Bidirectional PE stretch film as well as preparation method and application thereof
By using a three-layer structure and modified talc additives, the problems of insufficient mechanical and barrier properties of biaxially oriented polyethylene film were solved, resulting in a biaxially oriented PE film with high strength, wear resistance, and good processing performance.
Patent Information
- Application Number
- CN202411311783.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-20
AI Technical Summary
Biaxially oriented polyethylene film has shortcomings in terms of mechanical properties, abrasion resistance and barrier properties, and is also complex to process and has poor environmental adaptability.
The biaxially oriented PE stretch film adopts a three-layer structure: an outer TPU film, a middle matte PE film, and an inner milky white PE film. The interfacial bonding and compatibility are improved by a composite additive composed of modified talc powder and polytetrafluoroethylene micro powder. The stretching and compounding are carried out in combination with an optimized process flow.
It significantly improves tensile strength, elongation at break, and puncture resistance, while also enhancing oxygen barrier properties and processability, ensuring consistent film performance.
Smart Images

Figure BDA0005050871250000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyethylene film materials, and in particular relates to a bidirectional PE stretch film and a preparation method and application thereof. Background Art
[0002] Polyethylene film (PE film) is a widely used plastic film made of polyethylene resin with good moisture resistance, chemical resistance, insulation and oil resistance. Polyethylene film can be divided into various types such as low-density polyethylene (LDPE) and high-density polyethylene (HDPE) according to different densities, and each type has its own unique performance characteristics. LDPE film has good transparency, is soft and easy to heat seal, while HDPE film has higher mechanical strength and heat resistance. Polyethylene film is widely used in the packaging industry because of its advantages such as lightness, transparency, flexibility, wear resistance and corrosion resistance. It can be used for the packaging of various products such as food, medicine, cosmetics, daily necessities, etc., to protect the products from external pollution and oxidation, and extend the shelf life of the products. In addition, polyethylene film can also be used in agricultural covering, building waterproofing and other fields.
[0003] Biaxial stretching is a widely used orientation processing method. By stretching the film in both the longitudinal and transverse directions, the mechanical properties, optical properties, heat resistance and gas barrier properties of the material can be significantly improved. Biaxially oriented polyethylene (BOPE) film is a new type of packaging material emerging in the film industry in recent years. It has many excellent properties, making it a major type of polyolefin film material in the field of flexible packaging.
[0004] Although biaxially oriented polyethylene (BOPE) film has many excellent properties, it still has some disadvantages, such as limited mechanical properties, poor wear resistance and scratch resistance, insufficient barrier properties, poor heat sealing performance, processing complexity and poor environmental adaptability. Therefore, it is necessary to provide a biaxial PE stretched film with excellent mechanical properties such as wear resistance and tensile resistance. Summary of the invention
[0005] In order to solve the problems existing in the prior art, the object of the present invention is to provide a bidirectional PE stretch film and a preparation method and application thereof.
[0006] The technical solution of the present invention is:
[0007] A bidirectional PE stretch film, consisting of an outer layer, a middle layer and an inner layer:
[0008] The outer layer is a TPU film, including 70-80 parts of TPU particles, 0.2-0.4 parts of ultraviolet absorber, and 0.1-0.3 parts of antioxidant;
[0009] The middle layer is a matte PE film, including 40-60 parts of low-density polyethylene, 20-30 parts of linear low-density polyethylene, 10-15 parts of metallocene polyethylene, 2-6 parts of composite additives, 1-3 parts of polyphthalamide, 0.3-0.5 parts of dispersant, and 0.2-0.5 parts of antioxidant;
[0010] The inner layer is a milky white PE film, which includes 60 to 70 parts of low-density polyethylene, 20 to 25 parts of high-density polyethylene, and 1 to 5 parts of titanium dioxide.
