High-vanadium solid solution hydrogen storage alloy and preparation method of fine spherical powder of high-vanadium solid solution hydrogen storage alloy

High-vanadium solid solution hydrogen storage alloy powder was prepared by vacuum magnetic levitation melting and electrode induction melting gas atomization method, which solved the problems of high oxygen content and impurity contamination, and achieved high efficiency in hydrogen storage performance and purity, with a significant increase in maximum hydrogen absorption and release.

CN119035534APending Publication Date: 2024-11-29BEIHANG UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411156726.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing technologies for preparing hydrogen storage alloy powders suffer from problems such as excessive oxygen content, impurity contamination from crucibles and electrodes, and uneven melting, all of which affect hydrogen storage performance.

Method used

High-purity metal raw materials are prepared using vacuum magnetic levitation melting technology, combined with electrode induction melting gas atomization method to produce powder, avoiding contact with the crucible, and the alloy properties are improved by adding rare earth elements.

Benefits of technology

Fine spherical powder with high purity, good sphericity, and uniform composition was prepared, which improved the hydrogen storage and activation performance, with a maximum hydrogen absorption capacity of 3.5 wt% H2 and a maximum hydrogen release capacity of 2.4 wt% H2.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035534A_ABST
    Figure CN119035534A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of powder material preparation, in particular to a high-vanadium solid solution hydrogen storage alloy and a preparation method of fine spherical powder of the high-vanadium solid solution hydrogen storage alloy, and the preparation method comprises the following steps: the chemical formula of the high-vanadium solid solution hydrogen storage alloy is Vx-Tiy-Crz-M (1-x-y-z)-1-3wt% RE, the preparation method comprises the following steps: burdening high-purity metal raw materials according to chemical formula components of the alloy, carrying out vacuum magnetic suspension smelting, casting the high-purity metal raw materials into a cylindrical bar-shaped mold after smelting is completed, and demolding to obtain an initial blank bar; machining the initial blank bar to prepare a high-vanadium solid solution hydrogen storage alloy electrode bar; the high-vanadium solid solution hydrogen storage alloy electrode bar is subjected to gas atomization powder making through an electrode induction melting gas atomization powder making technology, and high-purity fine spherical powder is obtained; carrying out vibration screening and airflow classification on the fine spherical powder under the protection of an argon atmosphere; the prepared alloy is more accurate and uniform in component, and the hydrogen storage performance is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of powder material preparation, and in particular to a preparation method of a high-vanadium solid solution hydrogen storage alloy and a fine spherical powder thereof. Background Art

[0002] The use of hydrogen storage alloys for solid-state hydrogen storage has the advantages of high hydrogen storage density, good safety, moderate hydrogen storage pressure, and high hydrogen release purity, and is considered to be the most promising hydrogen storage method. The hydrogen storage alloys that are currently being studied include rare earth hydrogen storage alloys, titanium hydrogen storage alloys, magnesium-based hydrogen storage alloys, and vanadium-based solid solution hydrogen storage alloys. Among them, the theoretical hydrogen storage capacity of rare earth hydrogen storage alloys and titanium hydrogen storage alloys is relatively low, and the hydrogen storage capacity at room temperature does not exceed 2wt% H2; magnesium-based hydrogen storage alloys are difficult to use in practice due to their excessively high hydrogen release temperature and relatively poor kinetic properties. The theoretical hydrogen storage capacity of vanadium-based solid solution hydrogen storage alloys at room temperature is as high as 3.8wt% H2, and metal V is the only metal element in single metals with an equilibrium pressure of 0.1 to 1MPa near room temperature. The working pressure is mild and has good application prospects.

[0003] At present, the preparation methods of hydrogen storage alloy powders mainly include smelting method, melt spinning method, mechanical alloying method, etc. The hydrogen storage alloy powders prepared by smelting method have problems such as component segregation, foreign impurity contamination, irregular shape, low efficiency and high energy consumption, which are only suitable for basic research in laboratories and are not conducive to the large-scale production of hydrogen storage alloy powders; the hydrogen storage alloy powders prepared by melt spinning method have problems such as easy oxidation and amorphization, and the production cost is also high; the alloy powders prepared by mechanical alloying method are very easy to agglomerate, which leads to a decrease in hydrogen storage capacity.

