Method for synthesizing ZSM-5 molecular sieve by taking silica fume as all silicon source and aluminum source
By mixing and stirring and crystallization reaction of microsilicon powder and template agent, the high cost and long-term problems of traditional hydrothermal methods are avoided, and the low-cost and efficient synthesis of ZSM-5 molecular sieve is achieved, which solves the environmental protection of traditional methods and Due to the problem of solid waste utilization, efficient and green ZSM-5 molecular sieve was obtained.
Patent Information
- Application Number
- CN202411145400.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-29
AI Technical Summary
The traditional hydrothermal method of synthesis of ZSM-5 molecular sieve is high cost, has a long crystallization time, is not green and environmentally friendly enough, and cannot effectively utilize industrial solid waste.
Microsilicon powder is used as the entire silicon source and aluminum source. By mixing and stirring with water and template agent, crystallization reaction, washing, drying and calcining are carried out, avoiding the steps of adding silicon source and aluminum source in the traditional method, achieving low Cost and efficient synthesis of ZSM-5 molecular sieve.
It has achieved low-cost, short crystallization time, green and environmentally friendly ZSM-5 molecular sieve synthesis, with high crystallinity, purity and structural stability, suitable for industrial production, and high-value utilization of industrial solid waste.
Smart Images

Figure CN119038574A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of zeolite molecular sieve synthesis and process solid waste resource utilization, and in particular to a method for synthesizing a ZSM-5 molecular sieve using microsilica powder as all silicon and aluminum sources. Background Art
[0002] Microsilicon fume is the main solid waste generated in the manufacturing process of metal silicon and silicon alloy materials. According to some studies, at least 200 kg of silicon fume waste is generated per ton of metal silicon. Such a large amount of silicon fume emissions leads to serious environmental pollution and waste of useful resources. With the increasing awareness of environmental protection and sustainable development, people are exploring the reuse of microsilicon fume instead of traditional disposal solutions.
[0003] ZSM-5 molecular sieve has many unique features in chemical composition, crystal structure and physicochemical properties, and has shown excellent catalytic performance in many organic catalytic reactions. Therefore, it has been more and more widely used in industry and has become a promising new catalyst in petrochemical industry. At present, most ZSM-5 molecular sieves are synthesized by traditional hydrothermal method. Traditional hydrothermal synthesis method refers to a method in which a certain proportion of silicon source, aluminum source, alkali source, water, template agent and other substances are added to a hot autoclave, and ZSM-5 crystals are precipitated by adjusting pressure and temperature. However, the traditional hydrothermal method currently has the disadvantages of high cost, long crystallization time, and lack of green environmental protection. Summary of the invention
[0004] In order to solve the above technical problems, the purpose of the present invention is to provide a method for synthesizing ZSM-5 molecular sieve using microsilica powder as all silicon and aluminum sources, so as to solve the problems of high cost, long crystallization time and lack of green environmental protection in the existing traditional hydrothermal method for synthesizing ZSM-5 molecular sieve.
[0005] The technical solution of the present invention to solve the above technical problems is as follows:
[0006] A method for synthesizing ZSM-5 molecular sieve using microsilica powder as all silicon source and aluminum source comprises the following steps:
[0007] (1) mixing microsilica powder with water and stirring, then adding a template and continuing to stir to obtain a mixed reactant;
[0008] (2) subjecting the mixed reactant obtained in the step to a crystallization reaction, then washing and filtering the solid product after the reaction, and finally drying to obtain a ZSM-5 molecular sieve semi-finished product;
[0009] (3) calcining the ZSM-5 molecular sieve semi-finished product obtained in step (2) to obtain.
[0010] The beneficial effects of the present invention are as follows: the present invention avoids the traditional hydrothermal synthesis method of adding silicon source, aluminum source and alkali source, only uses microsilica powder as raw material, adds a template for crystallization reaction, has low cost, realizes high-value utilization of industrial solid waste, and has the characteristics of green and environmentally friendly production.
[0011] Furthermore, in step (1), the molar ratio of microsilica powder, template and water is 1:0.2-0.3:15-20, and the template is tetrapropylammonium hydroxide.
[0012] Furthermore, in step (1), the molar ratio of microsilica powder, template and water is 1:0.25:18.
[0013] Furthermore, in step (1), the mixing and stirring time is 20-40 minutes; and the stirring time is continued for 2-4 hours.
[0014] Furthermore, in step (2), the temperature of the crystallization reaction is 200-250° C., and the time is 3-24 hours.
[0015] The beneficial effects of adopting the above further technical solution are: the crystallization time is short and the production cycle is short when the method of the present invention is used for preparation, which is conducive to large-scale industrial rapid production.
[0016] Furthermore, in step (2), the drying temperature is 100-150° C. and the drying time is 10-15 hours.
