O-phthalic anhydride catalyst and preparation method thereof
By using a combination of magnesium oxide support and active components such as vanadium, titanium, and phosphorus, the stability and life problems of existing catalysts under high temperature and high pressure conditions are solved, and the high activity and long life of the catalysts are achieved, which is suitable for industrial production.
Patent Information
- Application Number
- CN202411156106.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing phthalic anhydride catalysts have poor stability under high temperature and high pressure conditions, short service life, low mechanical strength and poor thermal conductivity of the support, which affect the activity and performance of the catalyst.
Using magnesium oxide as a support, combining active components such as vanadium, titanium, phosphorus and cocatalysts such as potassium, tungsten, and tin, the catalyst is prepared by kneading, granulation, drying, and calcining, and the active components are cured by spraying. On the support, the loading and selectivity of the catalyst are improved.
It improves the service life and stability of the catalyst, increases the specific surface area of the magnesium oxide support, reduces the diffusion resistance of the product, improves the selectivity and activity of the catalyst, and is suitable for industrial production.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalyst preparation, in particular to an o-phthalic anhydride catalyst and a preparation method thereof. Background Art
[0002] Phthalic anhydride is an important organic chemical product, widely used in the fields of plastics, paints, dyes, drugs and pesticides. The main production route of phthalic anhydride is to use o-xylene and naphthalene as raw materials, mostly by fixed-bed gas-phase oxidation. In a fixed-bed tubular reactor, o-xylene can be selectively oxidized to produce phthalic anhydride at atmospheric pressure, temperature of 300℃~450℃, and o-xylene concentration of 0.005~0.018mol / L. The production of phthalic anhydride from o-xylene is an oxidation reaction, which is highly exothermic and fast. The key to controlling the reaction rate and making the reaction proceed in the expected direction is the preparation of phthalic anhydride catalyst. In the catalyst preparation process, the internal structural characteristics of the catalyst carrier and the type and content of the auxiliary elements will have a great influence on the performance of the catalyst.
[0003] Catalysts are generally composed of active components and carriers, wherein the active components are mainly vanadium pentoxide and titanium dioxide, and the carriers are mostly any one of talc, silicon carbide, aluminum silicate, quartz and ceramics. In order to improve the activity of the catalyst, existing researchers often add various metals or non-metals to improve the catalytic performance of the catalyst. However, in the face of some harsh reaction conditions, such as high temperature and high pressure, when impurities are mixed in the raw materials, no matter how good the effect of adding metals or non-metals is, the mechanical strength of the carrier is low and the thermal conductivity is poor, thereby causing the activity of the catalyst to decrease and the life span to be shortened. Therefore, how to provide a phthalic anhydride catalyst with high catalytic activity and long service life has become a problem that those skilled in the art need to solve urgently. Summary of the invention
[0004] In view of this, the present invention provides an o-phthalic anhydride catalyst and a preparation method thereof, the purpose of which is to solve the technical problems of poor stability and short service life of the existing phthalic anhydride catalyst.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides an o-phthalic anhydride catalyst, which comprises an active component, a co-catalyst and a magnesium oxide carrier;
[0007] The preparation of the magnesium oxide carrier comprises the following steps:
[0008] The talcum powder, magnesium carbonate and kaolin are mixed to obtain a mixed material, and the mixed material is kneaded, granulated, formed, dried and calcined in sequence to obtain a magnesium oxide carrier.
[0009] Furthermore, the active component includes one or more of a vanadium compound, a titanium compound and a phosphorus compound.
[0010] Furthermore, the active component also includes a cesium compound and / or a rubidium compound.
[0011] Furthermore, the promoter includes one or more of potassium, tungsten, tin, lanthanum, samarium and neodymium.
[0012] Furthermore, the mass ratio of the co-catalyst to the active component is ≤1%; the mass ratio of the active component to the carrier is 10-40%.
[0013] Furthermore, the mass ratio of the talc powder, magnesium carbonate and kaolin is 40-60:30-40:10-20.
[0014] Furthermore, the drying temperature is 80-120° C., and the drying time is 24-48 hours; the calcination temperature is 1400-1800° C., and the calcination time is 3-8 hours.
