Lightweight porous ecological reef-based material and preparation method thereof
By optimizing the component ratio and process flow of artificial reef base materials, combined with glass fiber and shell powder, the problem of large proportion and insufficient durability of artificial reef base materials in the existing technology is solved, and the specific gravity, high durability and ecological results are achieved. Lightweight porous ecological reef base materials with good properties adapt to the marine environment and promote ecological balance and biodiversity.
Patent Information
- Application Number
- CN202410925451.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-29
AI Technical Summary
The existing artificial reef foundation materials have a large proportion, insufficient corrosion resistance of seawater and insufficient ecology, making them difficult to arrange and position in the ocean, and have low resource utilization, which has problems of insufficient durability and strength.
Using lightweight porous ecological reef base materials, including gelling materials, alkali triggers, aggregates, foaming materials and water, the gelling materials are composed of cement, slag powder and fly ash, and glass fiber and shell powder are added to optimize Component ratio and process flow improve the specific gravity, durability and ecology of materials, reduce the amount of cement, and enhance the bioenrichment ability.
Artificial reef base materials with light specific gravity, strong seawater corrosion resistance and high structural strength have been achieved to adapt to the marine environment, promote ecosystem balance and biodiversity, simplify preparation processes, improve production efficiency, and reduce negative impacts on marine ecology.
Smart Images

Figure CN119038915A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of artificial reef foundations, and in particular to a lightweight porous ecological reef foundation material and a preparation method thereof. Background Art
[0002] As global temperatures continue to rise, coral reefs are facing multiple environmental pressures such as illegal dredging, overfishing, aquaculture pollution, and coastal engineering, which have led to serious bleaching and degradation. According to research by authoritative organizations, more than 15% of the world's coral reefs have been damaged and are even at risk of disappearing by the end of this century. The degradation of coral reefs poses a serious threat to marine life, fishery resources, coastal safety, and even global climate stability. Therefore, protecting coral reefs and curbing their degradation has become an important task in maintaining the balance of the earth's ecosystem and the sustainable development of mankind.
[0003] At the same time, with the rapid advancement of urbanization and industrialization, the generation of a large amount of construction waste and fly ash, as well as the increasing amount of slag emissions, have become environmental issues that need to be urgently addressed. The output of fly ash and slag from industrial enterprises has also shown an increasing trend year by year. The utilization rate of slag and fly ash is only about 70%, and the remaining large amount of waste is mostly piled up for treatment. This treatment method is not only a huge waste of resources, but also poses a serious threat to human health and the environment. Harmful substances in slag and fly ash may seep into the soil and groundwater, causing long-term damage to the ecosystem.
[0004] Although the prior art discloses the technology of preparing artificial reef foundation using slag and fly ash, the specific gravity of the artificial reef foundation product may be too large, which is not conducive to its layout and positioning in the ocean. There are still problems such as insufficient durability, insufficient strength, and insufficient ecology of the artificial reef foundation. How to take into account the above-mentioned performances and utilize the resources of construction waste is a technical problem that urgently needs to be solved in this field. Summary of the invention
[0005] The present invention provides a lightweight porous ecological reef base material and a preparation method thereof. Currently, artificial reef bases have the problems of large specific gravity, insufficient seawater corrosion resistance, and insufficient ecology, and are difficult to arrange and position in the ocean. The artificial reef base provided by the present invention has the advantages of light specific gravity, strong seawater corrosion resistance and high structural strength, and the porous structure is also conducive to biological enrichment.
[0006] In order to solve the above technical problems, one of the purposes of the present invention is to provide a lightweight porous ecological reef-based material, including a cementitious material, an alkali activator, an aggregate, a foaming material, an additive and water; the cementitious material includes 20wt%-40wt% cement, 30wt%-60wt% slag powder and 20wt%-40wt% fly ash; the aggregate includes 30wt%-60wt% sand and gravel and 40wt%-70wt% fine sand; the alkali activator is 4-8wt% of the mass of the cementitious material; the mass ratio of the cementitious material to the aggregate is (3-4):2; the foaming material is formed by stirring and foaming a cement foaming agent and water, and the volume of the foaming material is 10vt%-20vt% of the total volume of the reef-based material; the water is 45wt%-60wt% of the mass of the cementitious material.