[0004] The powders prepared by gas atomization have many advantages such as good sphericity, high purity, and strong uniformity of composition. The electrode induction melting gas atomization (EIGA) powder making technology directly uses induction heating to heat and melt metal rods. During the powder making process, the melt flow does not contact refractory materials such as crucibles. As a highly active refractory metal, the melting point of pure V is as high as 1890°C. It is easy to react with oxygen and non-metallic elements in the crucible at high temperatures. Therefore, it is expected that high-purity vanadium-based solid solution hydrogen storage alloy powders can be prepared by EIGA powder making technology. However, since vacuum arc melting technology or vacuum induction melting technology is currently used to prepare the hydrogen storage alloy electrode rods required for EIGA equipment, this will lead to excessively high oxygen content in the rods, and there are problems such as impurity contamination and uneven melting caused by crucibles and electrodes. Summary of the invention

[0005] In view of the above problems, the present invention provides a method for preparing a high-vanadium solid solution hydrogen storage alloy and its fine spherical powder, which solves the technical problems in the prior art of excessively high oxygen content in hydrogen storage alloy rods, impurity contamination caused by crucibles and electrodes, and uneven smelting.

[0006] In one aspect, the present invention provides a high vanadium solid solution hydrogen storage alloy having a chemical formula of V x -Ti y -Cr z -M (1-x-y-z) -1~3wt% RE, wherein x, y, z are the atomic percentages of V, Ti, and Cr respectively, the value range of x is 67~79at%, the value range of y is 2~14at%, the value range of x+y+z is 90~98at%, and M includes a combination of one or more of Fe, Mn, Ni and Co. The rare earth element RE is Ce or Y, and the RE content is 1~3wt% of the weight of the high vanadium solid solution hydrogen storage alloy.

[0007] Preferably, the chemical formula V x -Ti y -Cr z -M (1-x-y-z) -1~3wt% RE, the value range of x+y is 75~85at%.

[0008] In one aspect, the present invention provides a method for preparing a fine spherical powder of a high-vanadium solid solution hydrogen storage alloy, comprising the following steps:

[0009] Step S1, mixing high-purity metal raw materials according to the chemical formula of the alloy, performing vacuum magnetic suspension smelting, casting into a cylindrical rod-shaped mold after smelting, and obtaining an initial blank rod after demoulding;

[0010] Step S2, machining the initial blank rod to produce a high vanadium solid solution hydrogen storage alloy electrode rod;

[0011] Step S3, using electrode induction melting gas atomization powder making technology to gas atomize and powder-make the high vanadium solid solution hydrogen storage alloy electrode rod to obtain high-purity fine spherical powder;

[0012] Step S4: vibrating screen and air flow classify the fine spherical powder under the protection of argon atmosphere.

[0013] Preferably, in step S1, the purity of the high-purity metal raw materials is >99.5%; the vacuum magnetic levitation smelting process is carried out under an argon protection environment; the smelting parameters are: smelting power 100-300kW, smelting time 30-120min, smelting times 3-6 times; the diameter of the cylindrical rod mold is 30-90mm, and the length is 150-300mm.

[0014] Preferably, step S2 specifically includes: using a milling machine and a lathe to perform surface processing and thread processing on the initial blank rod obtained in step S1 to produce a high-vanadium solid solution hydrogen storage alloy electrode rod, and the thread processing length is 20 to 40 mm.

[0015] Preferably, step S3 specifically includes:

[0016] Step S3-1, loading the high vanadium solid solution hydrogen storage alloy electrode rod into the EIGA electrode induction melting feeding system, and sealing the atomization chamber;

[0017] Step S3-2, evacuate the atomization chamber, then fill it with inert gas and start the circulation pump to make the inert gas in the atomization chamber evenly distributed;

[0018] Step S3-3, using an EIGA powder making furnace to melt the rod tip of the high vanadium solid solution hydrogen storage alloy electrode rod to form a freely falling metal liquid flow, which flows into an annular gap atomizer, and the inert gas enters the atomizer through a nozzle, interacts with the metal liquid flow at the outlet of the atomizer, and breaks the metal liquid flow into small droplets. The small droplets are quickly solidified under the cooling action of the water cooling system to obtain high-purity fine spherical powder.