[0015] The present invention also provides a method for preparing the above-mentioned o-phthalic anhydride catalyst, comprising the following steps:
[0016] The active component, the co-catalyst and the binder are mixed to obtain a mixed slurry, the mixed slurry is sprayed on a magnesium oxide carrier, and the mixed slurry is cured to obtain an o-phthalic anhydride catalyst;
[0017] The viscosity of the mixed slurry is 10-30 Pa·s.
[0018] Furthermore, the amount of the binder used is 5-20% of the solid mass of the active component.
[0019] Furthermore, during spraying, the temperature of the magnesium oxide carrier is 100-120°C.
[0020] It can be seen from the above technical solution that compared with the prior art, the beneficial effects of the present invention are as follows:
[0021] The magnesium oxide carrier used in the present invention has a small pressure drop and a small loss of active components due to abrasion, which can extend the service life of the catalyst. The magnesium oxide carrier has a large specific surface area and a large carrier loading capacity under the same coating thickness, which increases the catalyst load compared with other catalysts, not only making the active component coating thinner, reducing the diffusion resistance of the product, reducing deep oxidation, but also improving the selectivity of the catalyst. DETAILED DESCRIPTION
[0022] The present invention provides an o-phthalic anhydride catalyst, which comprises an active component, a co-catalyst and a magnesium oxide carrier;
[0023] The preparation of the magnesium oxide carrier comprises the following steps:
[0024] The talcum powder, magnesium carbonate and kaolin are mixed to obtain a mixed material, and the mixed material is kneaded, granulated, formed, dried and calcined in sequence to obtain a magnesium oxide carrier.
[0025] In the present invention, the particle sizes of talc, magnesium carbonate and kaolin are all ≤74 μm, preferably ≤72 μm, and more preferably ≤70 μm.
[0026] In the present invention, the active component includes one or more of a vanadium compound, a titanium compound and a phosphorus compound, and the vanadium compound includes one or more of ammonium metavanadate, vanadium pentoxide and sodium vanadate, preferably vanadium pentoxide and / or sodium vanadate, and more preferably vanadium pentoxide;
[0027] The titanium compound includes one or more of titanium dioxide, titanium trichloride and titanium tetrachloride, preferably titanium dioxide and / or titanium trichloride, and more preferably titanium dioxide;
[0028] The phosphorus compound includes one or more of diammonium phosphate, triammonium phosphate and phosphorus pentoxide, preferably triammonium phosphate and / or phosphorus pentoxide, and more preferably phosphorus pentoxide.
[0029] In the present invention, the active component further comprises a cesium compound and / or a rubidium compound, wherein the cesium compound comprises one or more of cesium nitrate, cesium sulfate, cesium chloride and cesium carbonate, preferably one or more of cesium nitrate, cesium sulfate and cesium carbonate, and further preferably cesium sulfate and / or cesium carbonate;
[0030] The rubidium compound includes one or more of rubidium nitrate, rubidium sulfate and rubidium carbonate, preferably rubidium sulfate and / or rubidium carbonate, and more preferably rubidium carbonate.
[0031] In the present invention, the promoter includes one or more of potassium, tungsten, tin, lanthanum, samarium and neodymium, preferably one or more of potassium, tungsten, tin, samarium and neodymium, and more preferably one or more of potassium, samarium and neodymium.
[0032] In the present invention, the mass ratio of the co-catalyst to the active component is ≤1%, preferably ≤0.8%, and more preferably ≤0.5%; the mass ratio of the active component to the carrier is 10-40%, preferably 15-35%, and more preferably 20-30%.
[0033] In the present invention, the mass ratio of talc, magnesium carbonate and kaolin is 40-60:30-40:10-20, preferably 45-55:32-38:12-18, and more preferably 48-52:34-36:14-16.
[0034] In the present invention, magnesium carbonate not only plays the role of flux, but also decomposes into magnesium oxide and carbon dioxide gas at high temperature. Carbon dioxide gas promotes the formation of small pores. Therefore, magnesium carbonate also plays the role of pore-forming agent in the present invention.
[0035] In the present invention, the drying temperature is 80-120°C, preferably 85-115°C, and more preferably 90-110°C; the drying time is 24-48h, preferably 30-42h, and more preferably 33-36h; the calcination temperature is 1400-1800°C, preferably 1450-1700°C, and more preferably 1500-1600°C; the calcination time is 3-8h, preferably 4-7h, and more preferably 5-6h.