[0011] Further, the outer layer is a TPU film, including 75 parts of TPU particles, 0.3 parts of ultraviolet absorber, and 0.2 parts of antioxidant;
[0012] The middle layer is a matte PE film, including 50 parts of low-density polyethylene, 25 parts of linear low-density polyethylene, 12 parts of metallocene polyethylene, 4 parts of composite additives, 2 parts of polyphthalamide, 0.4 parts of dispersant, and 0.3 parts of antioxidant;
[0013] The inner layer is a milky white PE film, which includes 65 parts of low-density polyethylene, 22 parts of high-density polyethylene, and 3 parts of titanium dioxide.
[0014] Furthermore, the composite auxiliary agent in the middle matte PE film is composed of modified talcum powder and polytetrafluoroethylene powder in a weight ratio of 2 to 4:1, preferably 3:1.
[0015] Furthermore, the preparation method of the modified talcum powder in the middle-layer matte PE film composite additive comprises the following steps:
[0016] S1, dissolving nano talcum powder in ethanol solution and using a magnetic stirrer to stir and disperse to obtain a nano talcum powder dispersion for later use;
[0017] S2, taking the composite modifier and stirring and dissolving it in anhydrous ethanol, heating and stirring in a water bath to obtain a composite modifier solution for standby use;
[0018] S3, slowly pouring the composite modifier solution obtained in step S2 into the nano-talc powder dispersion obtained in step S1, heating and stirring to react, and then washing and drying to obtain.
[0019] Furthermore, the concentration of the ethanol solution in step S1 is 75%, and the mass volume ratio of the added amount of the nano talc powder and the ethanol solution is 12-15 g:100 mL.
[0020] Furthermore, the mass concentration of the composite modifier solution in step S2 is 1.5-2.5%; the amount of the composite modifier added in step S2 is 5-8% of the weight of the nano talc powder, and the composite modifier is composed of sodium myristate and silane coupling agent KH-570 in a weight ratio of 2-3:1, preferably 2.5:1.
[0021] Furthermore, in step S2, the water bath heating temperature is 40-50° C., the stirring time is 20-30 min, and the stirring speed is 500-800 r / min.
[0022] Furthermore, in step S3, the heating temperature is 60-90° C., the reaction is stirred for 2-3 hours, the stirring speed is 2000-2500 r / min, the mixture is washed with anhydrous ethanol 2-3 times, and the washed modified talc is dried at 100° C. for 2 hours.
[0023] Furthermore, the dispersant in the middle-layer matte PE film is polyethylene wax and methyl stearate in a weight ratio of 1 to 3:1, preferably 2:1.
[0024] Furthermore, the ultraviolet absorber in the outer TPU film is one of ultraviolet absorber UV-326 and ultraviolet absorber UV-24.
[0025] Furthermore, the antioxidant in the outer layer and the middle layer is one of antioxidant 168, antioxidant 1076, and antioxidant 330.
[0026] The present invention also provides a method for preparing a bidirectional PE stretch film, comprising the following steps:
[0027] (1) adding the raw materials of the outer layer, the middle layer and the inner layer into a high-speed heating mixer, and mixing at high speed to obtain the outer layer, the middle layer and the inner layer mixtures respectively;
[0028] (2) respectively extruding the outer layer, middle layer and inner layer mixtures obtained in step (1) through a twin-screw extruder and cooling them through a cooling roller to form a gel sheet, wherein the extruder temperature is 200 to 220° C. and the cooling roller temperature is 30 to 40° C.;
[0029] (3) preheating the gel sheet obtained in step (2) in a biaxial stretching machine, and then performing step-by-step stretching, first longitudinal stretching, then transverse stretching, and after the stretching is completed, performing heat setting treatment;
[0030] (4) The middle matte PE film is then printed and double corona treated, and a polyurethane adhesive is evenly coated on one side of the outer film and the middle film using a doctor blade coater. The three layers of film are then aligned and composite cured using the polyurethane adhesive to obtain the result.
[0031] Furthermore, the temperature in the heating mixer in step (1) is 80-90° C., the rotation speed is 1500-2000 r / min, and the stirring time is 20-30 min.
