Preparation method and application of Fe3O4 / Au / Ag composite nanomaterial
By preparing Fe3O4/Au/Ag composite nanomaterials as Raman substrates, the problem of high-efficiency detection of levofloxacin in existing technologies has been solved, achieving high sensitivity and stable detection results.
Patent Information
- Application Number
- CN202411152410.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
AI Technical Summary
Existing technologies are insufficient for efficiently detecting levofloxacin concentrations, leading to environmental pollution and increased bacterial resistance.
Fe3O4/Au/Ag composite nanomaterials were prepared as Raman substrates, and surface-enhanced Raman spectroscopy and standard curve method were used for detection.
It achieves highly sensitive detection of levofloxacin, with an enhancement factor of up to several thousand times, capable of detecting single molecules, and possesses good stability and reproducibility.
Smart Images

Figure CN119035567A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of drug detection, and in particular to a preparation method and application of a Fe3O4 / Au / Ag composite nanomaterial. Background Art
[0002] Precious metals are widely used in many fields due to their special physical and chemical properties. Precious metals include gold (Au), silver (Ag), platinum (Pt), palladium (Pd), ruthenium (Ru), osmium (Os), rhodium (Rh) and iridium (Ir). In terms of optics, thermal, mechanical and chemical aspects, precious metals and their alloys show excellent comprehensive properties, especially gold and silver. With the continuous development of nanotechnology, nano precious metal materials not only have the properties of bulk materials, but also have the special physical and chemical properties of nanomaterials, and their properties are more prominent. In recent years, combining inorganic materials with magnetic nanoparticles to develop magnetic nanocomposites has gradually become a research hotspot. At present, magnetic nanomaterials mainly involve metal oxides such as iron, manganese, cobalt and their composites.
[0003] Fe3O4 has become one of the most widely used magnetic nanomaterials due to its simple preparation process, high stability, significant magnetism, biocompatibility and easy surface modification. This material not only inherits the physical and chemical properties of traditional magnetic materials, but also combines the surface effect and size effect of nanomaterials. In particular, when the particle size of magnetic nanoparticles is less than 30nm, they will show superparamagnetism, so they show great application potential in many fields. Magnetic composite materials can not only make full use of the characteristics of the constituent materials, but also compensate each other to produce synergistic effects, overcome the limitations of a single material, give full play to the performance advantages of the material, and obtain unique optical, electrochemical and chemical stability characteristics. Therefore, in the fields of photothermal conversion, biological detection, catalysis, sensing, etc., this type of material shows broad application prospects.
[0004] The functional technology of magnetic nanomaterials has been developing continuously in recent years. When the particle size is reduced to the nanometer level, the small size effect, surface effect, quantum size effect and macroscopic quantum tunneling effect of nanoparticles make them have special magnetic properties, which are different from conventional materials. Compared with traditional adsorption technology, magnetic nanomaterials are widely used in pollutant and drug detection due to their advantages such as small material diameter, large specific surface area, surface functionalization and chemical properties of magnetic materials.
[0005] Raman spectroscopy is a typical vibrational spectroscopy technique that can provide fingerprint information about the molecular composition and structure of a sample through the inelastic scattering phenomenon between vibrating molecules and monochromatic photons. When molecules are adsorbed on metals with rough surfaces, the molecular Raman signal can be significantly amplified, i.e., surface-enhanced Raman scattering. Therefore, surface-enhanced Raman scattering has become a powerful analytical tool for detecting trace drugs and organic pollutants due to its high sensitivity, specificity, and ability to detect molecular information from biological samples. Surface-enhanced Raman spectroscopy (SERS) is a highly sensitive detection tool that has been widely used in many fields. The SERS enhancement effect mainly includes electromagnetic enhancement effect and chemical enhancement effect. The mechanism of the electromagnetic enhancement effect is to generate a high-intensity electromagnetic field by excitation of local surface plasmon resonance. The chemical mechanism originates from the unique interaction between the target molecule and the SERS substrate, including electron exchange through sharing or transfer with the nanostructure. Therefore, SERS has the advantages of ordinary Raman spectroscopy and amplifies the Raman signal through the interaction between the analyte molecule and the nanostructure platform. However, when dealing with noble metal nanostructures, the amplification of the Raman signal observed in the SERS spectrum is mainly due to the electromagnetic field (electromagnetic enhancement) generated by the metal surface. In addition, electron transfer can occur between the analyte and the metal nanostructure, which can also produce a chemical enhancement process. Under the combined effect of the two enhancement mechanisms, the SERS enhancement factor can be amplified thousands of times, and even a single molecule can be detected.