[0036] The present invention also provides a method for preparing the above-mentioned o-phthalic anhydride catalyst, comprising the following steps:
[0037] The active component, the co-catalyst and the binder are mixed to obtain a mixed slurry, the mixed slurry is sprayed on a magnesium oxide carrier, and the o-phthalic anhydride catalyst is obtained after curing.
[0038] In the present invention, the viscosity of the mixed slurry is 10 to 30 Pa·s, preferably 15 to 25 Pa·s, and more preferably 20 Pa·s.
[0039] In the present invention, the adhesive comprises acrylic acid and maleic acid, and the mass ratio of acrylic acid to maleic acid is 3:1.
[0040] In the present invention, the amount of the binder is 5 to 20% of the solid mass of the active component, preferably 8 to 16%, and more preferably 10 to 15%.
[0041] In the present invention, during spraying, the temperature of the magnesium oxide support is 100 to 120°C, preferably 105 to 115°C, and more preferably 110°C.
[0042] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0043] Example 1
[0044] The talcum powder is crushed and passed through a 200-mesh sieve, and the magnesium carbonate and kaolin are also passed through a 200-mesh sieve; 50 parts of talcum powder, 40 parts of magnesium carbonate and 10 parts of kaolin are taken by weight and mixed evenly to obtain a mixed material; then the mixed material is put into a kneading machine for kneading and granulation, and then put into a mold and pressed into a ring shape with a size of 7×7×4mm; the ring-shaped semi-finished product is dried at 100°C for 36h, and then put into a calcining furnace and calcined at 1450°C for 7h to obtain a magnesium oxide carrier.
[0045] Mix 60g of titanium dioxide, 60g of vanadium pentoxide, 60g of phosphorus pentoxide, 30g of cesium nitrate and 30g of rubidium nitrate, then add 1g of potassium and 1g of neodymium, and finally add 10% of a binder (acrylic acid and maleic acid in a mass ratio of 3:1), stir well, and put into a colloid grinder to grind into a suspension emulsion, and control the viscosity of the suspension emulsion to 18Pa·s.
[0046] The suspension emulsion was loaded into the spraying equipment, and then 1000g of magnesium oxide carrier was put into the drum. The rotation speed was controlled to 5rpm, and hot air was started to preheat the magnesium oxide carrier. When the carrier temperature reached 100°C, spraying was started. The suspension emulsion was sprayed onto the surface of the magnesium oxide carrier, and it was quickly dried and solidified by hot air. The tail gas was discharged after dust removal. After the suspension emulsion was sprayed, the o-phthalic anhydride catalyst was obtained, which was recorded as catalyst A.
[0047] Example 2
[0048] The talcum powder is crushed and passed through a 200-mesh sieve, and the magnesium carbonate and kaolin are also passed through a 200-mesh sieve; 60 parts of talcum powder, 30 parts of magnesium carbonate and 10 parts of kaolin are taken by weight and mixed evenly to obtain a mixed material; then the mixed material is put into a kneading machine for kneading and granulation, and then put into a mold and pressed into a ring shape with a size of 7×7×4mm; the ring-shaped semi-finished product is dried at 110°C for 30h, and then put into a calcining furnace and calcined at 1500°C for 6.5h to obtain a magnesium oxide carrier.
[0049] 70g of titanium trichloride, 80g of sodium vanadate, 60g of triammonium phosphate, 40g of cesium carbonate and 50g of rubidium carbonate were mixed, and then 1g of potassium, 1g of neodymium and 1g of tungsten were added, and finally 15% of a binder (acrylic acid and maleic acid in a mass ratio of 3:1) was added, stirred thoroughly, and put into a colloid grinder for grinding to form a suspension emulsion, and the viscosity of the suspension emulsion was controlled to be 20Pa·s.
[0050] The suspended emulsion was loaded into the spraying equipment, and then 1000g of magnesium oxide carrier was put into the drum. The rotation speed was controlled to 5rpm, and hot air was started to preheat the magnesium oxide carrier. When the carrier temperature reached 100°C, spraying was started. The suspended emulsion was sprayed onto the surface of the magnesium oxide carrier, and the hot air was quickly dried and solidified. The tail gas was discharged after dust removal. After the spraying of the suspended emulsion was completed, the o-phthalic anhydride catalyst was obtained, which was recorded as catalyst B.