[0017] Furthermore, the calcination temperature in step (3) is 500-600°C and the calcination time is 3-7h.
[0018] Furthermore, in step (3), the calcination temperature is 550° C. and the calcination time is 5 h.
[0019] A ZSM-5 molecular sieve synthesized with microsilica powder as raw material is prepared by adopting the preparation method.
[0020] The above-mentioned ZSM-5 molecular sieve synthesized using microsilica powder as raw material is used in the preparation of petrochemical catalysts.
[0021] The present invention has the following beneficial effects:
[0022] (1) The present invention provides a ZSM-5 synthesis method that is simple to operate, efficient, and low-cost, using microsilica powder as raw material, thereby achieving high-value utilization of industrial solid waste.
[0023] (2) The ZSM-5 sample synthesized by the method of the present invention has high crystallinity, good purity, regular grains, uniform grain size, stable structure, and can be stored for a long time. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1The X-ray diffraction image of the ZSM-5 molecular sieve prepared in Example 4 and the X-ray diffraction image of the standard ZSM-5 molecular sieve;
[0025] Figure 2 This is a scanning electron microscope image of the ZSM-5 molecular sieve prepared in Example 4 and the molecular sieve prepared in Comparative Example 1;
[0026] Figure 3 The nitrogen adsorption curve of the ZSM-5 molecular sieve prepared in Example 4;
[0027] Figure 4 The XRD comparison diagram of the molecular sieve prepared in Comparative Example 1 and the ZSM-5 molecular sieve prepared in Example 5 is shown in FIG. 1 , wherein the red curve is Example 5 and the black curve is Comparative Example 1;
[0028] Figure 5 This is the SEM image of the molecular sieve prepared in Comparative Example 1. DETAILED DESCRIPTION
[0029] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples are only used to explain the present invention and are not used to limit the scope of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0030] Embodiment 1:
[0031] A method for synthesizing ZSM-5 molecular sieve using microsilica powder as raw material comprises the following steps:
[0032] (1) Weigh the raw material microsilica powder, add it into a 50 mL high-temperature reactor sleeve, then add deionized water, stir on a magnetic stirrer, stir for 30 minutes, add the weighed template TPAOH, and continue to stir at room temperature for 3 hours. Finally, after the stirring is completed, put the high-temperature reactor sleeve into a high-pressure reactor, wherein the molar ratio of microsilica powder, TPAOH and deionized water is 1:0.25:18.
[0033] (2) The high-pressure reactor was placed in an oven and subjected to a crystallization reaction at 210° C. for 12 h. After the reaction, the solid product was washed and filtered three times. The filtered product was dried in an oven at 120° C. for 12 h to obtain a ZSM-5 molecular sieve semi-finished product.
[0034] (3) The semi-finished ZSM-5 molecular sieve was placed in a muffle furnace and calcined at 550° C. for 5 h to remove the TPAOH template and obtain the ZSM-5 molecular sieve.
[0035] Embodiment 2:
[0036] A method for synthesizing ZSM-5 molecular sieve using microsilica powder as raw material comprises the following steps:
[0037] (1) Weigh the raw material microsilica powder, add it into a 50 mL high-temperature reactor sleeve, then add deionized water, stir on a magnetic stirrer, stir for 30 minutes, add the weighed template TPAOH, and continue to stir at room temperature for 3 hours. Finally, after the stirring is completed, put the high-temperature reactor sleeve into a high-pressure reactor, wherein the molar ratio of microsilica powder, TPAOH and deionized water is 1:0.25:18.
[0038] (2) The high-pressure reactor was placed in an oven and subjected to a crystallization reaction at 210° C. for 24 h. After the reaction, the solid product was washed and filtered three times. The filtered product was dried in an oven at 120° C. for 12 h to obtain a ZSM-5 molecular sieve semi-finished product.
[0039] (3) The semi-finished ZSM-5 molecular sieve was placed in a muffle furnace and calcined at 550° C. for 5 h to remove the TPAOH template and obtain the ZSM-5 molecular sieve.
[0040] Embodiment 3:
[0041] A method for synthesizing ZSM-5 molecular sieve using microsilica powder as raw material comprises the following steps:
[0042] (1) Weigh the raw material microsilica powder, add it into a 50 mL high-temperature reactor sleeve, then add deionized water, stir on a magnetic stirrer, stir for 30 minutes, add the weighed template TPAOH, and continue to stir at room temperature for 3 hours. Finally, after the stirring is completed, put the high-temperature reactor sleeve into a high-pressure reactor, wherein the molar ratio of microsilica powder, TPAOH and deionized water is 1:0.25:18.
[0043] (2) The high-pressure reactor was placed in an oven and subjected to a crystallization reaction at 240° C. for 3 h. After the reaction, the solid product was washed and filtered for 3 times. The filtered product was dried in an oven at 120° C. for 12 h to obtain a ZSM-5 molecular sieve semi-finished product.