[0019] Preferably, in step S3-2, the vacuum is evacuated to a vacuum degree less than 1.0×10 -1 Pa; the inert gas is one of nitrogen, argon or helium

[0020] Preferably, in step S3-3, the smelting parameters of the EIGA powder making furnace are set to: power 20-50kW, atomization parameters are set to: atomization pressure 3-10MPa; the feed speed of the EIGA electrode bar is set to 10-120mm / min, and the rotation speed is 30-300RPM.

[0021] Preferably, in step S4, the vibration screening and airflow classification of the fine spherical powder are carried out under the protection of argon, and the powder particle size range obtained after vibration screening is >150μm, 106~150μm and 0~106μm; the powder of 0~106μm is subjected to airflow classification to obtain powders with particle size ranges of 0~53μm and 53~106μm.

[0022] Compared with the prior art, the present invention has at least the following beneficial effects:

[0023] (1) The present invention adopts EIGA powder making technology to prepare fine spherical hydrogen storage alloy powder with high purity, good sphericity and strong composition uniformity, and adopts vacuum magnetic levitation melting technology instead of conventional vacuum arc melting or vacuum induction melting to prepare the hydrogen storage alloy electrode rod required for EIGA equipment. Vacuum magnetic levitation melting technology has the characteristics of "non-contact" melting. The metal raw materials usually achieve non-contact suspension with the wall of the crucible before melting. The melting process does not require a crucible, and has electromagnetic stirring, so that the melt is free from impurity contamination caused by electrodes and crucibles under high temperature conditions, and the alloy composition is more accurate and uniform, so that the hydrogen storage performance of the vanadium-based solid solution hydrogen storage alloy prepared by the method of the present invention is significantly improved.

[0024] (2) The high vanadium solid solution hydrogen storage alloy provided by the present invention has a high V content, which ensures that the alloy has a high hydrogen storage capacity and excellent cycle performance; by adding a rare earth element RE with high oxygen affinity and controlling its content, rare earth oxides can be formed and cracks and fresh surfaces can be generated on the basis of inhibiting the oxidation of other elements, providing more channels for hydrogen atoms to enter the alloy matrix, thereby improving the hydrogen storage performance and activation performance of the alloy. Specifically, at 25°C, the maximum hydrogen absorption capacity of the optimal sample is ≥3.5wt%H2, and the maximum hydrogen release capacity is ≥2.4wt%H2. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The drawings are only for the purpose of illustrating particular embodiments and are not to be construed as limiting the invention.

[0026] Figure 1 The present invention provides a flow chart of a method for preparing a high-vanadium solid solution hydrogen storage alloy and its fine spherical powder.

[0027] Figure 2 V provided by the embodiment of the present invention 71 Ti 10 Cr 17 XRD pattern of Fe2-1.5wt%Ce alloy fine spherical powder.

[0028] Figure 3 V provided by the embodiment of the present invention 71 Ti 10 Cr 17 Secondary electron image of Fe2-1.5wt%Ce alloy fine spherical powder.

[0029] Figure 4 V provided by the embodiment of the present invention 71 Ti 10 Cr 17 Backscattered electron image and EDS element surface scan of Fe2-1.5wt%Ce alloy fine spherical powder.

[0030] Figure 5 V provided by the embodiment of the present invention 71 Ti 10 Cr 17 Room temperature hydrogen absorption kinetic curve and room temperature hydrogen desorption kinetic curve of Fe2-1.5wt%Ce alloy fine spherical powder. DETAILED DESCRIPTION

[0031] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. In addition, the present invention can also be implemented in other ways different from those described herein, and therefore, the protection scope of the present invention is not limited by the specific embodiments disclosed below.

[0032] In order to illustrate the effectiveness of the method proposed in the present invention, the above technical solution of the present invention is described in detail below through specific embodiments to better reflect the advantages of the present invention.

[0033] The present invention provides a high-vanadium solid solution hydrogen storage alloy, the chemical formula of which is V x -Ti y -Cr z -M (1-x-y-z) -1~3wt% RE; wherein x, y, and z represent the atomic percentages of V, Ti, and Cr, respectively, the value range of x is 67~79at%, the value range of y is 2~14at%, the value range of x+y+z is 90~98at%, and M includes one or a combination of more than two transition metal elements such as Fe, Mn, Ni, and Co. The rare earth element RE is one of the rare earth metal elements such as Ce and Y, and the RE content is 1~3wt% of the weight of the high vanadium solid solution hydrogen storage alloy.