[0051] Example 3
[0052] The talcum powder is crushed and passed through a 200-mesh sieve, and the magnesium carbonate and kaolin are also passed through a 200-mesh sieve; 40 parts of talcum powder, 40 parts of magnesium carbonate and 20 parts of kaolin are taken by weight and mixed evenly to obtain a mixed material; then the mixture is put into a kneading machine for kneading and granulation, and then put into a mold and pressed into a ring shape with a size of 7×7×4mm; the ring-shaped semi-finished product is dried at 120°C for 24h, and then put into a calcining furnace and calcined at 1550°C for 6h to obtain a magnesium oxide carrier.
[0053] 80g of titanium tetrachloride, 60g of ammonium metavanadate, 100g of ammonium dihydrogen phosphate, 70g of cesium sulfate and 90g of rubidium carbonate were mixed, and then 1g of tin, 1g of neodymium and 1g of lanthanum were added, and finally 20% of a binder (acrylic acid and maleic acid in a mass ratio of 3:1) was added and fully stirred, and then put into a colloid grinder and ground to form a suspension emulsion, and the viscosity of the suspension emulsion was controlled to be 25Pa·s.
[0054] The suspension emulsion was loaded into the spraying equipment, and then 1000g of magnesium oxide carrier was put into the drum. The rotation speed was controlled to 5rpm, and hot air was started to preheat the magnesium oxide carrier. When the carrier temperature reached 105°C, spraying was started. The suspension emulsion was sprayed onto the surface of the magnesium oxide carrier, and the hot air was quickly dried and solidified. The tail gas was discharged after dust removal. After the suspension emulsion was sprayed, the o-phthalic anhydride catalyst was obtained, which was recorded as catalyst C.
[0055] Example 4
[0056] The talcum powder is crushed and passed through a 200-mesh sieve, and the magnesium carbonate and kaolin are also passed through a 200-mesh sieve; 45 parts of talcum powder, 40 parts of magnesium carbonate and 15 parts of kaolin are taken by weight and mixed evenly to obtain a mixed material; then the mixture is put into a kneading machine for kneading and granulation, and then put into a mold and pressed into a ring shape with a size of 7×7×4mm; the ring-shaped semi-finished product is dried at 90°C for 40h, and then put into a calcining furnace and calcined at 1650°C for 5h to obtain a magnesium oxide carrier.
[0057] 100g of titanium dioxide, 100g of vanadium pentoxide, 40g of ammonium dihydrogen phosphate, 10g of cesium carbonate and 30g of rubidium carbonate were mixed, and then 1g of samarium, 1g of neodymium and 1g of tungsten were added, and finally 20% of a binder (acrylic acid and maleic acid in a mass ratio of 3:1) was added and fully stirred, and then put into a colloid grinder and ground to form a suspension emulsion, and the viscosity of the suspension emulsion was controlled to be 30Pa·s.
[0058] The suspension emulsion was loaded into the spraying equipment, and then 1000 g of the magnesium oxide carrier was placed in the drum. The rotation speed was controlled to 5 rpm, and hot air was started to preheat the magnesium oxide carrier. When the carrier temperature reached 105°C, spraying was started, and the suspension emulsion was sprayed onto the surface of the magnesium oxide carrier. After hot air rapid drying and solidification, the tail gas was discharged after dust removal. After the suspension emulsion was sprayed, the o-phthalic anhydride catalyst was obtained, which was recorded as catalyst D.
[0059] Comparative Example 1
[0060] The same as Example 1, except that the carrier is silicon carbide, denoted as Catalyst E.
[0061] Comparative Example 2
[0062] The same as Example 1, except that the carrier is alumina, denoted as Catalyst F.
[0063] Comparative Example 3
[0064] The same as Example 3, except that the carrier is alumina, denoted as Catalyst G.
[0065] Catalyst evaluation
[0066] The catalyst performance was evaluated by using a single tube reactor simulating industrial production conditions. The fixed bed single tube reactor had an inner diameter of 28 mm and a tube length of 4000 mm. The outside of the reaction tube used a molten salt circulation heat transfer method, and there was a multi-point temperature measurement system inside the reaction tube. The phthalic anhydride catalyst was loaded in multiple stages. Catalyst A was evaluated with a loading height of 1400 mm, a loading height of 800 mm for catalyst B, a loading height of 700 mm for catalyst C, and a loading height of 500 mm for catalyst D. The reactor outlet was connected to the analysis system and the reactant collection system.