[0044] (3) The semi-finished ZSM-5 molecular sieve was placed in a muffle furnace and calcined at 550° C. for 5 h to remove the TPAOH template and obtain the ZSM-5 molecular sieve.
[0045] Embodiment 4:
[0046] A method for synthesizing ZSM-5 molecular sieve using microsilica powder as raw material comprises the following steps:
[0047] (1) Weigh the raw material microsilica powder, add it into a 50 mL high-temperature reactor sleeve, then add deionized water, stir on a magnetic stirrer, stir for 30 minutes, add the weighed template TPAOH, and continue to stir at room temperature for 3 hours. Finally, after the stirring is completed, put the high-temperature reactor sleeve into a high-pressure reactor, wherein the molar ratio of microsilica powder, TPAOH and deionized water is 1:0.25:18.
[0048] (2) The high-pressure reactor was placed in an oven and subjected to a crystallization reaction at 240° C. for 6 h. After the reaction, the solid product was washed and filtered for 3 times. The filtered product was dried in an oven at 120° C. for 12 h to obtain a semi-finished ZSM-5 molecular sieve.
[0049] (3) The semi-finished ZSM-5 molecular sieve was placed in a muffle furnace and calcined at 550° C. for 5 h to remove the TPAOH template and obtain the ZSM-5 molecular sieve.
[0050] Embodiment 5:
[0051] A method for synthesizing ZSM-5 molecular sieve using microsilica powder as raw material comprises the following steps:
[0052] (1) Weigh the raw material microsilica powder, add it into a 50 mL high-temperature reactor sleeve, then add deionized water, stir on a magnetic stirrer, stir for 30 minutes, add the weighed template TPAOH, and continue to stir at room temperature for 3 hours. Finally, after the stirring is completed, put the high-temperature reactor sleeve into a high-pressure reactor, wherein the molar ratio of microsilica powder, TPAOH and deionized water is 1:0.25:18.
[0053] (2) The high-pressure reactor was placed in an oven and subjected to a crystallization reaction at 240° C. for 12 h. After the reaction, the solid product was washed and filtered three times. The filtered product was dried in an oven at 120° C. for 12 h to obtain a ZSM-5 molecular sieve semi-finished product.
[0054] (3) The semi-finished ZSM-5 molecular sieve was placed in a muffle furnace and calcined at 550° C. for 5 h to remove the TPAOH template and obtain the ZSM-5 molecular sieve.
[0055] Embodiment 6:
[0056] A method for synthesizing ZSM-5 molecular sieve using microsilica powder as raw material comprises the following steps:
[0057] (1) Weigh the raw material microsilica powder, add it into a 50 mL high-temperature reactor sleeve, then add deionized water, stir on a magnetic stirrer, stir for 30 minutes, add the weighed template TPAOH, and continue to stir at room temperature for 3 hours. Finally, after the stirring is completed, put the high-temperature reactor sleeve into a high-pressure reactor, wherein the molar ratio of microsilica powder, TPAOH and deionized water is 1:0.25:18.
[0058] (2) The high-pressure reactor was placed in an oven and subjected to a crystallization reaction at 240° C. for 24 h. After the reaction, the solid product was washed and filtered three times. The filtered product was dried in an oven at 120° C. for 12 h to obtain a ZSM-5 molecular sieve semi-finished product.
[0059] (3) The semi-finished ZSM-5 molecular sieve was placed in a muffle furnace and calcined at 550° C. for 5 h to remove the TPAOH template and obtain the ZSM-5 molecular sieve.
[0060] Comparative Example 1:
[0061] A method for synthesizing a ZSM-5 molecular sieve using TEOS as a raw material comprises the following steps:
[0062] (1) Weigh silicon source tetraethoxysilane (TEOS) and aluminum source NaAlO2, add them into a 50 mL high-temperature reactor sleeve, then add deionized water, and stir on a magnetic stirrer. After stirring for 30 min, add weighed TPAOH and continue stirring at room temperature for 3 h. Finally, after stirring, place the high-temperature reactor sleeve into a high-pressure reactor, wherein the molar ratio of TEOS, NaAlO2, TPAOH and deionized water is 1:0.31:0.25:18.
[0063] (2) The high-pressure reactor was placed in an oven and subjected to a crystallization reaction at 240° C. for 12 h. After the reaction, the solid product was washed and filtered three times. The filtered product was dried in an oven at 120° C. for 12 h to obtain a molecular sieve semi-finished product.
[0064] (3) The semi-finished molecular sieve was placed in a muffle furnace and calcined at 550° C. for 5 h to remove the TPAOH template and obtain the final molecular sieve product.