[0007] The artificial reef foundation of the present invention adopts slag powder, fly ash and cement as cementitious materials, which can improve the seawater corrosion resistance and structural strength of the artificial reef foundation and save cement consumption. The consumption of slag powder can reduce the waste discharge of slag and improve resource utilization. The foaming material is used to optimize the specific gravity of the artificial reef foundation. The lightweight artificial reef foundation is conducive to layout and positioning in the ocean. At the same time, the inventor studies the use of composite aggregates to meet the lightweight specific gravity requirements while improving the structural strength and durability, so that it can better adapt to the needs of the marine environment. Alkaline materials such as gypsum are not added to avoid the alkalinity increase on the outside of the artificial reef foundation affecting the attachment of microorganisms and the growth of algae. The porous structure is conducive to improving the biological enrichment of the artificial reef foundation, which can promote the balance of the ecosystem and biodiversity.
[0008] As a preferred solution, the reef foundation material also includes glass fiber, and the glass fiber accounts for 0.5wt%-4wt% of the mass of the aggregate.
[0009] The reef base material of the present application further improves the compressive strength and flexural strength by adding glass fiber, so that the strength of the reef base material is improved, and the specific gravity of the reef base material is less affected, which can ensure that the specific gravity of the reef base material is 1.4-1.8g˙cm -3 In the better range.
[0010] As a preferred solution, the cementitious material includes 20wt% cement, 40wt%-60wt% slag powder and 20wt%-40wt% fly ash.
[0011] As a preferred solution, the aggregate includes 40wt%-60wt% sand and gravel and 40wt%-60wt% fine sand.
[0012] The present application can further reduce the specific gravity of the reef foundation material by limiting the proportion of each component in the cementitious material and the aggregate of the reef foundation material, while maintaining a high level of compressive strength and flexural strength.
[0013] As a preferred solution, it also includes construction waste powder and shell powder, and the shell powder is attached to the surface of the artificial reef base.
[0014] The artificial reef base of the present invention is added with construction waste powder as a reinforcing material of the artificial reef base, which can reduce the production cost of the artificial reef base, and can also reduce the large amount of construction waste discarded, so as to realize the recycling of resources and environmental protection. The surface of the artificial reef base is attached with a substance with a high calcium carbonate content such as shell powder, and the artificial reef base itself is porous, which is more conducive to attracting coral polyps to attach and improving biodiversity.
[0015] As a preferred solution, the construction waste powder accounts for 5wt%-15wt% of the mass of the cementitious material, and the shell powder accounts for 2wt%-5wt% of the mass of the cementitious material.
[0016] As a preferred solution, the construction waste powder and shell powder are each independent and have a mesh size of 100-200 meshes.
[0017] As a preferred solution, the auxiliary agent is an accelerating agent and / or an early strength agent.
[0018] As a preferred embodiment, the quick-setting agent and early-strength agent are each independent and are carbonates and / or sulfates.
[0019] As a preferred solution, the additive is 4-8wt% of the cement mass.
[0020] As a preferred solution, the mass ratio of cement foaming agent to water in the foaming material is 1:28-32.
[0021] As a preferred solution, the cement is PO42.5 ordinary Portland cement.
[0022] As a preferred solution, the slag powder is S95 specification Shougang slag powder.
[0023] As a preferred solution, the fly ash is Grade II or above.
[0024] As a preferred embodiment, the alkaline activator is at least one of silicates, aluminates, phosphates, sulfates and carbonates containing alkaline elements.
[0025] As a preferred solution, the length of the glass fiber is 1 cm-3 cm.
[0026] As a preferred solution, the size of the sand and gravel is 1cm-3cm.
[0027] As a preferred embodiment, the cement foaming agent is a polymer foaming agent and / or an animal or plant foaming agent.
