Efficient beneficiation method for high-silicon gangue type low-grade zinc oxide ore
Through the combination of fatty acid collectors and amine + yellow medicine vulcanization processes, the development and utilization problems of high-silica gangue low-grade zinc oxide ore are solved, and efficient recycling of high-grade zinc oxide concentrate is achieved, reducing production costs and SiO2 impurities The content increases the utilization rate of zinc ore.
Patent Information
- Application Number
- CN202410960134.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-07-17
AI Technical Summary
The existing technology is difficult to efficiently develop and utilize high-silica gangue-type low-grade zinc oxide ore. The traditional acid leaching process is costly and has low selectivity. The flotation of amine sulfide method has problems such as low concentrate grade and high SiO2 impurity content.
Adopt fatty acid collectors to preferentially desilicate carbonate + carbonate concentrate amine + yellow drug sulfide zinc selection combination process, and achieve high efficiency of zinc oxide through carbonate positive flotation and amine + yellow drug sulfide processes. Recycle, reduce SiO2 impurity content and improve zinc concentrate grade.
High-grade zinc oxide concentrate was obtained, which reduced production costs, improved the utilization rate of gangue-type low-grade zinc oxide ore, reduced leaching of soluble silicon, and improved the filtration of leaching liquid.
Smart Images

Figure CN119034951A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of zinc oxide ore dressing, and in particular to a high-efficiency dressing method for high-silicon gangue type low-grade zinc oxide ore. Background Art
[0002] According to statistics from relevant departments in 2008, my country's zinc resources amounted to 103.93 million tons, ranking second in the world, of which zinc oxide resources accounted for more than 40 million tons. Yunnan Province has zinc resources of 20.289 million tons, accounting for 23% of the country's zinc resources, ranking first in the country, of which oxide ores accounted for 41.8%, and most of them were low-grade ores. In addition, my country's northwest region also has a large amount of low-grade zinc oxide resources. In general, my country's zinc oxide resources are of low grade, with an average grade of less than 5%, and the resources are large, but they have not been efficiently developed and utilized due to the limitations of the existing technology level. Especially in the development and utilization of high-silicon gangue-type low-grade zinc oxide ores with SiO2 content greater than 70%, zinc content 2-6%, lead content less than 0.5%, and zinc oxidation rate greater than 80%, due to their low grade, the traditional acid leaching process is not applicable due to high production costs. At the same time, due to the low selectivity of the acid leaching process, a large amount of soluble silicon in the ore will be leached out, and the generated colloidal silicon is difficult to filter, resulting in difficulty in continuing the production process; the traditional sulfide amine flotation process is limited by the poor selectivity of amine collectors, and often has problems such as low concentrate grade and high SiO2 impurity content.
[0003] To solve the above or similar problems, Chinese patent CN202111067879.8 discloses "a collector and flotation method for flotation of quartzite-type zinc oxide ore smithsonite", which is obviously aimed at a newly developed quartzite zinc oxide ore collector; Chinese patent CN201811195420.4 discloses "a flotation method for dolomite and calcite-type sulfide oxide lead-zinc ore", which is aimed at mixed lead-zinc ore. This method has both a sulfide lead-zinc ore flotation method. There is also a flotation method for lead-zinc oxide ores. Dodecylamine and butyl xanthate collectors are used in the flotation of zinc oxide. The reason is that the gangue minerals are dolomite and calcite, the inhibitors used are different from the quartz gangue type, and the addition ratio of dodecylamine and butyl xanthate is different; Chinese patent CN202210395531.X discloses "a flotation recovery method for high calcium and magnesium high mud zinc carbonate", which is aimed at another type of high calcium and magnesium high mud zinc oxide ore. The gangue minerals are mainly dolomite and calcite, the grinding is easy to muddy, and there is too much ore mud It will deteriorate flotation. Therefore, there is a desludging process in the ore dressing process. The ore dressing process is different. Although dodecylamine and butyl xanthate are also used as collectors, the gangue minerals are dolomite and calcite, and the inhibitors used are different from the quartz gangue type. This method has both sulfide lead-zinc ore flotation method and oxide lead-zinc ore flotation method. Dodecylamine and butyl xanthate are used as collectors in the flotation of zinc oxide, but the gangue minerals are dolomite and calcite, and the inhibitors used are different from the quartz gangue type, and the addition ratio of dodecylamine and butyl xanthate is different.
