the present invention provides a method for preparing a copper-manganese composite adsorption material and graphite oxide, the method comprising:
[0031] S1 uses an improved Hummer method to prepare graphite oxide, and the obtained material is subjected to solid-liquid separation, the obtained liquid phase is a mixture of the filtered stock solution, and the obtained solid phase is graphite oxide after drying;
[0032] S2: hydrothermally treating the mixture of the copper source and the filtered stock solution and recovering the solid phase material to obtain a copper-manganese composite adsorption material;
[0033] Wherein, no nitrate and hydrogen peroxide are added during the reaction process of the improved Hummer method;
[0034] In a specific embodiment of the present invention, the molar ratio of manganese element in the mixture of the copper source and the filtered stock solution is (1-20):100, preferably (2-10):100.
[0035] In a specific embodiment of the present invention, the oxygen content of the graphite oxide is 20-30% by weight and the carbon content is 70-80% by weight. The obtained graphite oxide has a moderate oxygen content and is easy to be separated during the reaction process of the improved Hummer method. The method is suitable for graphite oxide with smaller graphite flake size.
[0036] In a specific embodiment of the present invention, the reaction process of the improved Hummer method is as follows: graphite and 98% concentrated sulfuric acid are added to a beaker placed in an ice water bath (<5°C) and stirred to mix evenly, then potassium permanganate is slowly added in batches under stirring, and after the addition of potassium permanganate, the mixture is stirred and reacted in a warm water bath at 40°C for 0.5h, and then an appropriate amount of deionized water is added and the temperature of the water bath is raised to 90-98°C for reaction; the beaker is removed from the water bath and deionized water of about 60°C is added, stirring is continued to reduce the temperature to below 30°C, and the graphite oxide solid is filtered and separated to obtain a graphite oxide filtration stock solution; the dosage ratio of the above reactants is graphite: concentrated sulfuric acid: potassium permanganate: water = 1g: 20-50ml: 3-6g: 50-1000ml.
[0037] In a specific embodiment of the present invention, in the mixture of the filtered stock solution, the manganese content calculated as divalent manganese ions is 2 to 30 g / L, preferably 8 to 20 g / L, the potassium content calculated as potassium ions is 1 to 20 g / L, preferably 2 to 15 g / L, the sulfur content calculated as sulfate ions is 10 to 150 g / L, preferably 30 to 100 g / L, and the carbon content calculated as carbon atoms is 0.5 to 10 g / L, preferably 1 to 6 g / L.
[0038] In a further preferred embodiment, the mixture of the filtered stock solution is an aqueous solution, mainly containing elements such as manganese, potassium, sulfur, and carbon, wherein the manganese content calculated as divalent manganese ions is 13 g / L, the potassium content calculated as potassium ions is 8 g / L, the sulfur content calculated as sulfate ions is 72 g / L, and the carbon content calculated as carbon atoms is 1.4 g / L (the main source of carbon is the soluble graphite oxide remaining in the stock solution).
[0039] In a specific embodiment of the present invention, step S2 includes:
[0040] (1) mixing a copper source with the mixture of the filtered stock solution and optionally water to obtain a mixed solution;
[0041] (2) subjecting the mixed solution to hydrothermal treatment, taking out a solid product, washing, drying and optionally calcining the solid product to obtain the copper-manganese composite adsorption material.
[0042] In a specific embodiment of the present invention, the valence state of the copper element in the copper source is monovalent or divalent, preferably divalent;
[0043] The copper source is one or more of an inorganic salt of copper, an oxide of copper or an organic copper-containing compound. Preferably, the inorganic salt of copper includes one or more of copper sulfate, copper chloride, copper nitrate, copper phosphate, basic copper carbonate, basic copper sulfate, copper carbonate and copper hydroxide; the copper oxide includes one or more of copper oxide and cuprous oxide; the organic copper-containing compound includes one or more of copper acetate, copper formate, fatty acid copper, copper succinate, dibasic acid copper, copper soap solution, amine acid copper, quinoline copper, thiophanate copper and rosinate copper.