[0006] Recently, a series of reports have been published on the use of precious metal nano-gold, silver or other gold-silver-containing composites as surface-enhanced Raman substrates to detect analytes. Levofloxacin is a commonly used fluoroquinolone antibiotic with good antibacterial properties against various bacteria. It is widely used to treat various diseases, such as bacterial infections and inflammation. Since animals cannot effectively decompose this antibiotic, to a large extent, the antibiotic will return to the environment in the form of derivatives or original substances, resulting in environmental pollution or increased bacterial resistance, ultimately causing health risks. Therefore, accurate detection of its concentration is crucial to protecting the environment and human health. Summary of the invention
[0007] The technical problem to be solved by the present invention is to provide a method for preparing a Fe3O4 / Au / Ag composite nanomaterial in view of the deficiencies of the above-mentioned prior art. Fe3O4, as a magnetic inorganic material, is compounded with Au and Ag nanomaterials to prepare a Fe3O4 / Au / Ag composite nanomaterial. The Fe3O4 / Au / Ag composite nanomaterial can be used as a Raman substrate to detect levofloxacin with the help of a surface enhanced Raman spectrometer and a standard curve.
[0008] The present invention provides a method for preparing a Fe3O4 / Au / Ag composite nanomaterial, comprising the following steps:
[0009] S1. Preparation of Fe3O4: FeCl3·6H2O is dissolved in ultrapure water, triethanolamine is added thereto and stirred thoroughly to obtain a Fe(III)-TEA alkaline solution, and then the Fe(III)-TEA alkaline solution is transferred into a high-pressure reactor, dried thoroughly for reaction, and the dried product is poured into a beaker, separated by a magnet, the supernatant is poured out, washed thoroughly, and dried to obtain the product Fe3O4;
[0010] S2. Preparation of Au-AgNPs: Boil ultrapure water and keep boiling. After 30 minutes, add AgNO3 solution and HAuCl4 solution, and then quickly add sodium citrate solution. Keep boiling. After sufficient reaction under stirring and condensation reflux conditions, stop heating, and after the solution is cooled to room temperature, dilute it to 100 mL to obtain Au-AgNPs.
[0011] S3, preparation of surface amino-treated Fe3O4: take the Fe3O4 prepared in S1 and add it into ultrapure water. After the Fe3O4 is evenly dispersed by ultrasound, add the polyethyleneimine solution in batches while stirring. After all the solution is added, continue stirring for 3 hours. Use a magnet to separate and remove the supernatant. After sufficient washing, remove the supernatant again to obtain surface amino-treated Fe3O4.
[0012] S4. Preparation of Fe3O4 / Au / Ag composite nanomaterials: Add the Au-AgNPs prepared in S2 to the surface-amino-treated Fe3O4 prepared in S3, stir thoroughly, and add the Au-AgNPs prepared in S2 again after the upper clear liquid becomes colorless. Repeat the addition of Au-AgNPs 10 times until the upper clear liquid turns light orange. Adsorb the lower solid with a magnet, wash thoroughly and dry to obtain Fe3O4 / Au / Ag composite nanomaterials.
[0013] According to the preparation method of Fe3O4 / Au / Ag composite nanomaterial provided by the present invention, the mass volume ratio of FeCl3·6H2O, ultrapure water and triethanolamine in S1 is 1.3907g:70mL:10mL.
[0014] According to the preparation method of Fe3O4 / Au / Ag composite nanomaterials provided by the present invention, the stirring time in S1 is 10 minutes, the drying reaction temperature is 180°C, the drying reaction time is 5 hours, the washing method is alternating washing with ultrapure water and anhydrous ethanol, the drying temperature is 65°C, and the drying time is 6 hours.