[0032] Furthermore, in step (2), the temperature of the extruder is 200-220° C., and the temperature of the cooling roller is 30-40° C.;
[0033] Furthermore, in the step (3), the preheating temperature in the biaxial stretching machine is 120-150° C., the stretching temperature for the transverse stretching and the longitudinal stretching is 100-130° C., the stretching ratio is 2-4 times, the stretching speed is 60-100 m / min, and after the stretching is completed, heat setting treatment is carried out at 120-140° C., and the heat setting time is 30-60 s.
[0034] Furthermore, the power density of the corona treatment in step (4) is 30 W / m 2 , processing speed is 300m / min,
[0035] Furthermore, the amount of polyurethane adhesive applied in step (4) is 1.8 to 2.2 g / m 3 .
[0036] Furthermore, in step (4), a doctor blade coater is used to evenly coat the polyurethane adhesive on one side of the outer film and the middle film, and then the three layers of film are aligned and composited by a pressure roller, and the composite pressure is 10 to 30 kg / cm 2 , and then cure at a temperature of 30-40°C for 24-48 hours to obtain the product.
[0037] Furthermore, the thickness of the outer TPU film is 2 filaments, the thickness of the middle matte PE film is 3 filaments, and the thickness of the inner milky white PE film is 2 filaments.
[0038] The present invention provides a bidirectional PE stretch film, which is formed by compounding the outer layer TPU film, the middle layer and the inner layer polyethylene film as basic raw materials through an adhesive, wherein the matte PE film of the middle layer is compounded with polyethylene materials of different proportions, such as low-density polyethylene, linear low-density polyethylene, metallocene polyethylene, etc., so as to improve the tensile strength and elongation at break of the PE film and improve the environmental stress cracking resistance of the prepared PE film.
[0039] The added composite auxiliary agent composed of modified talcum powder and polytetrafluoroethylene powder, wherein the modified talcum powder is modified by a composite modifier composed of sodium myristate and silane coupling agent KH-570, and the condition parameters of each step are strictly controlled, the obtained modified talcum powder can enhance the interfacial bonding force and compatibility between talcum powder and PE matrix, the modified talcum powder can be better dispersed in the PE matrix, and provide additional support points, can effectively improve the mechanical properties of the PE film including tensile strength, tear strength, etc., and improve barrier properties, such as effectively improving oxygen barrier properties, reducing water vapor transmission, etc., when the present invention is prepared by the modified talcum powder and polytetrafluoroethylene powder in a reasonable ratio, the two work synergistically, while maintaining the good mechanical properties of the PE film, its processing performance, wear resistance and puncture resistance can be improved. And a dispersant composed of polyethylene wax and methyl stearate is also added, which can help other additives to be evenly dispersed in the PE matrix during the production process, avoid agglomeration or precipitation, thereby ensuring that the film has better performance consistency.
[0040] Furthermore, the present invention can ensure the optimization of the modification effect by precisely controlling the condition parameters (such as temperature, time, etc.) of the modification step, so that the composite additive can exert its maximum effectiveness in the final product.
[0041] Compared with the prior art, the biaxial PE stretch film and the preparation method thereof provided by the present invention have the following advantages:
[0042] The bidirectional PE stretch film prepared by the present invention effectively improves the tensile strength, elongation at break and puncture resistance of the prepared bidirectional PE stretch film by improving raw materials and optimizing the process flow, and also has excellent processing performance and barrier performance, and can be applied to surface protective films of children's crawling mats, EPE, XPE splicing mat protective films, yoga mat protective films, and protective films including all floor mats. DETAILED DESCRIPTION
[0043] The present invention is further illustrated below through the description of specific implementation methods, but this is not a limitation of the present invention. Those skilled in the art can make various modifications or improvements based on the basic idea of the present invention, but as long as they do not deviate from the basic idea of the present invention, they are all within the protection scope of the present invention.