[0044] In a specific embodiment of the present invention, the conditions of the hydrothermal treatment include: a temperature of 100 to 200° C., preferably 140 to 180° C., for 1 to 72 hours, preferably 3 to 24 hours, under autogenous pressure;
[0045] The calcination conditions include: temperature of 300-600° C., preferably 350-500° C., time of 1-12 h, preferably 2-6 h, pressure of 0.1-0.5 Mpa, preferably 0.1-0.3 Mpa, and calcination atmosphere of nitrogen or air, preferably air.
[0046] The third aspect of the present invention provides a method for purifying hydrogen, which comprises: contacting hydrogen raw gas with the copper-manganese composite adsorption material provided by the second aspect of the present invention at a temperature of 20 to 50° C. to carry out a purification reaction.
[0047] In a specific embodiment of the present invention, the reaction conditions of the hydrogen purification method include: temperature of 20-50°C, preferably 30-40°C, pressure of 0.1-5.0 MPa, preferably 1-3 MPa, space velocity of 500-500000 h -1 , preferably 2000~100000h -1 ;
[0048] The mass content of sulfide in the hydrogen raw gas is less than 1000 ppm, and the content of sulfide in the hydrogen raw gas is calculated as hydrogen sulfide.
[0049] The present invention is further described below by way of examples, but the present invention is not limited thereto.
[0050] The reagents used in the present invention are all commercially available analytically pure reagents.
[0051] Example 1
[0052] a. Add 5 g of copper sulfate, graphite oxide filter stock solution and 50 g of water into a beaker and mix to obtain a mixed solution, wherein the molar ratio of manganese element in the graphite oxide filter stock solution to copper element in the copper sulfate is 100:6.1, the manganese element content in the graphite oxide filter stock solution is 13 g / L in terms of divalent manganese ions, the potassium element content in terms of potassium ions is 8 g / L, the sulfur element content in terms of sulfate ions is 72 g / L, and the carbon element content in terms of carbon atoms is 1.4 g / L;
[0053] b. subjecting the mixed solution obtained in step a to hydrothermal crystallization treatment at 140° C. under autogenous pressure for 12 h;
[0054] c. Separate the hydrothermal crystallized material into solid and liquid and dry the solid at 80°C for 6h;
[0055] d. Calcinate the dried solid at 300°C for 4 h.
[0056] Example 2
[0057] The preparation method in Example 1 is adopted, except that in step a, the molar ratio of manganese element in the graphite oxide filtration stock solution to copper element in copper sulfate is 100:19.6.
[0058] Example 3
[0059] The preparation method in Example 1 was adopted, except that in step d, the calcination temperature was 800° C. and the calcination time was 1 h.
[0060] Example 4
[0061] The preparation method in Example 1 is adopted, except that in step d, no calcination is performed.
[0062] Example 5
[0063] The preparation method in Example 1 was adopted, except that in step d, the hydrothermal treatment temperature was 190°C.
[0064] Example 6
[0065] The preparation method in Example 1 is adopted, except that, in step a, the manganese content in the graphite oxide filtration stock solution is 23 g / L in terms of divalent manganese ions, the potassium content in terms of potassium ions is 16 g / L, the sulfur content in terms of sulfate ions is 112 g / L, and the carbon content in terms of carbon atoms is 6.4 g / L; wherein the molar ratio of manganese in the graphite oxide filtration stock solution to copper in copper sulfate is consistent with that in Example 1.
[0066] Comparative Example 1
[0067] The preparation method in Example 1 was used, except that in step a, an equal amount of an aqueous solution of manganese sulfate with the same concentration was used to replace the graphite oxide filtration stock solution.
[0068] Comparative Example 2
[0069] The preparation method in Example 1 was used, except that in step a, manganese sulfate was used instead of copper sulfate, so that the molar ratio of manganese element in the graphite oxide filtration stock solution to manganese element in the added manganese sulfate was 100:6.1.
[0070] Comparative Example 3
[0071] The preparation method in Example 1 is adopted, except that in step a, the molar ratio of manganese element in the graphite oxide filtration stock solution to copper element in the copper source is 100:50.