[0065] Test example:
[0066] The ZSM-5 molecular sieve prepared in Example 4 was characterized, the crystal structure was analyzed by X-ray diffractometer, the surface morphology of the ZSM-5 molecular sieve was observed and analyzed by scanning electron microscopy, and the nitrogen adsorption curve was determined by nitrogen adsorption and desorption experiment using BET specific surface area analyzer at liquid nitrogen temperature (77K).
[0067] The experimental results are as follows Figure 1-Figure 3shown.
[0068] according to Figure 1 It can be seen from the experimental results in that the sample prepared in the present invention has the standard characteristic diffraction peak of pure phase ZSM-5 molecular sieve, and the diffraction peak is sharp, indicating that the crystallinity is very high.
[0069] according to Figure 2 It can be seen from the experimental results in that the ZSM-5 molecular sieve prepared in the present invention has a regular grain morphology and uniform size, and has the typical hexagonal flake morphology of the ZSM-5 molecular sieve.
[0070] according to Figure 3 The experimental results show that the specific surface area of ZSM-5 molecular sieve is 356.556m 2 / g; pore volume 0.122cc / g.
[0071] according to Figure 4 , Figure 5 It can be seen from the experimental results that compared with the method provided by this patent, the peak value of the crystallization peak of the product of comparative example 1 is low, and the characteristic peak of ZSM-5 disappears; the SEM morphology is significantly different from the morphology of the product of Example 4, and no ZSM-5 molecular sieve is obtained. The product may be a silicon-oxygen aluminum compound and its derivatives. It shows that it is difficult to form a ZSM-5 molecular sieve under this condition, or even if a ZSM-5 molecular sieve is formed, it is converted into other silicon-oxygen compounds. The above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for synthesizing ZSM-5 molecular sieve using microsilica powder as all silicon and aluminum sources, It is characterized in that The following steps are involved: (1) mixing microsilica powder with water and stirring, then adding a template and continuing to stir to obtain a mixed reactant; (2) subjecting the mixed reactant obtained in the step to a hydrothermal crystallization reaction, then washing and filtering the solid product after the reaction, and finally drying to obtain a ZSM-5 molecular sieve semi-finished product; (3) calcining the ZSM-5 molecular sieve semi-finished product obtained in step (2) to obtain.
2. The method for synthesizing ZSM-5 molecular sieve using microsilica powder as all silicon source and aluminum source according to claim 1, It is characterized in that In the step (1), the molar ratio of microsilica powder, template and water is 1:0.2-0.3:15-20, and the template is tetrapropylammonium hydroxide.
3. The method for synthesizing ZSM-5 molecular sieve using microsilica powder as all silicon source and aluminum source according to claim 2, It is characterized in that In the step (1), the molar ratio of microsilica powder, template and water is 1:0.25:
18.
4. The method for synthesizing ZSM-5 molecular sieve using microsilica powder as all silicon source and aluminum source according to claim 1, It is characterized in that The mixing and stirring time in step (1) is 20-40 minutes; the stirring time is continued for 2-4 hours.
5. The method for synthesizing ZSM-5 molecular sieve using microsilica powder as all silicon source and aluminum source according to claim 1, It is characterized in that The temperature of the hydrothermal crystallization reaction in step (2) is 200-250° C. and the time is 3-24 hours.
6. The method for synthesizing ZSM-5 molecular sieve using microsilica powder as all silicon source and aluminum source according to claim 1, It is characterized in that The drying temperature in step (2) is 100-150° C. and the drying time is 10-15 hours.
7. The method for synthesizing ZSM-5 molecular sieve using microsilica powder as all silicon source and aluminum source according to claim 1, It is characterized in that The calcination temperature in step (3) is 500-600°C and the calcination time is 3-7h.
8. The method for synthesizing ZSM-5 molecular sieve using microsilica powder as all silicon source and aluminum source according to claim 7, It is characterized in that The calcination temperature in step (3) is 550° C. and the calcination time is 5 hours.
9. A method for synthesizing ZSM-5 molecular sieve using microsilica powder as all silicon and aluminum sources. It is characterized in that The method is prepared by the method according to any one of claims 1 to 8.
10. Use of the ZSM-5 molecular sieve synthesized with microsilica powder as all silicon and aluminum sources as claimed in claim 9 in the preparation of petrochemical catalysts.
Citation Information
Patent Citations
Method for synthesizing ZSM-5 molecular sieve by using silica fume
CN105984885A
Method for solid-phase synthesis of ZSM-5 molecular sieve by using silica fume
CN106006670A
Seed-crystal-free rapid aging crystallization synthesis method of ZSM-5 micro-mesoporous molecular sieve
CN114229865A
Non-adhesive molecular sieve catalyst and preparation method therefor
WO2012024896A1
Cited By
Method for preparing ZSM-5 molecular sieve by utilizing industrial solid waste silica fume and application of ZSM-5 molecular sieve
CN122144757A