[0067] Catalyst B was evaluated, and the filling height of catalyst B was 1400 mm, the filling height of catalyst A was 800 mm, the filling height of catalyst C was 700 mm, and the filling height of catalyst D was 500 mm.
[0068] Catalyst C was evaluated, and the filling height of catalyst C was 1400 mm, the filling height of catalyst B was 800 mm, the filling height of catalyst A was 700 mm, and the filling height of catalyst D was 500 mm.
[0069] Catalyst D was evaluated, and the filling height of catalyst D was 1400 mm, the filling height of catalyst B was 800 mm, the filling height of catalyst C was 700 mm, and the filling height of catalyst A was 500 mm.
[0070] The evaluation of catalysts E, F, and G was carried out in the same manner as that of catalyst A.
[0071] The catalyst was activated in an oxidizing atmosphere for 12 hours. After adding the materials, the salt bath temperature was controlled between 300 and 450 °C and the air velocity was 3000 h -1 The o-xylene feed concentration was gradually increased, and sampling and analysis of various conditions were performed at the reactor outlet to assess performance indicators such as the maximum catalyst load and optimal yield. The evaluation results of each catalyst evaluation experiment are shown in Table 1 below.
[0072] Table 1 Evaluation results of catalyst evaluation experiment
[0073] type Molten salt temperature / ℃ Hot spot temperature / ℃ Phthalic anhydride yield / % Phthalic anhydride purity / % Catalyst A 353 455 118.6 99.88 Catalyst B 352 453 118.5 99.82 Catalyst C 355 458 119.4 99.90 Catalyst D 351 451 118.2 99.83 Catalyst E 347 432 117.5 99.41 Catalyst F 346 440 117.6 99.32 Catalyst G 342 439 117.1 99.26
[0074] As can be seen from Table 1, the molten salt temperature of the phthalic anhydride catalyst prepared by the present invention is relatively high, indicating that the catalyst has good stability; the hot spot temperature is also relatively high, indicating that the catalyst has good activity; and the yield and purity of phthalic anhydride are also relatively high, which is suitable for industrial production.
[0075] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. An o-phthalic anhydride catalyst, characterized in that: The o-phthalic anhydride catalyst comprises an active component, a co-catalyst and a magnesium oxide carrier; The preparation of the magnesium oxide carrier comprises the following steps: The talcum powder, magnesium carbonate and kaolin are mixed to obtain a mixed material, and the mixed material is kneaded, granulated, formed, dried and calcined in sequence to obtain a magnesium oxide carrier.
2. The o-phthalic anhydride catalyst according to claim 1, wherein The active component includes one or more of a vanadium compound, a titanium compound and a phosphorus compound.
3. The o-phthalic anhydride catalyst according to claim 2, wherein The active component also includes a cesium compound and / or a rubidium compound.
4. The o-phthalic anhydride catalyst according to any one of claims 1 to 3, characterized in that The promoter includes one or more of potassium, tungsten, tin, lanthanum, samarium and neodymium.
5. The o-phthalic anhydride catalyst according to claim 4, characterized in that The mass ratio of the co-catalyst to the active component is ≤1%; the mass ratio of the active component to the carrier is 10-40%.
6. The o-phthalic anhydride catalyst according to claim 1, 2, 3 or 5, characterized in that The mass ratio of the talc powder, magnesium carbonate and kaolin is 40-60:30-40:10-20.
7. The o-phthalic anhydride catalyst according to claim 6, characterized in that The drying temperature is 80-120° C., and the drying time is 24-48 hours; the calcination temperature is 1400-1800° C., and the calcination time is 3-8 hours.
8. The method for preparing the o-phthalic anhydride catalyst according to any one of claims 1 to 7, characterized in that: The following steps are involved: The active component, the co-catalyst and the binder are mixed to obtain a mixed slurry, the mixed slurry is sprayed on a magnesium oxide carrier, and the mixed slurry is cured to obtain an o-phthalic anhydride catalyst; The viscosity of the mixed slurry is 10-30 Pa·s.
9. The preparation method according to claim 8, characterized in that: The amount of the binder used is 5-20% of the solid mass of the active component.
10. The preparation method according to claim 9, characterized in that: During spraying, the temperature of the magnesium oxide carrier is 100-120°C.