[0015] According to the preparation method of Fe3O4 / Au / Ag composite nanomaterials provided by the present invention, the volume ratio of the total amount of ultrapure water, AgNO3 solution and HAuCl4 solution and the sodium citrate solution in S2 is 90mL:10mL:0.8mL, the concentrations of the AgNO3 solution and the HAuCl4 solution are both 0.01mol / L, the concentration of the sodium citrate solution is 0.1mol / L, and the time for sufficient reaction is 40min.
[0016] According to the preparation method of Fe3O4 / Au / Ag composite nanomaterial provided by the present invention, the mass volume ratio of Fe3O4, ultrapure water and polyethyleneimine solution in S3 is 0.1010g:20mL:20mL, and the concentration of the polyethyleneimine solution is 5mg / mL.
[0017] According to the preparation method of Fe3O4 / Au / Ag composite nanomaterial provided by the present invention, the method of adding polyethyleneimine solution in batches in S3 is: adding 5 mL of polyethyleneimine solution every 10 minutes.
[0018] According to the preparation method of Fe3O4 / Au / Ag composite nanomaterial provided by the present invention, the ultrasonic time in S3 is 20 minutes, the stirring speed is 300r / min, and the detergent used for the washing is ultrapure water.
[0019] According to the preparation method of Fe3O4 / Au / Ag composite nanomaterial provided by the present invention, the mass volume ratio of the surface amino-treated Fe3O4 and Au-AgNPs in S4 is 0.02g:20mL.
[0020] According to the preparation method of Fe3O4 / Au / Ag composite nanomaterial provided by the present invention, the stirring speed in S4 is 200r / min, the washing method is alternating washing with ultrapure water and anhydrous ethanol, the drying temperature is 65°C, and the drying time is 6h.
[0021] The present invention also provides an application of the Fe3O4 / Au / Ag composite nano material, wherein the Fe3O4 / Au / Ag composite nano material is used for detecting levofloxacin.
[0022] Compared with the prior art, the present invention has the following advantages:
[0023] The invention provides a preparation method of a Fe3O4 / Au / Ag composite nanomaterial. Superparamagnetic nano Fe3O4 is synthesized by a triethanolamine hydrothermal method, Au-AgNPs are synthesized by a co-reduction method, and Au-AgNPs are subsequently loaded on Fe3O4 to synthesize the Fe3O4 / Au / Ag composite nanomaterial.
[0024] Fe3O4 / Au / Ag composite nanomaterials can be used to detect levofloxacin. The material is used as a Raman substrate, and with the help of surface enhanced Raman spectroscopy technology, levofloxacin can be detected using the standard curve method. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the X-ray diffraction pattern of ferroferric oxide prepared by triethanolamine hydrothermal method;
[0026] Figure 2 is the UV-visible spectra of AuNPs;
[0027] Figure 3 is the UV-visible spectra of AgNPs;
[0028] Figure 4 is the UV image of Au-AgNPs prepared in Comparative Example 1;
[0029] Figure 5 is the UV image of Au-AgNPs prepared in Example 1;
[0030] Figure 6 TEM image of Fe3O4 / Au / Ag composite nanomaterial;
[0031] Figure 7 This is the energy spectrum of Fe3O4 / Au / Ag composite nanomaterials;
[0032] Figure 8 This is the Raman spectrum of levofloxacin solid;
[0033] Fig. 9 SERS spectra of levofloxacin series solutions;
[0034] Fig.10 It is the working curve diagram;
[0035] Fig.11 This is a diagram of repeated experiments;
[0036] Fig.12 It is a bar graph of RSD. DETAILED DESCRIPTION
[0037] Example 1
[0038] This embodiment provides a method for preparing a Fe3O4 / Au / Ag composite nanomaterial. In this embodiment, a co-reduction method is used to prepare Au-Ag nano alloy sol. The specific steps are as follows:
[0039] S1. Preparation of Fe3O4 (triethanolamine method): 1.3907 g of FeCl3·6H2O was dissolved in 70 mL of ultrapure water, and then 10.0 mL of triethanolamine (TEA) was added thereto and stirred for 10 min using a magnetic stirrer to obtain an Fe(III)-TEA alkaline solution. The Fe(III)-TEA alkaline solution was then poured into a 100 mL polytetrafluoroethylene (Teflon) autoclave, and then the Teflon autoclave was placed in an oven at 180° C. for reaction for 5 h. The black product obtained in the Teflon autoclave was poured into a beaker, and layered with a permanent magnet, the supernatant was poured out, and then the product was cross-washed with ultrapure water and anhydrous ethanol for three times. The product was placed in an oven at 65° C. and dried for 6 h. After drying, the product Fe3O4 was scraped off with a glass rod and stored in a centrifuge tube for later use;