[0004] Therefore, it is of great significance to develop a low-cost, environmentally friendly and efficient beneficiation method for high-silicon gangue type low-grade zinc oxide ore. Summary of the invention
[0005] The task of the present invention is to overcome the shortcomings of the prior art and propose an efficient beneficiation method for high-silicon gangue type low-grade zinc oxide ore, which can not only obtain higher-grade zinc oxide concentrate, but also reduce production costs and improve the utilization rate of silicon gangue type low-grade zinc oxide ore.
[0006] The method for the efficient beneficiation of high-silicon gangue type low-grade zinc oxide ore is aimed at the problems of high SiO2 content in the ore and zinc mainly occurring in smithsonite. The combined process of preferential desiliconization flotation of carbonate + carbonate concentrate amine + xanthate sulfidation zinc selection using fatty acid collector is used to obtain zinc oxide concentrate with low SiO2 impurity content, and the efficient recovery of high-silicon gangue type low-grade zinc oxide ore is realized. The method specifically includes the following steps and conditions:
[0007] (1) One-stage grinding, with a grinding fineness of -0.074 mm accounting for 40-60%, using sulfuric acid for slurry preparation, using fatty acid collectors for carbonate roughing, adding inhibitors to roughing foam for three rounds of fine cleaning, obtaining a carbonate concentrate with preliminary enrichment of smithsonite, and the degree of dissociation of smithsonite in the ore reaching more than 85%;
[0008] (2) Add inhibitors to carbonate concentrate and use amine + xanthate sulfidation process to carry out zinc oxide roughing. Add inhibitors to roughing foam and carry out four rounds of fine separation to obtain zinc oxide concentrate. Add amine + xanthate combined collector to roughing tailings for scavenging. The fine ore and scavenged concentrate are returned in sequence.
[0009] The innovative features of the present invention are as follows: carbonate positive flotation is used to remove a large amount of SiO2, so that smithsonite is initially enriched in the carbonate concentrate, which can effectively improve the inhibitory effect of the subsequent carbonate concentrate and then zinc selection by amine + xanthate sulfidation process on SiO2, and obtain a higher-grade zinc oxide concentrate; reducing the SiO2 impurity content in the concentrate is beneficial to the subsequent wet zinc extraction process, which will greatly reduce the leaching of soluble silicon, can improve the filterability of the leachate, reduce the cost and enable the efficient development and utilization of low-grade zinc oxide ores.
[0010] In summary, compared with the prior art, the present invention has the following advantages or effects:
[0011] Because of the characteristics of the ore, carbonates are given priority to remove a large amount of SiO2, so the inhibition of SiO2 by the carbonate concentrate amine + xanthate sulfidation process for zinc selection is greatly improved, and a higher-grade zinc oxide concentrate is obtained; at the same time, the obtained zinc oxide concentrate with low SiO2 impurity content is beneficial to the subsequent wet zinc extraction process, so the leaching of soluble silicon is greatly reduced and the filterability of the leachate is improved; in addition, due to the simple process, the production cost is low and the utilization rate of high-silicon gangue-type low-grade zinc oxide ore is greatly improved.
[0012] The % mentioned in the application documents refers to mass percentage. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 The present invention provides a schematic diagram of a process flow of a high-efficiency beneficiation method for high-silicon gangue type low-grade zinc oxide ore.