[0034] Example 1

[0035] This embodiment provides a high vanadium solid solution hydrogen storage alloy and a method for preparing a fine spherical powder of the high vanadium solid solution hydrogen storage alloy. In this embodiment, the element composition of the high vanadium solid solution hydrogen storage alloy is V 71 Ti 10 Cr 17 Fe2-1.5wt%Ce. Figure 1 As shown, the method for preparing the fine spherical powder of the high vanadium solid solution hydrogen storage alloy comprises the following steps:

[0036] Step S1, mixing high-purity metal raw materials according to alloy components, performing vacuum magnetic suspension smelting, casting into a cylindrical rod-shaped mold after smelting, and obtaining an initial blank rod after demoulding.

[0037] In this step, high-purity metal raw materials V (≥99.95%), Ti (≥99.99%), Cr (≥99.99%), Fe (≥99.99%), and Ce (≥99.9%) are prepared according to the elemental composition of V 71 Ti 10 Cr 17 The alloy composition of Fe2-1.5wt% Ce is prepared, and high-purity smelting is carried out under argon protection environment by vacuum magnetic levitation smelting technology. The smelting power is 150kW, the smelting time is 35min, and the number of smelting is 5 times. After the smelting is completed, it is cast into a cylindrical rod mold with a diameter of 30mm and a length of 160mm, and the initial blank rod is obtained after demolding.

[0038] Step S2: machining the initial blank rod to produce a high-vanadium solid solution hydrogen storage alloy electrode rod.

[0039] In this step, the initial blank bar is surface processed and threaded by a milling machine and a lathe to form the V required by the EIGA mill. 71 Ti 10 Cr 17 Fe2-1.5wt%Ce alloy electrode rod, wherein the thread processing length is 30mm.

[0040] Step S3: adopting electrode induction melting gas atomization (EIGA) powder making technology to gas atomize and powder the high vanadium solid solution hydrogen storage alloy electrode rod to obtain high-purity fine spherical powder.

[0041] In this step, V 71 Ti 10 Cr 17 The Fe2-1.5wt%Ce alloy electrode rods are loaded into the EIGA electrode induction melting feeding system and sealed; the atomization chamber is evacuated to a vacuum degree of <5×10 -4 Pa, then fill in argon as inert gas and start the circulation pump to make the argon in the atomization chamber evenly distributed; use EIGA powder making furnace to 71 Ti 10 Cr 17 The tip of the Fe2-1.5wt%Ce alloy electrode rod melts to form free-falling droplets or liquid flows. The molten liquid flows into the annular gap atomizer under the action of gravity. High-pressure and high-speed inert gas enters the atomizer through the nozzle and interacts with the metal liquid flow below the gas outlet to break the metal liquid flow into small droplets, which are quickly solidified under the cooling effect of the water cooling system to obtain high-purity V 71 Ti 10 Cr 17Fe2-1.5wt%Ce alloy fine spherical powder; wherein, the smelting parameters are set as: power 20kW; atomization parameters are set as: atomization pressure 5MPa; EIGA electrode rod feeding speed 60mm / min, rotation speed 120RPM.

[0042] Step S4: vibrating screen and air flow classify the fine spherical powder under the protection of argon atmosphere.

[0043] In this step, V 71 Ti 10 Cr 17 Fe2-1.5wt%Ce alloy fine spherical powder is subjected to vibration screening and airflow classification, and the vibration screening and airflow classification of the fine spherical powder are both carried out under the protection of high-purity argon; wherein, the powder particle size range obtained after vibration screening is +150μm, 106~150μm, 0~106μm; the powder of 0~106μm is subjected to airflow classification to obtain powders with particle size ranges of 0~53μm and 53~106μm.

[0044] The V prepared in Example 1 71 Ti 10 Cr 17 Fe2-1.5wt%Ce alloy fine spherical powder was subjected to X-ray diffraction (XRD) test, and the results are as follows Figure 2 As shown in the figure, it can be seen that high purity V 71 Ti 10 Cr 17 The XRD spectrum of the Fe2-1.5wt%Ce alloy fine spherical powder only shows the diffraction peak of the BCC phase. Since the content of the rare earth element Ce in the alloy is relatively low (only 1.5wt%), no diffraction peak related to the rare earth element Ce is detected.