[0044] In the following examples and comparative examples, reagents not otherwise specified are conventional reagents and can be purchased from conventional reagent production and sales companies. The methods used, unless otherwise specified, are all existing technologies. Information such as some raw material manufacturers is as follows:
[0045] The TPU particles were purchased from Haozheng New Materials Technology (Dongguan) Co., Ltd., with the item number TPU521;
[0046] The CAS number of UV absorber UV-326 is 3896-11-5, and the CAS number of UV absorber UV-24 is 131-53-3;
[0047] The CAS number of antioxidant 168 is 31570-04-4; the CAS number of antioxidant 1076 is 2082-79-3; the CAS number of antioxidant 330 is 1709-70-2;
[0048] Low-density polyethylene (LDPE), item number FB0875, brand LG Chem; linear low-density polyethylene LLDPE, item number 41E710, brand DuPont, purchased from Dongguan Bailing New Materials Co., Ltd.;
[0049] Metallocene polyethylene, DuPont Fusabond E528;
[0050] High-density polyethylene (HDPE), product number DMDA8008, brand Sinopec Fulian;
[0051] Polytetrafluoroethylene powder, item number 05131, was purchased from Dongguan Shenghao Plastic Raw Materials Co., Ltd.;
[0052] The CAS number of sodium myristic acid is 822-12-8; the CAS number of stearic acid is 822-16-2;
[0053] The CAS number of silane coupling agent KH-570 is 2530-85-0;
[0054] The CAS number of polyvinylidene fluoride is 24937-79-9.
[0055] Example 1
[0056] A bidirectional PE stretch film, consisting of an outer layer, a middle layer and an inner layer:
[0057] The outer layer is a TPU film, including 70 parts of TPU particles, 0.2 parts of ultraviolet absorber UV-326, and 0.1 parts of antioxidant 168;
[0058] The middle layer is a matte PE film, including 40 parts of low-density polyethylene, 20 parts of linear low-density polyethylene, 10 parts of metallocene polyethylene, 2 parts of composite additives, 1 part of polyphthalamide, 0.3 parts of dispersant, and 0.2 parts of antioxidant 330;
[0059] The dispersant in the middle matte PE film is polyethylene wax and methyl stearate in a weight ratio of 1:1;
[0060] The inner layer is a milky white PE film, including 60 parts of low-density polyethylene, 20 parts of high-density polyethylene, and 1 part of titanium dioxide. The composite additive in the middle matte PE film is composed of modified talcum powder and polytetrafluoroethylene micropowder in a weight ratio of 2:1.
[0061] The preparation method of the modified talcum powder in the composite auxiliary agent of the middle matte PE film comprises the following steps:
[0062] S1, take 12g of nano talc powder and dissolve it in 100mL of 75% ethanol solution, use a magnetic stirrer to stir and disperse, and obtain a nano talc powder dispersion for use;
[0063] S2, take the composite modifier and stir and dissolve it in anhydrous ethanol, heat it to 40°C in a water bath, stir for 30min, and the stirring speed is 500r / min to obtain a composite modifier solution with a mass concentration of 1.5%, wherein the addition amount of the composite modifier is 8% of the mass of nano talc powder, and the composite modifier is composed of sodium myristate and silane coupling agent KH-570 in a weight ratio of 2:1;
[0064] S3. Slowly pour the composite modifier solution obtained in step S2 into the nano talc dispersion obtained in step S1, stir and react for 3 hours at a temperature of 60° C. and a stirring speed of 2000 r / min, then wash twice with anhydrous ethanol, and dry the washed modified talc at 100° C. for 2 hours to obtain.
[0065] The method for preparing the bidirectional PE stretched film comprises the following steps:
[0066] (1) adding the raw materials of the outer layer, the middle layer and the inner layer into a high-speed heating mixer respectively, stirring at a speed of 1500 r / min for 30 min at a temperature of 80° C. to obtain the outer layer, the middle layer and the inner layer mixture;
[0067] (2) respectively extruding the outer layer, middle layer and inner layer mixtures obtained in step (1) through a twin-screw extruder and cooling them through a cooling roller to form a gel sheet, the extruder temperature is 200° C., and the cooling roller temperature is 30° C.;
[0068] (3) preheating the gel sheet obtained in step (2) to 120° C. in a biaxial stretching machine, and then performing step-by-step stretching, first longitudinal stretching and then transverse stretching; the stretching temperature for the transverse stretching and longitudinal stretching is 100° C., the stretching ratio is 2 times, the stretching speed is 60 m / min, and after the stretching is completed, each film is heat-set at 120° C. for 30 seconds to maintain the shape after stretching;
[0069] (4) Then, the middle matte PE film obtained in step (3) was printed and double corona treated (the corona treatment power density was 30 W / m2 , processing speed is 300m / min), a doctor blade coater is used to evenly coat the polyurethane adhesive on one side of the outer film and the middle film, and the amount of the polyurethane adhesive applied is 1.8g / m 3 Then align the three layers of film and laminate them through the pressure roller. The lamination pressure is 10kg / cm 2 , and then cure at 30°C for 48h to obtain the product.