[0072] Test Case
[0073] The copper-manganese composite adsorption materials, copper sulfate and manganese sulfate of Examples 1 to 6 and Comparative Examples 1 to 3 were tested in the following manner:
[0074] The element content of the sample was determined by XPS on a VGESCA-LABS X-ray photoelectron spectrometer, using Mg Kα X-rays as the laser source and the C1s binding energy (284.6 eV) of the surface contamination carbon to calibrate the binding energy of each element in the desulfurizer surface species.
[0075] The average particle size of the prepared product was measured by scanning electron microscopy (ISI-60A electron microscope, ISI Corporation, USA, accelerating voltage 20 kV), and random sampling was performed for particle size statistics.
[0076] The warm nitrogen adsorption-desorption test (BET) was carried out on a JW-BK200C surface area and pore size analyzer produced by Beijing Jingwei Gaobo Co., Ltd. The surface area and pore volume were calculated using the two-parameter BET equation, and the pore distribution and most probable pore size were calculated and counted using the BJH method.
[0077] The sulfide content in the hydrogen after adsorption by the adsorbent was analyzed by online chromatography (Nexis-2030, Shimadzu Corporation, Japan) and SCD fluorescence detector (SCD-2030).
[0078] 250 mg of the examples and comparative examples prepared by the present invention and copper sulfate as adsorbents were loaded into the constant temperature section of the reactor of a fixed bed micro reactor with an inner diameter of 12 mm and a length of 500 mm after passivation, and quartz sand was filled up and down. The hydrogen sulfide content in the hydrogen raw material standard gas was 1000 ppm, and the hydrogen raw material standard gas was introduced at a flow rate of 200 ml / min at 40°C and 2.1 MPa for purification reaction. The hydrogen sulfide content in the purified hydrogen was analyzed online, and the time from the introduction of hydrogen to the time when the hydrogen sulfide content in the purified hydrogen exceeded 0.004 ppm was counted as the penetration time. The penetration time test results of each sample are shown in Table 1, and other characterization results of the prepared product are shown in Table 2.
[0079] Table 1
[0080] Breakthrough time / min Example 1 183 Example 2 112 Example 3 154 Example 4 135 Example 5 97 Example 6 108 Comparative Example 1 34 Comparative Example 2 21 Comparative Example 3 45 Copper sulfate 8 Manganese sulfate 13
[0081] Table 2
[0082]
[0083]
[0084] According to the test results in Table 1 and Table 2, it can be seen that the copper-manganese composite adsorption material prepared by the preparation method provided by the present method has a larger specific surface area and pore volume than the material prepared in the comparative example, a longer hydrogen feed gas penetration time, a better adsorption effect, and exhibits more excellent performance in the hydrogen purification reaction. The sulfide content in the purified hydrogen can meet the content requirements of sulfide impurities in hydrogen for fuel cells, and the manganese element in the mixture of the filtered stock solution of graphite oxide is fully utilized, without the need to add an additional manganese source, thereby reducing the preparation cost of the material.
[0085] It can be seen from the test results of Examples 1 to 6 that when the method for preparing the filtered stock solution of graphite oxide, the molar ratio of manganese in the mixture of the copper source and the filtered stock solution, the element content in the filtered stock solution of graphite oxide, the hydrothermal crystallization treatment conditions, and the roasting conditions are within the specified range of the present invention, the effect and performance of the product prepared by the present invention can be further improved.
[0086] In Comparative Example 1, manganese sulfate is used instead of graphite oxide to filter the stock solution, and the element type of the prepared material is single, the specific surface area, pore volume and most probable pore size are significantly reduced, the penetration time is short, and the adsorption effect of sulfides in the hydrogen raw gas is poor; in Comparative Example 2, manganese sulfate is used instead of copper sulfate, and the prepared product does not contain copper element, the specific surface area, pore volume and most probable pore size are significantly reduced, and the penetration time is short; in Comparative Example 3, the molar ratio of manganese element in the graphite oxide filtration stock solution to copper element in the copper source is not within the scope of the claims of the present invention, resulting in a reduction in the specific surface area and pore volume of the prepared material, and the penetration time and the purification effect on the hydrogen raw gas are worse than those in Example 1.