[0040] S2, preparation of Au-Ag nano alloy sol (co-reduction method): 90mL of ultrapure water was boiled and kept boiling for 30min, then a 0.01mol / L AgNO3 solution and a 0.01mol / L HAuCl4 solution were added, the total amount of the added AgNO3 solution and the HAuCl4 solution was 10mL, i.e., the total concentration of Au and Ag in the reaction solution was 0.2mmol / L, and the molar fractions of Au and Ag were 0.4 and 0.2, and then 0.8mL of a 0.1mol / L sodium citrate solution was quickly added to keep the reaction system boiling, and the reaction was continued for 40min under stirring and reflux conditions, and the heating was stopped, and the solution was cooled to room temperature and then fixed to 100mL to obtain Au-Ag nano alloy sol (Au-AgNPs), which was stored in dark conditions for standby use;
[0041] S3, preparation of surface amino-treated Fe3O4: take 0.1010g of Fe3O4 prepared in S1 and put it into a 250mL beaker, add 20mL ultrapure water, shake it evenly and put it into an ultrasonic cleaner, ultrasonicate it for 20min, take out the beaker after the Fe3O4 is evenly dispersed, put it into a mechanical stirring device after it cools down slightly, stir it at a speed of 300r / min, and add 5mL of 5mg / mL polyethyleneimine (PEI) solution every 10min, stop stirring after adding 20mL PEI solution, continue stirring for 3h, separate it with a magnet and remove the supernatant, then wash it 3 times with ultrapure water and remove the supernatant, to obtain surface amino-treated Fe3O4;
[0042] S4, preparation of Fe3O4 / Au / Ag composite nanomaterials: add 20mL of Au-AgNPs prepared in S2 to 0.02g of surface-aminated Fe3O4 prepared in S3, stir at a speed of 200r / min, add 20mL of Au-AgNPs prepared in S2 again after the supernatant becomes colorless, repeat the above operation, add 200mL of Au-AgNPs in total, the supernatant becomes light orange, and the color of the supernatant does not become lighter with the extension of stirring time, indicating that the Fe3O4 loading of Au-AgNPs is close to saturation, adsorb the obtained solid with a magnet, and wash it alternately with anhydrous ethanol and ultrapure water three times, put it in a 65°C oven for drying, and obtain Fe3O4 / Au / Ag composite nanomaterials, take it out and store it in a centrifuge tube for standby use.
[0043] Comparative Example 1
[0044] This comparative example provides a method for preparing a Fe3O4 / Au / Ag composite nanomaterial. In this example, a seed growth method is used to prepare Au-Ag nano alloy sol. The specific steps are as follows:
[0045] S1. Preparation of Fe3O4: 1.3907 g of FeCl3·6H2O was dissolved in 70 mL of ultrapure water, and then 10.0 mL of TEA was added thereto and stirred for 10 min using a magnetic stirrer to obtain an Fe(Ⅲ)-TEA alkaline solution. The Fe(Ⅲ)-TEA alkaline solution was then poured into a 100 mL Teflon autoclave, and then the Teflon autoclave was placed in an oven at 180°C for reaction for 5 h. The black product obtained in the Teflon autoclave was poured into a beaker, and layered with a permanent magnet, and the supernatant was poured out. The product was then cross-washed with ultrapure water and anhydrous ethanol for three times, and the product was placed in an oven at 65°C for drying for 6 h. After drying, the product Fe3O4 was scraped off with a glass rod and stored in a centrifuge tube for later use;
[0046] S2. Preparation of AuNPs: Pipette 0.25 mL of 0.1 mol / L chloroauric acid (HAuCl4) solution into 100 mL of ultrapure water, stir thoroughly and heat until completely boiled, quickly inject 1.5 mL of 1% sodium citrate solution with a syringe, and continue the reaction for 30 min under condensation reflux. Stop heating when the solution turns wine red, stop stirring after cooling to room temperature, and obtain AuNPs, which are refrigerated after taking measures to protect from light for later use;
[0047] S3. Preparation of AgNPs: 36 mg of silver nitrate was dissolved in 100 mL of ultrapure water, and the mixture was heated with stirring until it was completely boiled. Then, 4 mL of 1% sodium citrate solution was added, and the boiling reaction was maintained for 1 h. After the reaction was complete, the mixture was cooled to room temperature to obtain AgNPs, which appeared light yellow.