[0070] The thickness of the outer TPU film is 2 threads, the thickness of the middle matte PE film is 3 threads, and the thickness of the inner milky white PE film is 2 threads.
[0071] Example 2
[0072] A bidirectional PE stretch film, consisting of an outer layer, a middle layer and an inner layer:
[0073] The outer layer is a TPU film, including 75 parts of TPU particles, 0.3 parts of ultraviolet absorber UV-326, and 10760.2 parts of antioxidant;
[0074] The middle layer is a matte PE film, including 50 parts of low-density polyethylene, 25 parts of linear low-density polyethylene, 12 parts of metallocene polyethylene, 4 parts of composite additives, 2 parts of polyphthalamide, 0.4 parts of dispersant, and 0.3 parts of antioxidant 1076;
[0075] The dispersant in the middle matte PE film is polyethylene wax and methyl stearate in a weight ratio of 2.5:1;
[0076] The inner layer is a milky white PE film, which includes 65 parts of low-density polyethylene, 22 parts of high-density polyethylene, and 3 parts of titanium dioxide.
[0077] The composite auxiliary agent in the middle-layer matte PE film is composed of modified talcum powder and polytetrafluoroethylene powder in a weight ratio of 3:1.
[0078] The preparation method of the modified talcum powder in the composite auxiliary agent of the middle matte PE film comprises the following steps:
[0079] S1, take 13g of nano talc powder and dissolve it in 100mL of 75% ethanol solution, use a magnetic stirrer to stir and disperse, and obtain a nano talc powder dispersion for use;
[0080] S2, take the composite modifier and stir and dissolve it in anhydrous ethanol, heat it to 45 ° C in a water bath, stir for 25 minutes, and the stirring speed is 700r / min to obtain a composite modifier solution with a mass concentration of 2.0%, wherein the addition amount of the composite modifier is 9% of the mass of nano talc powder, and the composite modifier is composed of sodium myristate and silane coupling agent KH-570 in a weight ratio of 2.5:1;
[0081] S3. Slowly pour the composite modifier solution obtained in step S2 into the nano talc dispersion obtained in step S1, stir and react for 2.5 hours at a temperature of 80° C. and a stirring speed of 2200 r / min, then wash twice with anhydrous ethanol, and dry the washed modified talc at 100° C. for 2 hours to obtain.
[0082] The method for preparing the bidirectional PE stretched film comprises the following steps:
[0083] (1) adding the raw materials of the outer layer, the middle layer and the inner layer into a high-speed heating mixer respectively, stirring at a temperature of 85° C. and a speed of 1800 r / min for 25 min to obtain the outer layer, the middle layer and the inner layer mixture;
[0084] (2) extruding the outer layer, middle layer and inner layer mixtures obtained in step (1) through a twin-screw extruder and cooling them through a cooling roller to form a gel sheet, the extruder temperature is 210° C., and the cooling roller temperature is 35° C.;
[0085] (3) preheating the gel sheet obtained in step (2) to 130° C. in a biaxial stretching machine, and then performing step-by-step stretching, first longitudinal stretching and then transverse stretching; the stretching temperature for the transverse stretching and longitudinal stretching is 120° C., the stretching ratio is 3 times, the stretching speed is 80 m / min, and after the stretching is completed, each film is heat-set at 135° C. for 50 seconds to maintain the shape after stretching;
[0086] (4) Then, the middle matte PE film obtained in step (3) was printed and double corona treated (the corona treatment power density was 30 W / m 2 , processing speed is 300m / min), a doctor blade coater is used to evenly coat the polyurethane adhesive on one side of the outer film and the middle film, and the amount of the polyurethane adhesive applied is 2.0g / m 3 Then align the three layers of film and laminate them through the pressure roller. The lamination pressure is 20kg / cm 2 , and then cured at 35°C for 36 hours to obtain the product.