[0087] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0088] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0089] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A copper-manganese composite adsorption material, wherein: The copper-manganese composite adsorption material comprises copper, manganese, sulfur, potassium and oxygen. Based on the mass of the copper-manganese composite adsorption material, the copper content is 1-15% by weight, the manganese content is 20-60% by weight, the sulfur content is 1-10% by weight, and the potassium content is 2-15% by weight.
2. The copper-manganese composite adsorption material according to claim 1, wherein: The copper-manganese composite adsorption material is a black powder with an average particle size of less than 0.28 mm, preferably less than 0.1 mm, and a specific surface area of 180 to 400 m 2 / g, preferably 200 to 300 m 2 / g, the pore volume is 0.3-1.0 ml / g, preferably 0.5-0.8 ml / g, and the most probable pore diameter is 15-50 nm, preferably 20-40 nm.
3. A method for preparing a copper-manganese composite adsorption material and graphite oxide, the method comprising: S1 uses an improved Hummer method to prepare graphite oxide, and the obtained material is subjected to solid-liquid separation, the obtained liquid phase is a mixture of the filtered stock solution, and the obtained solid phase is graphite oxide after drying; S2: hydrothermally treating the mixture of the copper source and the filtered stock solution and recovering the solid phase material to obtain a copper-manganese composite adsorption material; Wherein, no nitrate and hydrogen peroxide are added during the reaction process of the improved Hummer method; The molar ratio of manganese element in the mixture of the copper source and the filtered stock solution is (1-20):
100.
4. The method according to claim 3, wherein: The graphite oxide has an oxygen content of 20 to 30% by weight and a carbon content of 70 to 80% by weight.
5. The method according to claim 3, wherein: The molar ratio of manganese element in the mixture of the copper source and the filtered stock solution is (2-10):100; Among them, in the mixture of the filtered raw liquid, the manganese content calculated as divalent manganese ions is 2-30 g / L, the potassium content calculated as potassium ions is 1-20 g / L, the sulfur content calculated as sulfate ions is 10-150 g / L, and the carbon content calculated as carbon atoms is 0.5-10 g / L.
6. The method according to claim 3, wherein: Step S2 includes: (1) mixing a copper source with the mixture of the filtered stock solution and optionally water to obtain a mixed solution; (2) subjecting the mixed solution to hydrothermal treatment, taking out a solid product, washing, drying and optionally calcining the solid product to obtain the copper-manganese composite adsorption material.
7. The method according to claim 3, wherein: The valence state of the copper element in the copper source is monovalent or divalent; The copper source is one or more of an inorganic copper salt, a copper oxide or an organic copper-containing compound.
8. The method according to claim 3, wherein: The conditions of the hydrothermal treatment include: a temperature of 100 to 200° C. and a time of 1 to 72 hours under autogenous pressure; The calcination conditions include: temperature of 300-600° C., time of 1-12 hours, pressure of 0.1-0.5 MPa, and calcination atmosphere of nitrogen or air.
9. A method for purifying hydrogen, the method comprising: The hydrogen raw gas is brought into contact with the copper-manganese composite adsorbent material according to any one of claims 1 to 2 at a temperature of 20 to 50° C. to carry out a purification reaction.
10. The method according to claim 9, wherein: The reaction conditions of the hydrogen purification method include: temperature of 20-50°C, pressure of 0.1-5.0 MPa, and space velocity of 500-500000 h -1 ; The mass content of sulfide in the hydrogen raw gas is less than 1000 ppm, and the content of sulfide in the hydrogen raw gas is calculated as hydrogen sulfide.
Citation Information
Patent Citations
Preparation method of nanometer magnetic chitosan / graphene biological adsorption material
CN103394332A
Palygorskite loaded type copper manganese oxide, and preparation method and application thereof
CN107442130A
Hydrogen sulfide removal agent as well as preparation method and application thereof
CN113522302A
Regeneration method of catalyst containing manganese oxide molecular sieve
CN113893872A