[0048] S4. Preparation of Au-AgNPs (seed growth method): 10.0 mL of the AuNPs prepared in S2 and 1.5 mL of 0.1 mol / L ascorbic acid were mixed in a round-bottom flask, and then 2.0 mL of 1 mmol / L AgNO3 solution was added thereto at a rate of 30 seconds per drop. Since AgNO3 was reduced by ascorbic acid, the generated AgNPs continued to grow on the surface of the Au seeds. After the solution changed from wine red to orange-yellow, it was stirred for another 30 minutes to obtain Au-AgNPs.
[0049] S5, preparation of surface amino-treated Fe3O4: 0.1010g of Fe3O4 prepared in S1 was placed in a 250mL beaker, 20mL of ultrapure water was added, and the mixture was shaken evenly and placed in an ultrasonic cleaner for 20min. After the Fe3O4 was evenly dispersed, the beaker was taken out, and after it was slightly cooled, it was placed in a mechanical stirring device and stirred at a speed of 300r / min. At the same time, 5mL of 5mg / mL PEI solution was added every 10min, and the stirring was stopped after 20mL of PEI solution was added. The stirring was continued for 3h, and the supernatant was removed after separation with a magnet, and then washed 3 times with ultrapure water and the supernatant was removed to obtain surface amino-treated Fe3O4;
[0050] S6. Preparation of Fe3O4 / Au / Ag composite nanomaterials: Add 20 mL of Au-AgNPs prepared in S4 to the surface-aminated Fe3O4 prepared in S5, stir at a speed of 200 r / min, and add 20 mL of Au-AgNPs prepared in S4 again after the supernatant becomes colorless. Repeat the above operation. After adding 200 mL of Au-AgNPs in total, the supernatant appears light orange, and the color of the supernatant does not fade with the extension of stirring time, indicating that the Fe3O4 loaded with Au-AgNPs is close to saturation. The obtained solid is adsorbed by a magnet, and washed alternately with anhydrous ethanol and ultrapure water three times, and then dried in a 65°C oven to obtain Fe3O4 / Au / Ag composite nanomaterials, which are taken out and stored in a centrifuge tube for later use.
[0051] In Example 1 and Comparative Example 1, superparamagnetic nano-Fe3O4 was synthesized by triethanolamine hydrothermal method, and Au-AgNPs were synthesized by seed growth method and co-reduction method. Au-AgNPs were then loaded on Fe3O4 to finally synthesize Fe3O4 / Au / Ag composite materials.
[0052] Example 2
[0053] This embodiment provides a SERS determination method for levofloxacin.
[0054] ①. Preparation of levofloxacin standard curve:
[0055] The test parameters of the Raman spectrometer were set to: dynamic, laser 633nm, laser power 50% and exposure time 10s, a levofloxacin (LVFX) solid sample was placed on a glass slide, the phase in the eyepiece of the Raman spectrometer was adjusted, and scanning was performed to obtain a Raman spectrum.
[0056] Prepare a series of levofloxacin aqueous solutions (10 -3 , 10 -4、 10 -5 , 10 -6 and 10 -7 mol / L), the composite material was coated on a glass slide, and the Raman spectra of a series of levofloxacin concentrations were tested.
[0057] Before testing SERS, a substrate-free levofloxacin solution was tested first. When the concentration was less than 0.1 mol / L, the pure aqueous solution of levofloxacin had almost no Raman peak.