[0045] The V prepared in Example 1 71 Ti 10 Cr 17 The Fe2-1.5wt%Ce alloy fine spherical powder was observed under a scanning electron microscope (SEM). Figure 3 , Figure 4 As shown, from Figure 3 , Figure 4 It can be seen that: high purity V 71 Ti 10 Cr 17The sphericity of the Fe2-1.5wt%Ce alloy fine spherical powder is good. The alloy is composed of a gray matrix BCC phase and a fine and dispersed cerium oxide phase (white bright spots). The high oxygen affinity of the rare earth element Ce induces the redistribution of the elements in the alloy, effectively inhibits the segregation of the Ti element, and prevents the precipitation of the Ti-rich phase. After adding Ce, the composition uniformity of the BCC main phase of the alloy is also significantly increased.

[0046] The V prepared in Example 1 71 Ti 10 Cr 17 The room temperature hydrogen storage performance of Fe2-1.5wt%Ce alloy fine spherical powder was evaluated. The test results are as follows Figure 5 As shown, after high-temperature activation at 400°C, the alloy can reach the maximum hydrogen absorption capacity (~3.5wt% H2) and hydrogen desorption capacity (~2.4wt% H2) at the first hydrogen absorption and desorption at 25°C.

[0047] Example 2

[0048] This embodiment provides a high vanadium solid solution hydrogen storage alloy and a method for preparing a fine spherical powder of the high vanadium solid solution hydrogen storage alloy. In this embodiment, the element composition of the high vanadium solid solution hydrogen storage alloy is V 77 Ti6Cr 10 Fe7-1wt%Ce, the preparation method of the fine spherical powder of the high vanadium solid solution hydrogen storage alloy comprises the following steps:

[0049] (1) High-purity metal raw materials V (≥99.95%), Ti (≥99.99%), Cr (≥99.99%), Fe (≥99.99%), and Ce (≥99.9%) are prepared according to the elemental composition of V 77 Ti6Cr 10 The alloy composition of Fe7-1 wt% Ce is prepared, and high-purity smelting is carried out in an argon protection environment using vacuum magnetic levitation smelting technology. The smelting power is 200 kW, the smelting time is 60 min, and the number of smeltings is 4 times. After the smelting is completed, it is cast into a cylindrical rod mold with a diameter of 60 mm and a length of 200 mm, and the initial blank rod is obtained after demolding.

[0050] (2) The initial blank rod is subjected to surface processing and thread processing, wherein the thread processing length is 30 mm, to produce a high-vanadium solid solution hydrogen storage alloy electrode rod.

[0051] (3) The electrode induction melting gas atomization (EIGA) powder making technology was used to gas atomize and powder the high vanadium solid solution hydrogen storage alloy electrode rod. Nitrogen was filled into the atomization chamber as an inert gas. The melting parameters were set as follows: power 30 kW; atomization parameters were set as follows: atomization pressure 5 MPa; EIGA electrode rod feed speed 90 mm / min, rotation speed 200 RPM, and finally high-purity fine spherical powder was obtained.

[0052] (4) The fine spherical powder is vibrated and air flow classified under the protection of argon atmosphere.

[0053] The V prepared in Example 2 77 Ti6Cr 10 The room temperature hydrogen storage performance of Fe7-1 wt% Ce alloy fine spherical powder was evaluated. After high-temperature activation at 400℃, the alloy could reach the maximum hydrogen absorption capacity (~3.6wt% H2) and hydrogen desorption capacity (~2.4wt% H2) at the first hydrogen absorption and desorption at 25℃.

[0054] Example 3

[0055] This embodiment provides a high vanadium solid solution hydrogen storage alloy and a method for preparing a fine spherical powder of the high vanadium solid solution hydrogen storage alloy. In this embodiment, the element composition of the high vanadium solid solution hydrogen storage alloy is V 69 Ti 12 Cr 13 Co6-2wt%Ce, the preparation method of the fine spherical powder of the high vanadium solid solution hydrogen storage alloy comprises the following steps:

[0056] (1) High-purity metal raw materials V (≥99.95%), Ti (≥99.99%), Cr (≥99.99%), Co (≥99.99%), and Ce (≥99.9%) are prepared according to the elemental composition of V 69 Ti 12 Cr 13 The alloy composition of Co6-2wt%Ce is prepared, and high-purity smelting is carried out under argon protection environment by vacuum magnetic levitation smelting technology. The smelting power is 280kW, the smelting time is 90min, and the smelting times are 5 times. After the smelting is completed, it is cast into a cylindrical rod mold with a diameter of 80mm and a length of 150mm, and the initial blank rod is obtained after demolding.