[0028] In order to solve the above technical problems, the second object of the present invention is to provide a method for preparing a lightweight porous ecological reef-based material, comprising the following steps:
[0029] (1) mixing cementitious material, alkali activator, additive, glass fiber, aggregate, and construction waste powder to form a mixture;
[0030] (2) mixing a cement foaming agent with water to form foam under the action of a foaming device to obtain a foaming material;
[0031] (3) adding water and foaming material to the mixture and stirring to obtain a foaming slurry;
[0032] (4) applying the shell powder evenly on the inner surface of the mold, pouring the foaming slurry into the mold, smoothing it and evenly sprinkling the shell powder on the surface;
[0033] (5) Curing the material in the mold, and after it is shaped, watering and curing it every day to obtain a lightweight and porous ecological reef base.
[0034] As a preferred solution, in step (5), curing is carried out at a temperature not lower than 10° C. for 7-14 days.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] (1) The present invention uses cement, slag powder and fly ash as main raw materials, which have excellent seawater corrosion resistance and structural strength. The specific gravity of the artificial reef foundation is optimized by foaming materials, which can meet the requirements of sinking in the ocean and not floating at will, and is convenient for its arrangement and positioning in the ocean. At the same time, glass fiber and aggregate are added to improve the durability and structural strength of the artificial reef foundation while ensuring the requirement of lighter specific gravity, so that it can maintain stable performance for a long time in a complex marine environment, better adapt to the needs of the marine environment, simplify the preparation process of the artificial reef foundation, and improve production efficiency and convenience.
[0037] (2) The artificial reef base of the present invention does not contain alkaline materials, which can avoid the alkalinity increase on the outside of the artificial reef base affecting the attachment of microorganisms and the growth of algae, thereby improving the ecology of the artificial reef base and reducing the negative impact on the marine ecology. The surface of the artificial reef base is covered with shell powder with a high calcium carbonate content and is porous in design, which is more conducive to attracting coral polyps to attach and promoting the balance of the ecosystem and biodiversity.
[0038] (3) Considering the large amount of construction waste and slag powder generated and their impact on the environment, the artificial reef foundation raw materials of this application realize the resource utilization of construction waste and slag powder, and effectively convert construction waste and slag powder into raw materials for artificial reef foundation, which can improve the durability and structural strength of the artificial reef foundation, while realizing the recycling of resources and environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1: is a schematic diagram of a preparation process of a lightweight porous ecological reef-based material in an embodiment of the present invention;
[0040] Figure 2 : It is a test site for a lightweight porous ecological reef-based material of the present invention;
[0041] Figure 3 : It is a test sample of a lightweight porous ecological reef-based material of the present invention. DETAILED DESCRIPTION
[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] Example 1
[0044] A lightweight porous ecological reef-based material, comprising a cementitious material, an alkali activator, an accelerating agent, glass fiber, aggregate, construction waste powder, shell powder, a foaming material and water; the cementitious material comprises 20wt% cement, 40wt% slag powder and 40wt% fly ash, the slag powder is S95 Shougang slag powder, the cement is PO42.5 ordinary Portland cement, and the fly ash is Class II fly ash; the mass ratio of water to the cementitious material is 0.6; the alkali activator is sodium silicate, which accounts for 4wt% of the mass of the cementitious material; The quick-setting agent is sodium carbonate, which is 5wt% of the cement mass; the aggregate includes 60wt% sand and gravel and 40wt% fine sand, the mass ratio of cementitious material to aggregate is 3:2, the size of the sand and gravel is 2cm, and the fine sand is ordinary river sand; the glass fiber is 2wt% of the aggregate mass, and the length of the glass fiber is 2cm; the mesh size of construction waste powder and shell powder are both 150 meshes, the construction waste powder is 5wt% of the cementitious material mass, and the shell powder is 2wt% of the cementitious material mass; every 50kg of foaming material foams 1m 3 Volume, the volume of the foamed material after foaming accounts for 20vt% of the total volume of the reef foundation material, the bubble size is 1-2mm, the foamed material includes a cement foaming agent and water in a mass ratio of 1:30, and the cement foaming agent is specifically a polymer cement foaming agent of model TH-IV produced by Anhui Taiheng Machinery Manufacturing Co., Ltd.