[0014] The present invention is further described in detail below in conjunction with the accompanying drawings. DETAILED DESCRIPTION
[0015] like Figure 1 As shown, in order to solve the problems of high SiO2 content in the ore and zinc mainly occurring in smithsonite, a combined process of preferential desiliconization flotation of carbonate + carbonate concentrate amine + xanthate sulfidation zinc selection using fatty acid collectors is used to obtain zinc oxide concentrate with low SiO2 impurity content, and to achieve efficient recovery of high-silicon gangue type low-grade zinc oxide ore, which specifically includes the following steps and conditions:
[0016] (1) One-stage grinding, with a grinding fineness of -0.074 mm accounting for 40-60%, using sulfuric acid for slurry preparation, using fatty acid collectors for carbonate roughing, adding inhibitors to roughing foam for three rounds of fine cleaning, obtaining a carbonate concentrate with preliminary enrichment of smithsonite, and the degree of dissociation of smithsonite in the ore reaching more than 85%;
[0017] (2) Add inhibitors to carbonate concentrate and use amine + xanthate sulfidation process to carry out zinc oxide roughing. Add inhibitors to roughing foam and carry out four rounds of fine separation to obtain zinc oxide concentrate. Add amine + xanthate combined collector to roughing tailings for scavenging. The fine ore and scavenged concentrate are returned in sequence.
[0018] The process of the present invention may further be:
[0019] In the step (1), a fatty acid collector is added to the roughing tailings for scavenging.
[0020] In the step (1), the selected middlings and scavenged concentrates are sequentially returned for reselection.
[0021] In the step (2), the roughing tailings are added with an amine + xanthate combined collector for scavenging.
[0022] In the step (2), the selected middlings and scavenged concentrates are sequentially returned for reselection.
[0023] In the step (1), sulfuric acid is used to adjust the pH value of the slurry, and the pH value of the slurry is controlled at 5.5 to 6.5.
[0024] The carbonate roughing and scavenging collector in step (1) is fatty acid collector PA67, which has good selectivity and collection ability for carbonate minerals under weakly acidic conditions.
[0025] The dosage of carbonate crude fatty acid collector PA67 in the step (1) is 400-800 g / t.
[0026] The dosage of the carbonate scavenging fatty acid collector PA67 in step (1) is 100-150 g / t.
[0027] The carbonate concentration inhibitor in step (1) is water glass with a modulus of 2.5 to 3.0, and the dosage is 100 to 150 g / t, which can inhibit quartz.
[0028] The carbonate zinc reselection inhibitor in step (2) is a combination of carboxymethyl cellulose (CMC) and water glass with a modulus of 2.5 to 3.0, which can further enhance the inhibition of quartz. The amount of CMC used in the rough selection is 40 to 60 g / t, the amount of water glass used is 80 to 120 g / t, the amount of CMC used in the fine selection is 4 to 25 g / t, and the amount of water glass used is 8 to 50 g / t.
[0029] In the step (2), the zinc sulfiding agent for the carbonate concentrate is sodium sulfide, and the dosage is 500-800 g / t.
[0030] The collector for the zinc roughing and scavenging of the carbonate concentrate in step (2) is a fatty acid collector consisting of dodecylamine and butyl xanthate, which has a strong collecting ability for smithsonite.
[0031] In the step (2) of zinc roughing of carbonate concentrate, the amount of dodecylamine used as collector is 5-15 g / t, and the amount of butyl xanthate used is 10-30 g / t.
[0032] In the step (2) of zinc scavenging of carbonate concentrate, the amount of dodecylamine used is 2-5 g / t, and the amount of butyl xanthate used is 4-8 g / t.
[0033] The flotation process of preferentially floating carbonate in step (1) is a "one roughing-three fines-one scavenging" closed-circuit process, and the selected middlings and scavenged concentrates are returned in sequence for reselection.
[0034] The flotation process of carbonate concentrate zinc in step (2) is a "one roughing-four fines-one scavenging" closed-circuit process, and the selected middlings and scavenged concentrates are returned in sequence for reselection.