[0057] (2) The initial blank rod is subjected to surface processing and thread processing, wherein the thread processing length is 35 mm, to produce a high-vanadium solid solution hydrogen storage alloy electrode rod.

[0058] (3) The electrode induction melting gas atomization (EIGA) powder making technology is used to gas atomize and powder the high vanadium solid solution hydrogen storage alloy electrode rod. Helium is filled into the atomization chamber as an inert gas. The melting parameters are set as follows: power 45kW; atomization parameters are set as follows: atomization pressure 8MPa; EIGA electrode rod feed speed 45mm / min, rotation speed 250RPM, and finally high-purity fine spherical powder is obtained.

[0059] (4) The fine spherical powder is vibrated and air flow classified under the protection of argon atmosphere.

[0060] The V prepared in Example 3 69 Ti 12 Cr 13 The room temperature hydrogen storage performance of Co6-2 wt%Ce alloy fine spherical powder was evaluated. After high-temperature activation at 400℃, the alloy could reach the maximum hydrogen absorption capacity (~3.5wt% H2) and hydrogen desorption capacity (~2.4wt% H2) at the first hydrogen absorption and desorption at 25℃.

[0061] Example 4

[0062] This embodiment provides a high vanadium solid solution hydrogen storage alloy and a method for preparing a fine spherical powder of the high vanadium solid solution hydrogen storage alloy. In this embodiment, the element composition of the high vanadium solid solution hydrogen storage alloy is V 73 Ti8Cr 15 Mn2Ni2-3wt%Y, the preparation method of the fine spherical powder of the high vanadium solid solution hydrogen storage alloy comprises the following steps:

[0063] (1) High-purity metal raw materials V (≥99.95%), Ti (≥99.99%), Cr (≥99.99%), Mn (≥99.99%), Ni (≥99.99%), and Y (≥99.9%) are prepared according to the elemental composition of V 73 Ti8Cr 15 The alloy composition of Mn2Ni2-3wt%Y is prepared, and high-purity smelting is carried out under argon protection environment by vacuum magnetic levitation smelting technology. The smelting power is 150kW, the smelting time is 40min, and the smelting times are 4 times. After the smelting is completed, it is cast into a cylindrical rod mold with a diameter of 40mm and a length of 280mm, and the initial blank rod is obtained after demolding.

[0064] (2) The initial blank rod is subjected to surface processing and thread processing, wherein the thread processing length is 40 mm, to produce a high-vanadium solid solution hydrogen storage alloy electrode rod.

[0065] (3) Electrode induction melting gas atomization (EIGA) powder making technology is used to gas atomize and powder make high vanadium solid solution hydrogen storage alloy electrode rods, wherein argon is filled into the atomization chamber as an inert gas, the melting parameters are set as follows: power 30kW; atomization parameters are set as follows: atomization pressure 4MPa; EIGA electrode rod feed speed 120mm / min, rotation speed 60RPM, and finally high-purity fine spherical powder is obtained.

[0066] (4) The fine spherical powder is vibrated and air flow classified under the protection of argon atmosphere.

[0067] The V prepared in Example 4 73 Ti8Cr 15 The room temperature hydrogen storage performance of Mn2Ni2-3 wt%Y alloy fine spherical powder was evaluated. After high-temperature activation at 400℃, the alloy could reach the maximum hydrogen absorption capacity (~3.6wt% H2) and hydrogen desorption capacity (~2.4wt% H2) at the first hydrogen absorption and desorption at 25℃.

[0068] Although the specific embodiments of the present invention depict various actions or steps in a specific order, this should be understood as requiring such actions or steps to be performed in the specific order shown or in a sequential order, or requiring all illustrated actions or steps to be performed to obtain the desired results. Under certain circumstances, multitasking and parallel processing may be advantageous. Similarly, although several specific implementation details are included in the above discussion, these should not be interpreted as limiting the scope of the present disclosure. Certain features described in the context of a separate embodiment can also be implemented in a single implementation in combination. On the contrary, the various features described in the context of a single implementation can also be implemented in multiple implementations individually or in any suitable sub-combination. The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or replacements that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

[0069] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A high vanadium solid solution hydrogen storage alloy, characterized in that: The chemical formula of the high vanadium solid solution hydrogen storage alloy is V x -Ti y -Cr z -M (1-x-y-z) -1~3wt% RE, wherein x, y, z are the atomic percentages of V, Ti, and Cr respectively, the value range of x is 67~79at%, the value range of y is 2~14at%, the value range of x+y+z is 90~98at%, and M includes a combination of one or more of Fe, Mn, Ni and Co. The rare earth element RE is Ce or Y, and the RE content is 1~3wt% of the weight of the high vanadium solid solution hydrogen storage alloy.