[0045] The above-mentioned method for preparing a lightweight porous ecological reef-based material is as follows: Figure 1 As shown, the following steps are included:
[0046] (1) Mix the cementitious material, alkali activator, accelerating agent, early strength agent, glass fiber, aggregate and construction waste powder in a mixing bucket to form a mixture;
[0047] (2) taking a cement foaming agent and mixing it with water under the action of a foaming machine, and forming foam under the action of the foaming machine to obtain a foaming material;
[0048] (3) adding part of the water to the mixture and stirring it twice, adding the foaming material and the remaining water after stirring it evenly, stirring it three times at a speed of 500 revolutions per minute to obtain a foaming slurry containing uniform bubbles;
[0049] (4) Apply the shell powder evenly on the inner surface of the mold, and the mold volume is fixed at 0.004m 3 , pour the foaming slurry into the mold, smooth it and sprinkle shell powder evenly on the surface;
[0050] (5) Maintain the surface at a temperature not lower than 10°C. After it takes shape, water it once a day for 14 days to form a lightweight and porous ecological reef base.
[0051] Example 2
[0052] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 1, except that the cementitious material comprises 20wt% cement, 50wt% slag powder and 30wt% fly ash.
[0053] Example 3
[0054] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 1, except that the cementitious material comprises 20wt% cement, 60wt% slag powder and 20wt% fly ash.
[0055] Example 4
[0056] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 2, except that glass fiber is not added.
[0057] Example 5
[0058] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 2, except that the glass fiber accounts for 0.5wt% of the aggregate mass.
[0059] Example 6
[0060] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 2, except that the glass fiber accounts for 1wt% of the aggregate mass.
[0061] Example 7
[0062] A lightweight porous ecological reef-based material, wherein the steps of the preparation method and the reagents and process parameters used in the steps are the same as those in Example 2, except that the glass fiber accounts for 3wt% of the aggregate mass.
[0063] Example 8
[0064] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 2, except that the glass fiber accounts for 4wt% of the aggregate mass.
[0065] Example 9
[0066] A lightweight porous ecological reef-based material, wherein the steps of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that the volume of the foaming material after foaming accounts for 10vt% of the total volume of the reef-based material.
[0067] Example 10
[0068] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that the aggregate comprises 50wt% sand and gravel and 50wt% fine sand.
[0069] Embodiment 11
[0070] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that the aggregate comprises 40wt% sand and gravel and 60wt% fine sand.
[0071] Example 12
[0072] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that the aggregate comprises 30wt% sand and gravel and 70wt% fine sand.
[0073] Embodiment 13
[0074] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that the cementitious material includes 20wt% cement, 60wt% slag powder and 20wt% fly ash.
[0075] Embodiment 14
[0076] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that the cementitious material includes 30wt% cement, 40wt% slag powder and 30wt% fly ash.
[0077] Embodiment 15
[0078] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that the cementitious material includes 40wt% cement, 30wt% slag powder and 30wt% fly ash.
[0079] Example 16
[0080] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that the cementitious material includes 40wt% cement, 40wt% slag powder and 20wt% fly ash.
[0081] Comparative Example 1
[0082] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 1, except that the cementitious material comprises 20wt% cement and 80wt% fly ash.
[0083] Comparative Example 2
[0084] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 1, except that the cementitious material comprises 20wt% cement, 30wt% slag powder and 50wt% fly ash.
[0085] Comparative Example 3
[0086] An ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that the foaming material is not added.
[0087] Comparative Example 4
[0088] A lightweight porous ecological reef-based material, wherein the steps of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that the volume of the foaming material after foaming accounts for 30vt% of the total volume of the reef-based material.
[0089] Comparative Example 5
[0090] A lightweight porous ecological reef-based material, wherein the steps of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that the volume of the foaming material after foaming accounts for 40vt% of the total volume of the reef-based material.
[0091] Comparative Example 6
[0092] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that no aggregate is added.
[0093] Comparative Example 7
[0094] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that the aggregate comprises 90wt% sand and gravel and 10wt% fine sand.
[0095] Comparative Example 8
[0096] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that the aggregate comprises 70wt% sand and gravel and 30wt% fine sand.
[0097] Comparative Example 9
[0098] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that the aggregate comprises 20wt% sand and gravel and 80wt% fine sand.