[0035] Example 1
[0036] The method of the present invention was used to conduct a beneficiation test study on a high-silicon low-grade zinc oxide ore from a zinc oxide mine site 1 in Xinjiang. The element analysis of the raw ore is shown in Table 1.
[0037] Table 1 Element analysis results of the original ore of mine site 1 (%)
[0038]
[0039] *g / t
[0040] From the data in Table 1, it can be seen that the main metal element that can be recovered from the ore is Zn. According to the properties of the original ore, the process of the present invention is adopted. The specific process flow is as follows:
[0041] (1) In the first stage of grinding, sulfuric acid is used for slurry preparation, and a fatty acid collector is used for carbonate roughing. An inhibitor is added to the roughing foam for three rounds of fine separation to obtain a carbonate concentrate. A fatty acid collector is added to the roughing tailings for scavenging, and the fine middlings and scavenged concentrates are returned in sequence.
[0042] (2) Add inhibitors to carbonate concentrate and use amine + xanthate sulfidation process for zinc oxide roughing. Add inhibitors to roughing foam for 4 rounds of cleaning to obtain zinc oxide concentrate; add (amine + xanthate) combined collector to roughing tailings for scavenging, and the selected middlings and scavenged concentrates are returned in sequence.
[0043] As attached Figure 1As shown, the ore is first ground to a grinding fineness of -0.074mm accounting for 54.38%, and then flotation is carried out. Sulfuric acid is added to adjust the pH value of the ore pulp to 6, and fatty acid collector PA67 550g / t is added for roughing; the coarse concentrate is finely selected three times, and inhibitor water glass (modulus 2.7) 140g / t and 120g / t are added to fine selection I and fine selection II respectively, and no inhibitor is added to fine selection III; the roughing tailings are scavenged once, and collector PA67 130g / t is added.
[0044] In the carbonate concentrate reselection step, a combined inhibitor CMC + water glass is added in a roughing process at a dosage of 50 + 100 g / t, sodium sulfide is used as a sulfiding agent at a dosage of 600 g / t, and a combined collector of dodecylamine + butyl xanthate is used at a dosage of 10 + 20 g / t; the rough concentrate is subjected to four rounds of selection, and a combined agent CMC + water glass (modulus 2.7) of 20 + 40 g / t, 10 + 20 g / t, and 5 + 10 g / t are added to selection I, selection II, and selection III, respectively; no inhibitor is added to selection IV; the roughing tailings are subjected to one scavenging process, and a collector of dodecylamine + butyl xanthate is added at 3 + 5 g / t.
[0045] The test results are shown in Table 2. From the test results in Table 2, it can be seen that through the combined process of carbonate selection (one coarse-three fines-one sweep)-carbonate concentrate sulfidation (amine + xanthate) zinc selection (one coarse-four fines-one sweep), a zinc concentrate with a zinc grade of 29.79%, a lead content of 1.66%, and a SiO2 content of 8.88% can be obtained, and the zinc recovery rate is 74.28%.
[0046] Table 2 Experimental results of Example 1 (%)
[0047]
[0048] Example 2
[0049] The method of the present invention was used to conduct a beneficiation test study on a high-silicon low-grade zinc oxide ore from a zinc oxide mine site 2 in Xinjiang. The element analysis of the raw ore is shown in Table 3.
[0050] Table 3 Element analysis results of the original ore of mine site 2 (%)
[0051]
[0052] *g / t
[0053] From the data in Table 1, it can be seen that the main metal element that can be recovered from the ore is Zn. According to the properties of the original ore, the process of the present invention is adopted. The specific process flow is as follows:
[0054] (1) In the first stage of grinding, sulfuric acid is used for slurry preparation, and a fatty acid collector is used for carbonate roughing. An inhibitor is added to the roughing foam for three rounds of fine separation to obtain a carbonate concentrate. A fatty acid collector is added to the roughing tailings for scavenging, and the fine middlings and scavenged concentrates are returned in sequence.