[0087] The thickness of the outer TPU film is 2 threads, the thickness of the middle matte PE film is 3 threads, and the thickness of the inner milky white PE film is 2 threads.
[0088] Example 3
[0089] A bidirectional PE stretch film, consisting of an outer layer, a middle layer and an inner layer:
[0090] The outer layer is a TPU film, including 80 parts of TPU particles, 0.4 parts of ultraviolet absorber UV-24, and 0.3 parts of antioxidant 330;
[0091] The middle layer is a matte PE film, including 60 parts of low-density polyethylene, 30 parts of linear low-density polyethylene, 15 parts of metallocene polyethylene, 6 parts of composite additives, 3 parts of polyphthalamide, 0.5 parts of dispersant, and 0.5 parts of antioxidant 168;
[0092] The dispersant in the middle matte PE film is polyethylene wax and methyl stearate in a weight ratio of 3:1;
[0093] The inner layer is a milky white PE film, which includes 70 parts of low-density polyethylene, 25 parts of high-density polyethylene, and 5 parts of titanium dioxide.
[0094] The composite auxiliary agent in the middle-layer matte PE film is composed of modified talcum powder and polytetrafluoroethylene powder in a weight ratio of 4:1.
[0095] The preparation method of the modified talcum powder in the composite auxiliary agent of the middle matte PE film comprises the following steps:
[0096] S1, take 15g of nano talc powder and dissolve it in 100mL of 75% ethanol solution, use a magnetic stirrer to stir and disperse, and obtain a nano talc powder dispersion for use;
[0097] S2, take the composite modifier and stir and dissolve it in anhydrous ethanol, heat it to 50°C in a water bath, stir for 20min, and stir at a speed of 800r / min to obtain a composite modifier solution with a mass concentration of 2.5%, wherein the addition amount of the composite modifier is 10% of the mass of the nano talc powder, and the composite modifier is composed of sodium myristate and silane coupling agent KH-570 in a weight ratio of 3:1;
[0098] S3. Slowly pour the composite modifier solution obtained in step S2 into the nano talc dispersion obtained in step S1, stir and react for 2 hours at a temperature of 90° C. and a stirring speed of 2500 r / min, then wash with anhydrous ethanol for 3 times, and dry the washed modified talc at 100° C. for 2 hours to obtain.
[0099] The method for preparing the bidirectional PE stretched film comprises the following steps:
[0100] (1) adding the raw materials of the outer layer, the middle layer and the inner layer into a high-speed heating mixer respectively, stirring at a speed of 2000 r / min for 20 min at a temperature of 90° C. to obtain the outer layer, the middle layer and the inner layer mixture;
[0101] (2) extruding the outer layer, middle layer and inner layer mixtures obtained in step (1) through a twin-screw extruder and cooling them through a cooling roller to form a gel sheet, the extruder temperature is 220° C., and the cooling roller temperature is 40° C.;
[0102] (3) preheating the gel sheet obtained in step (2) to 150° C. in a biaxial stretching machine, and then performing step-by-step stretching, first longitudinal stretching and then transverse stretching; the stretching temperature for the transverse stretching and longitudinal stretching is 130° C., the stretching ratio is 4 times, the stretching speed is 100 m / min, and after the stretching is completed, each film is heat-set at 140° C. for 60 seconds to maintain the shape after stretching;
[0103] (4) Then, the middle matte PE film obtained in step (3) was printed and double corona treated (the corona treatment power density was 30 W / m 2 , processing speed is 300m / min), and a scraper coater is used to evenly coat the polyurethane adhesive on one side of the outer film and the middle film, and the amount of the polyurethane adhesive applied is 2.2g / m 3 Then align the three layers of film and laminate them through the pressure roller. The lamination pressure is 30kg / cm 2 , and then cure at 40°C for 24 hours to obtain the product.