2. The high vanadium solid solution hydrogen storage alloy according to claim 1, characterized in that: The value range of x+y is 75 to 85 at%.

3. A method for preparing a fine spherical powder of a high vanadium solid solution hydrogen storage alloy as claimed in any one of claims 1 to 2, characterized in that: The following steps are involved: Step S1, mixing high-purity metal raw materials according to the chemical formula of the alloy, performing vacuum magnetic suspension smelting, casting into a cylindrical rod-shaped mold after smelting, and obtaining an initial blank rod after demoulding; Step S2, machining the initial blank rod to produce a high vanadium solid solution hydrogen storage alloy electrode rod; Step S3, using electrode induction melting gas atomization powder making technology to gas atomize and powder-make the high vanadium solid solution hydrogen storage alloy electrode rod to obtain high-purity fine spherical powder; Step S4: vibrating screen and air flow classify the fine spherical powder under the protection of argon atmosphere.

4. The method for preparing high vanadium solid solution hydrogen storage alloy fine spherical powder according to claim 3, characterized in that: In step S1, the purity of the high-purity metal raw materials is >99.5%; the vacuum magnetic levitation smelting process is carried out under an argon protection environment; the smelting parameters are: smelting power 100-300kW, smelting time 30-120min, smelting times 3-6 times; the diameter of the cylindrical rod mold is 30-90mm, and the length is 150-300mm.

5. The method for preparing high vanadium solid solution hydrogen storage alloy fine spherical powder according to claim 4, characterized in that: Step S2 specifically includes: The initial blank rod material obtained in step S1 is subjected to surface processing and thread processing by a milling machine and a lathe to produce a high-vanadium solid solution hydrogen storage alloy electrode rod material, and the thread processing length is 20 to 40 mm.

6. The method for preparing high vanadium solid solution hydrogen storage alloy fine spherical powder according to claim 5, characterized in that: Step S3 specifically includes: Step S3-1, loading the high vanadium solid solution hydrogen storage alloy electrode rod into the EIGA electrode induction melting feeding system, and sealing the atomization chamber; Step S3-2, evacuate the atomization chamber, then fill it with inert gas and start the circulation pump to make the inert gas in the atomization chamber evenly distributed; Step S3-3, using an EIGA powder making furnace to melt the rod tip of the high vanadium solid solution hydrogen storage alloy electrode rod to form a freely falling metal liquid flow, which flows into an annular gap atomizer, and the inert gas enters the atomizer through a nozzle, interacts with the metal liquid flow at the outlet of the atomizer, and breaks the metal liquid flow into small droplets. The small droplets are quickly solidified under the cooling action of the water cooling system to obtain high-purity fine spherical powder.

7. The method for preparing high vanadium solid solution hydrogen storage alloy fine spherical powder according to claim 6, characterized in that: In step S3-2, the vacuum is evacuated to a vacuum degree less than 1.0×10 -1 Pa; the inert gas is one of nitrogen, argon or helium.

8. The method for preparing high vanadium solid solution hydrogen storage alloy fine spherical powder according to claim 7, characterized in that: In step S3-3, the smelting parameters of the EIGA powder making furnace are set to: power 20-50kW, atomization parameters are set to: atomization pressure 3-10MPa; the feed speed of the EIGA electrode bar is set to 10-120mm / min, and the rotation speed is 30-300RPM.

9. The method for preparing high vanadium solid solution hydrogen storage alloy fine spherical powder according to claim 8, characterized in that: In step S4, the vibration screening and airflow classification of the fine spherical powder are carried out under the protection of argon gas. The powder particle size range obtained after vibration screening is >150μm, 106~150μm and 0~106μm; the powder of 0~106μm is subjected to airflow classification to obtain powders with particle size ranges of 0~53μm and 53~106μm.

Citation Information

Cited By

  • Device and method for preparing titanium hydrogen storage alloy for solid hydrogen storage

    CN121163220A