[0058] ②. SERS reproducibility analysis:
[0059] Take the concentration as 10 -3 mol / L levofloxacin solution was used for stability analysis, and the SERS spectra of the 9 tests were as follows: Fig.11 and Fig.12 As shown, then 1615cm -1 The SERS peak at was analyzed for error.
[0060] ③、Determination of actual samples:
[0061] Take water samples from the environment, filter them, treat them according to the above method, test them, and do a spike recovery experiment.
[0062] Example 3
[0063] In this example, the material prepared in Example 1 is characterized.
[0064] ①. XRD characterization of Fe3O4 / Au / Ag composite nanomaterials and Fe3O4.
[0065] The XRD characterization results of Fe3O4 prepared in S1 are as follows Figure 1As shown, there are six groups of peaks, namely 30.1°, 35.5°, 43.1°, 53.5°, 57.0° and 62.5°. Among them, 30.1° is the peak of the (220) crystal plane, 35.5° is the peak of the (311) crystal plane, 43.1° is the peak of the (400) crystal plane, 53.5° is the peak of the (422) crystal plane, 57.0° is the peak of the (511) crystal plane, and 62.5° is the peak of the (440) crystal plane.
[0066] Through XRD analysis, the prepared Fe3O4 has a cubic spinel structure. Compared with the XRD spectrum of Fe3O4, there are still 6 peaks at 30.1°, 35.5°, 43.1°, 53.5°, 57.0° and 62.5° in the XRD spectrum of Fe3O4 / Au / Ag composite material, which shows that the crystal structure of Fe3O4 has not changed after loading nano-Au and nano-Ag. Moreover, in the XRD spectrum of the Fe3O4 / Au / Ag composite material, there are four additional peaks at 38.2°, 44.5°, 64.5°, and 77.8° compared with the XRD spectrum of Fe3O4. The peak at 38.2° corresponds to the (111) crystal plane of Au or Ag, the peak at 44.5° corresponds to the (200) crystal plane of Au or Ag, the peak at 64.5° corresponds to the (220) crystal plane of Au or Ag, and the peak at 77.8° corresponds to the (311) crystal plane of Au or Ag, all of which come from the Bragg reflection of their corresponding crystal planes.
[0067] ②. Ultraviolet absorption spectrum characterization of AuNPs and AgNPs.
[0068] The AuNPs and AgNPs prepared in Comparative Example 1 were scanned by UV-visible spectrophotometry, and the obtained spectra were as follows: Figure 2 and Figure 3 shown.
[0069] from Figure 2 It can be seen that AuNPs have a maximum absorption peak near the wavelength of 520nm, which is the characteristic absorption peak of spherical AuNPs. Figure 3 It can be seen that AgNPs only have a unique absorption peak in the wavelength range of 400-430nm, which is the characteristic absorption peak of typical spherical AgNPs.
[0070] comprehensive Figure 2 and Figure 3 , indicating that AuNPs and AgNPs were successfully prepared in Comparative Example 1.
[0071] ③Ultraviolet absorption spectrum characterization of Au-AgNPs.
[0072] The Au-AgNPs prepared by the seed growth method in Comparative Example 1 were characterized by ultraviolet absorption spectroscopy. The characterization results are as follows: Figure 4 As shown in the figure, compared with the UV-visible spectra of AuNPs, there is a certain degree of blue shift, which is speculated to be related to the preparation method.
[0073] Since the surface of Au-AgNPs is coated with a certain amount of AgNPs, and Ag is deposited on the surface of Au with very small gaps, the electron density in the Au nanoparticles increases due to the electron overflow effect of the metal, thus causing the resonance absorption band of AuNPs to blue shift.
[0074] The Au-AgNPs prepared by the co-reduction method in Example 1 were characterized by ultraviolet absorption spectroscopy. The characterization results are as follows: Figure 5 As shown, the spectra all have different degrees of red shift. It is speculated that the alloy structure formed by them makes the average diameter of the particles larger, thus causing the spectra to red shift.
[0075] comprehensive Figure 4 and Figure 5 Although the absorption peak of Au-AgNPs prepared by the seed growth method is not much different from that of the original nanoparticles, to a certain extent, it shows that its properties are closer to the original gold-silver nanoparticles than the Au-Ag composite material prepared by the co-reduction method, but its preparation complexity is greater than that of the gold-silver co-reduction method.