[0055] (2) Add inhibitors to carbonate concentrate and use amine + xanthate sulfidation process for zinc oxide roughing. Add inhibitors to roughing foam for 4 rounds of cleaning to obtain zinc oxide concentrate; add (amine + xanthate) combined collector to roughing tailings for scavenging, and the selected middlings and scavenged concentrates are returned in sequence.
[0056] The ore was first ground to a fineness of -0.074mm, accounting for 49.93%. Then flotation was carried out, sulfuric acid was added to adjust the pH value of the ore pulp to 6, and fatty acid collector PA67 500g / t was added for roughing. The coarse concentrate was finely selected three times, and inhibitor water glass (modulus 2.7) 130g / t and 110g / t were added to fine selection I and fine selection II respectively, and no inhibitor was added to fine selection III. The rough tailings were scavenged once and collector PA67 120g / t was added.
[0057] In the carbonate concentrate reselection step, a combined inhibitor CMC + water glass is added in a roughing process at a dosage of 50 + 100 g / t, sodium sulfide is used as a sulfiding agent at a dosage of 600 g / t, and a combined collector of dodecylamine + butyl xanthate is used at a dosage of 10 + 20 g / t; the rough concentrate is subjected to four rounds of selection, and a combined agent CMC + water glass (modulus 2.7) of 20 + 40 g / t, 10 + 20 g / t, and 5 + 10 g / t are added to selection I, selection II, and selection III, respectively; no inhibitor is added to selection IV; the roughing tailings are subjected to one scavenging process, and a collector of dodecylamine + butyl xanthate is added at 3 + 5 g / t.
[0058] The test results are shown in Table 4. From the test results in Table 4, it can be seen that through the combined process of carbonate selection (one coarse-three fines-one sweep)-carbonate concentrate sulfidation (amine + xanthate) zinc selection (one coarse-four fines-one sweep), a zinc concentrate with a zinc grade of 27.71%, a lead content of 2.41%, and a SiO2 content of 9.83% can be obtained, and the zinc recovery rate is 69.92%.
[0059] Table 4 Experimental results of Example 2 (%)
[0060]
[0061] *g / t
[0062] As described above, the present invention can be better implemented. The above embodiments are only the best implementation methods of the present invention, but the implementation methods of the present invention are not limited by the above embodiments. Other changes, modifications, replacements, combinations, and simplifications made without departing from the spirit and principle of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. High-efficiency beneficiation method for high-silicon gangue type low-grade zinc oxide ore, targeting at SiO 2 The zinc content is high and the zinc is mainly present in smithsonite. Features The combined process of using fatty acid collectors to preferentially desiliconize carbonate flotation + carbonate concentrate amine + xanthate sulfidation zinc selection can obtain low SiO 2 The high-efficiency recovery of high-silicon gangue-type low-grade zinc oxide ore is achieved by using the following steps and conditions: (1) One-stage grinding, with a grinding fineness of -0.074 mm accounting for 40-60%, using sulfuric acid for slurry preparation, using fatty acid collectors for carbonate roughing, adding inhibitors to roughing foam for three rounds of fine cleaning, obtaining a carbonate concentrate with preliminary enrichment of smithsonite, and the degree of dissociation of smithsonite in the ore reaching more than 85%; (2) Add inhibitors to carbonate concentrate and use amine + xanthate sulfidation process to carry out zinc oxide roughing. Add inhibitors to roughing foam and carry out four rounds of fine separation to obtain zinc oxide concentrate. Add amine + xanthate combined collector to roughing tailings for scavenging. The fine ore and scavenged concentrate are returned in sequence.
2. The method according to claim 1, Its characteristics are In the step (1), fatty acid collector is added to the roughing tailings for scavenging.