[0104] The thickness of the outer TPU film is 2 threads, the thickness of the middle matte PE film is 3 threads, and the thickness of the inner milky white PE film is 2 threads.
[0105] Comparative Example 1
[0106] Compared with Example 2, the difference is that the metallocene polyethylene in the middle-layer matte PE film is replaced by high-density polyethylene, and the other components and preparation method are the same as those in Example 2.
[0107] Comparative Example 2
[0108] Compared with Example 2, the difference is that in the preparation step S2 of the modified talc, the sodium myristic acid in the composite modifier is replaced by sodium stearate, that is, the composite modifier is composed of sodium stearate and silane coupling agent KH-570 in a weight ratio of 2.5:1. The other components and preparation method are the same as those in Example 2.
[0109] Comparative Example 3
[0110] Compared with Example 2, the difference is that in the preparation step S2 of the modified talc, no sodium myristic acid is added to the composite modifier, and only the silane coupling agent KH-570 is added. The other components and the preparation method are the same as those in Example 2.
[0111] Comparative Example 4
[0112] Compared with Example 2, the difference is that the polytetrafluoroethylene powder in the composite additive of the middle-layer matte PE film is replaced by polyvinylidene fluoride, and the other components and preparation method are the same as those in Example 2.
[0113] Test Example 1: Performance Testing
[0114] 1. Test materials: biaxially stretched PE films prepared in Examples 1 to 3 and Comparative Examples 1 to 4.
[0115] 2. Test method: The tensile strength (MPa), elongation at break (%), puncture resistance (N), water vapor permeability (g / m 2 , 24h).
[0116] The tensile properties test is carried out according to the method in the national standard GB / T1040.2-2022; the puncture resistance is tested according to the method in the national standard GB / T37841-2019; and the water vapor permeability is tested according to the method in the national standard GB / T 26253-2010.
[0117] The test results are shown in Table 1.
[0118] Table 1
[0119]
[0120] As can be seen from Table 1, the biaxial PE stretched films prepared in Examples 1 to 3 have excellent tensile strength, elongation at break and puncture resistance, and at the same time have excellent barrier properties and low water vapor permeability. However, in Comparative Examples 1 to 4, when certain raw materials and preparation methods in the preparation process of the present invention were changed, the various properties of the obtained biaxial PE stretched films were reduced compared with Examples 1 to 3 of the present invention.
[0121] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A bidirectional PE stretch film, characterized in that: It consists of outer layer, middle layer and inner layer: The outer layer is a TPU film, including 70-80 parts of TPU particles, 0.2-0.4 parts of ultraviolet absorber, and 0.1-0.3 parts of antioxidant; The middle layer is a matte PE film, including 40-60 parts of low-density polyethylene, 20-30 parts of linear low-density polyethylene, 10-15 parts of metallocene polyethylene, 2-6 parts of composite additives, 1-3 parts of polyphthalamide, 0.3-0.5 parts of dispersant, and 0.2-0.5 parts of antioxidant; The inner layer is a milky white PE film, which includes 60-70 parts of low-density polyethylene, 20-25 parts of high-density polyethylene, and 1-5 parts of titanium dioxide.
2. The bidirectional PE stretch film according to claim 1, characterized in that: The composite auxiliary agent in the middle-layer matte PE film is composed of modified talcum powder and polytetrafluoroethylene powder in a weight ratio of 2 to 4:
1.
3. The bidirectional PE stretch film according to claim 2, characterized in that: The preparation method of the modified talcum powder comprises the following steps: S1, dissolving nano talcum powder in ethanol solution and using a magnetic stirrer to stir and disperse to obtain a nano talcum powder dispersion for later use; S2, taking the composite modifier and stirring and dissolving it in anhydrous ethanol, heating and stirring in a water bath to obtain a composite modifier solution for standby use; S3, slowly pouring the composite modifier solution obtained in step S2 into the nano-talc powder dispersion obtained in step S1, heating and stirring to react, and then washing and drying to obtain.