[0076] ④TEM and EDX characterization of Fe3O4 / Au / Ag composite nanomaterials.
[0077] Figure 6 and Figure 7 TEM and energy spectrum characterization of the Fe3O4 / Au / Ag composite nanomaterial prepared in Example 1 respectively.
[0078] from Figure 6 It can be seen that the gray particles are Fe3O4 nanoparticles. The dark black particles are nano-Au and Ag. Since Fe3O4, Au and Ag nanoparticles are in agglomerated state, Figure 7 It can be seen that the product contains elements such as Fe, O, Au and Ag, indicating that Example 1 successfully prepared the Fe3O4 / Au / Ag composite nanomaterial.
[0079] Example 4
[0080] This embodiment provides an application of a Fe3O4 / Au / Ag composite nanomaterial for determining levofloxacin (LVFX).
[0081] ① SERS spectra of LVFX solutions with different concentrations.
[0082] The LVFX solid sample was placed on a glass slide and scanned to obtain the following Figure 8From the Raman spectrum shown in the figure, it can be seen that the main characteristic peak of LVFX molecule is located at 1362cm -1 、1400cm -1 、1532cm -1 and 1618cm -1 .
[0083] Among them, 1362cm -1 The peak at 1400 cm-1 is attributed to the CH vibration of the benzene ring. -1 The Raman band at 1532 cm is attributed to the vibration of the quinolone ring. -1 and 1618cm -1 The Raman bands at are attributed to the vibration of the quinolone ring and the antisymmetric stretching vibration of C=C in the aromatic ring.
[0084] The Raman spectra of LVFX were tested over a range of concentrations, such as Fig. 9 As shown in Figure 2, with the decrease of LVFX, the Raman spectrum signal of LVFX solution gradually weakened, and the more obvious 1603cm -1 The characteristic peak intensity, the relationship between its Raman spectrum intensity and solution concentration is as follows Fig.10 As shown. In 10 -3 ~10 -7 It is linear in the concentration range of mol / L, and the standard curve equation is y=957x+6559.2, with a correlation coefficient of R 2 =0.9822.
[0085] ②Performance analysis of Fe3O4 / Au / Ag composite nanomaterials method.
[0086] Take the concentration as 10 -3 mol / L LVFX solution was used for repeatability analysis. The SERS spectra of the 9 tests were as follows: Fig.11 and 12 As shown, take 1615cm -1 The SERS peak at 10 was analyzed and the relative standard deviation (RSD) of the test results was calculated. The calculated RSD was 2.2%, indicating that the SERS detection of LVFX adsorbed on the Fe3O4 / Au / Ag composite material has good stability, and its enhancement factor (EF) is 2.26×10 4 .
[0087] This is attributed to the fact that Fe3O4 / Au / Ag composites have two different enhancement mechanisms, namely electromagnetic enhancement and chemical enhancement.
[0088] The detection limit was calculated by the detection limit formula LOD = 3δ / k, where δ is the standard deviation of the blank sample and k is the slope of the calibration curve at 1615 cm -1 At the peak, LOD is 0.2×10-8 .
[0089] ③Detection of LVFX in domestic water
[0090] LVFX in domestic water was tested and no LVFX was detected. A spike recovery test was also conducted. The results are shown in Table 1.
[0091] Table 1 Spiked recovery experiment
[0092]
[0093] In summary, Fe3O4 / Au / Ag as the Raman substrate has a strong Raman signal enhancement effect, and establishes a relatively good linear relationship between the SERS signal and the logarithm of the LVFX concentration. When using this material for Raman enhanced spectroscopy detection, it has good stability and reproducibility.
[0094] This embodiment establishes a new method for rapid, simple and accurate detection of levofloxacin antibiotics, which is expected to be used in the detection of actual LVFX samples in the fields of food, environment, medicine, health and agriculture in the future.