3. The method according to claim 1 or 2, Its characteristics are In the step (1), the selected middlings and scavenged concentrates are sequentially returned for reselection.
4. The method according to claim 1, Its characteristics are In the step (2), the roughing tailings are added with an amine + xanthate combined collector for scavenging.
5. The method according to claim 1 or 4, Its characteristics are In the step (2), the selected middlings and scavenged concentrates are sequentially returned for reselection.
6. The method according to claim 1, Its characteristics are In the step (1), sulfuric acid is used to adjust the pH value of the slurry, and the pH value of the slurry is controlled at 5.5 to 6.
5.
7. The method according to claim 1, Its characteristics are The carbonate roughing and scavenging collector in step (1) is fatty acid collector PA67, which has good selectivity and collection ability for carbonate minerals under weakly acidic conditions.
8. The method according to claim 1, Its characteristics are The dosage of carbonate crude fatty acid collector PA67 in the step (1) is 400-800 g / t.
9. The method according to claim 1, Its characteristics are The dosage of the carbonate scavenging fatty acid collector PA67 in step (1) is 100-150 g / t.
10. The method according to claim 1, Its characteristics are The carbonate concentration inhibitor in step (1) is water glass with a modulus of 2.5 to 3.0, and the dosage is 100 to 150 g / t, which can inhibit quartz.
11. The method according to claim 1 or 4 or 5, Its characteristics are The carbonate zinc reselection inhibitor in step (2) is a combination of carboxymethyl cellulose (CMC) and water glass with a modulus of 2.5 to 3.0, which can further enhance the inhibition of quartz. The amount of CMC used in the rough selection is 40 to 60 g / t, the amount of water glass used is 80 to 120 g / t, the amount of CMC used in the fine selection is 4 to 25 g / t, and the amount of water glass used is 8 to 50 g / t.
12. The method according to claim 1, Its characteristics are In the step (2), the zinc sulfiding agent for the carbonate concentrate is sodium sulfide, and the dosage is 500-800 g / t.
13. The method according to claim 1, Its characteristics are The collector for the zinc roughing and scavenging of the carbonate concentrate in step (2) is a fatty acid collector consisting of dodecylamine and butyl xanthate, which has a strong collecting ability for smithsonite.
14. The method according to claim 1, Its characteristics are In the step (2) of zinc roughing of carbonate concentrate, the amount of dodecylamine used as collector is 5-15 g / t, and the amount of butyl xanthate used is 10-30 g / t.
15. The method according to claim 1 or 12 or 13 or 14, Its characteristics are In the step (2) of zinc scavenging of carbonate concentrate, the amount of dodecylamine used is 2-5 g / t, and the amount of butyl xanthate used is 4-8 g / t.
16. The method according to claim 1, Its characteristics are The flotation process of the carbonate preferentially floated in step (1) is a "one roughing-three fines-one scavenging" closed-circuit process, and the selected middlings and scavenged concentrates are sequentially returned for reselection.
17. The method according to claim 1, Its characteristics are The flotation process of zinc separation from carbonate concentrate in step (2) is a closed-circuit process of "one roughing-four fines-one scavenging", in which the selected middlings and scavenged concentrates are returned in sequence for re-selection.
Citation Information
Patent Citations
Floating depressing agent for reducing silicon dioxide in zinc ore concentrate
CN101347763A
Zinc oxide mineral collector and use method thereof
CN103752416A
Novel composite collecting agent for recovering zinc oxide from peat slate lead-zinc oxide ore and preparation method and application thereof
CN111530633A
Flotation method of peaty slate lead zinc ore with high oxidation rate
CN113457852A
Flotation recovery method for high-calcium-magnesium high-argillaceous zinc carbonate
CN114798185A
Cited By
Zinc oxide ore flotation method based on combined collecting agent
CN119857592A
Method for improving quality of zinc sulfide concentrate and reducing silicon-containing gangue
CN120550927A