4. The bidirectional PE stretched film according to claim 3, characterized in that: The mass concentration of the composite modifier solution in step S2 is 1.5-2.5%; the added amount of the composite modifier in step S2 is 5-8% of the weight of the nano talc powder.
5. The bidirectional PE stretch film according to claim 3, characterized in that: The composite modifier in step S2 is composed of sodium myristate and silane coupling agent KH-570 in a weight ratio of 2 to 3:
1.
6. The bidirectional PE stretched film according to claim 1, characterized in that: The concentration of the ethanol solution in step S1 is 75%, and the mass volume ratio of the nano talc powder and the ethanol solution added is 12-15 g:100 mL; In the step S3, the heating temperature is 60-90° C., the reaction is stirred for 2-3 hours, the stirring speed is 2000-2500 r / min, the modified talc is washed with anhydrous ethanol 2-3 times, and the washed modified talc is dried at 100° C. for 2 hours.
7. The bidirectional PE stretched film according to claim 1, characterized in that: The dispersant in the middle matte PE film is polyethylene wax and methyl stearate in a weight ratio of 1 to 3:1; The ultraviolet absorber in the outer TPU film is one of ultraviolet absorber UV-326 and ultraviolet absorber UV-24; The antioxidant in the outer layer and the middle layer is one of antioxidant 168, antioxidant 1076 and antioxidant 330.
8. A method for preparing a biaxially PE stretched film according to any one of claims 1 to 7, characterized in that: The steps include: (1) adding the raw materials of the outer layer, the middle layer and the inner layer into a high-speed heating mixer, and mixing at high speed to obtain the outer layer, the middle layer and the inner layer mixtures respectively; (2) respectively extruding the outer layer, middle layer and inner layer mixtures obtained in step (1) through a twin-screw extruder and cooling them through a cooling roller to form a gel sheet, wherein the extruder temperature is 200 to 220° C. and the cooling roller temperature is 30 to 40° C.; (3) preheating the gel sheet obtained in step (2) in a biaxial stretching machine, and then performing step-by-step stretching, first longitudinal stretching, then transverse stretching, and after the stretching is completed, performing heat setting treatment; (4) The middle matte PE film is then printed and double corona treated, and a polyurethane adhesive is evenly coated on one side of the outer film and the middle film using a doctor blade coater. The three layers of film are then aligned and composite cured using the polyurethane adhesive to obtain the result.
9. The method for preparing a biaxially PE stretched film according to claim 8, characterized in that: The temperature of the heating mixer in step (1) is 80-90°C, the rotation speed is 1500-2000 r / min, and the stirring time is 20-30 min; the temperature of the extruder in step (2) is 200-220°C, and the temperature of the cooling roller is 30-40°C.
10. The method for preparing a biaxially PE stretched film according to claim 8, characterized in that: In the step (3), the preheating temperature in the biaxial stretching machine is 120-150° C., the stretching temperature of the transverse stretching and the longitudinal stretching is 100-130° C., the stretching ratio is 2-4 times, the stretching speed is 60-100 m / min, and after the stretching is completed, a heat setting treatment is performed at 120-140° C., and the heat setting time is 30-60 s; The amount of polyurethane adhesive applied in step (4) is 1.8 to 2.2 g / m 3 .
Citation Information
Patent Citations
Air bubble film and preparation method thereof
CN107815001A
Co-extrusion stretch film for packaging and preparation process of co-extrusion stretch film
CN117183520A
Puncture-resistant cold stretch film and preparation method thereof
CN118560128A
Directional stretched metallocene polyethylene film and its preparation
CN1252417A
Polyvinylidene chloride resin composition, biaxially stretched film, and method for producing such biaxially stretched film
WO2007013647A1
Cited By
Blowing wear-resistant packaging film for containing liquid bag, preparation method of blowing wear-resistant packaging film and containing liquid bag
CN120269912A
A blown wear-resistant packaging film for a liquid bag and a method for preparing the same and a liquid bag
CN120269912B
Waterproof and coldproof breathable winter glove and preparation method therefor