[0095] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a Fe3O4 / Au / Ag composite nanomaterial, characterized in that: The following steps are involved: S1. Preparation of Fe3O4: FeCl3·6H2O is dissolved in ultrapure water, triethanolamine is added thereto and stirred thoroughly to obtain a Fe(III)-TEA alkaline solution, and then the Fe(III)-TEA alkaline solution is transferred into a high-pressure reactor, dried thoroughly for reaction, and the dried product is poured into a beaker, separated by a magnet, the supernatant is poured out, washed thoroughly, and dried to obtain the product Fe3O4; S2. Preparation of Au-AgNPs: Boil ultrapure water and keep boiling. After 30 minutes, add AgNO3 solution and HAuCl4 solution, and then quickly add sodium citrate solution. Keep boiling. After sufficient reaction under stirring and condensation reflux conditions, stop heating, and after the solution is cooled to room temperature, dilute it to 100 mL to obtain Au-AgNPs. S3, preparation of surface amino-treated Fe3O4: take the Fe3O4 prepared in S1 and add it into ultrapure water. After the Fe3O4 is evenly dispersed by ultrasound, add the polyethyleneimine solution in batches while stirring. After all the solution is added, continue stirring for 3 hours. Use a magnet to separate and remove the supernatant. After sufficient washing, remove the supernatant again to obtain surface amino-treated Fe3O4. S4. Preparation of Fe3O4 / Au / Ag composite nanomaterials: Add the Au-AgNPs prepared in S2 to the surface-amino-treated Fe3O4 prepared in S3, stir thoroughly, and add the Au-AgNPs prepared in S2 again after the upper clear liquid becomes colorless. Repeat the addition of Au-AgNPs 10 times until the upper clear liquid turns light orange. Adsorb the lower solid with a magnet, wash thoroughly and dry to obtain Fe3O4 / Au / Ag composite nanomaterials.
2. The method for preparing the Fe3O4 / Au / Ag composite nanomaterial according to claim 1, characterized in that: The mass volume ratio of FeCl3·6H2O, ultrapure water and triethanolamine described in S1 is 1.3907 g:70 mL:10 mL.
3. The method for preparing the Fe3O4 / Au / Ag composite nanomaterial according to claim 1, characterized in that: The stirring time in S1 is 10 minutes, the drying reaction temperature is 180° C., the drying reaction time is 5 hours, the washing method is alternating washing with ultrapure water and anhydrous ethanol, the drying temperature is 65° C., and the drying time is 6 hours.
4. The method for preparing the Fe3O4 / Au / Ag composite nanomaterial according to claim 1, characterized in that: The volume ratio of the total amount of ultrapure water, AgNO3 solution and HAuCl4 solution and the sodium citrate solution in S2 is 90mL:10mL:0.8mL, the concentrations of the AgNO3 solution and HAuCl4 solution are both 0.01mol / L, the concentration of the sodium citrate solution is 0.1mol / L, and the time for full reaction is 40min.
5. The method for preparing the Fe3O4 / Au / Ag composite nanomaterial according to claim 1, characterized in that: The mass volume ratio of Fe3O4, ultrapure water and polyethyleneimine solution in S3 is 0.1010g:20mL:20mL, and the concentration of the polyethyleneimine solution is 5mg / mL.
6. The method for preparing the Fe3O4 / Au / Ag composite nanomaterial according to claim 5, characterized in that: The method of adding the polyethyleneimine solution in batches in S3 is: adding 5 mL of the polyethyleneimine solution every 10 minutes.
7. The method for preparing the Fe3O4 / Au / Ag composite nanomaterial according to claim 1, characterized in that: The ultrasonic time in S3 is 20 minutes, the stirring speed is 300 r / min, and the detergent used for the washing is ultrapure water.
8. The method for preparing the Fe3O4 / Au / Ag composite nanomaterial according to claim 1, characterized in that: The mass volume ratio of the surface amino-treated Fe3O4 and Au-AgNPs described in S4 is 0.02 g:20 mL.
9. The method for preparing the Fe3O4 / Au / Ag composite nanomaterial according to claim 1, characterized in that: The stirring speed in S4 is 200 r / min, the washing method is alternating washing with ultrapure water and anhydrous ethanol, the drying temperature is 65° C., and the drying time is 6 h.
10. An application of the Fe3O4 / Au / Ag composite nanomaterial according to any one of claims 1 to 9, characterized in that: The Fe3O4 / Au / Ag composite nanomaterial is used for detecting levofloxacin.