[0099] Comparative Example 10
[0100] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that the aggregate comprises 10wt% sand and gravel and 90wt% fine sand.
[0101] Comparative Example 11
[0102] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that the cementitious material includes 50wt% slag powder and 50wt% fly ash.
[0103] Comparative Example 12
[0104] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that the cementitious material includes 60wt% slag powder and 40wt% fly ash.
[0105] Comparative Example 13
[0106] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that the cementitious material includes 70wt% slag powder and 30wt% fly ash.
[0107] Comparative Example 14
[0108] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that the cementitious material includes 10wt% cement, 50wt% slag powder and 40wt% fly ash.
[0109] Comparative Example 15
[0110] A lightweight porous ecological reef-based material, wherein each step of the preparation method and the reagents and process parameters used in each step are the same as those in Example 7, except that the cementitious material includes 10wt% cement, 60wt% slag powder and 30wt% fly ash.
[0111] Performance testing
[0112] 1. Chloride ion penetration test: The chloride ion penetration capacity of the reef base materials prepared in the embodiment and the comparative example at different depths of 10 mm for 28 days was studied by natural immersion in a 3.5% NaCl solution. The experimental method was carried out in accordance with the relevant requirements of JTS / T236-2019 "Technical Specifications for Concrete Testing and Inspection of Water Transport Engineering". The concrete test blocks used met the size requirements of 100 mm × 100 mm × 100 mm. The test results are shown in Table 1 below.
[0113] 2. Flexural strength test: The reef foundation materials prepared in the examples and comparative examples were subjected to a 28d flexural strength test. The flexural test method referred to the national standard GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete". The size of the concrete specimen was 150 mm × 150 mm × 600 mm. The test results are shown in Table 1 below.
[0114] 3. Compressive strength test: The compressive strength test of the reef foundation materials of the embodiment and the comparative example was carried out with reference to the standard of GB / T 50081-2019 "Standard for Test Methods for Mechanical Properties of Ordinary Concrete". The specimen size was 150 mm × 150 mm × 150 mm. The compressive strength test was carried out when the specimens were cured to 28 days of age. The test results are shown in Table 1 below.
[0115] 4. Density test: Refer to GB / T 50080-2016 "Concrete Structure Engineering Construction Quality Acceptance Code" standard to test the density of the reef foundation materials in the embodiment and the comparative example. This application requires the density of the reef foundation material to be 1.4-1.8g˙cm-3 Range, preferably 1.4-1.6g˙cm -3 The test results are shown in Table 1 below.
[0116] Table 1 - Performance test results of the present application examples and comparative examples
[0117]
[0118]
[0119] As shown in Table 1, due to the different proportions of cement, slag powder and fly ash in the cementitious materials in Examples 1-3 and Comparative Examples 1-2, there are also large differences in their flexural strength and compressive strength. When the proportions of cement, slag powder and fly ash in the cementitious materials are in the range of 20wt%: 40wt%-60wt%: 20wt%-40wt%, relatively high flexural strength and compressive strength are obtained, and the density of the prepared reef base material reaches 1.4-1.6g˙cm -3 Within the preferred range, the reef base material has a lighter specific gravity and is not easy to float, and the 10mm chloride ion concentration is below 0.2%, indicating that it has excellent seawater corrosion resistance; however, in Comparative Example 1, due to the lack of added slag powder, the material's seawater corrosion resistance is insufficient, and in Comparative Example 2, due to the excessive amount of fly ash added, the material's compressive strength and flexural strength do not meet the requirements.
[0120] As shown in Table 1, there are differences in compressive strength and flexural strength in Examples 2 and 4-8 due to different glass fiber addition contents. It can be found that with the increase of glass fiber content, the compressive strength and flexural strength of the reef base material gradually increase, and then remain the same, reaching the highest when the glass fiber addition accounts for 3% of the aggregate mass.
[0121] As shown in Table 1, the density and strength of the solutions of Examples 7 and 9 and Comparative Examples 3-5 differ greatly due to the different proportions of the foaming material in the reef base material. The specific gravity of the reef base material without adding the foaming material reaches 1.9 g˙cm -3 In this application, the foaming material is controlled to occupy 10%-20% of the volume of the reef base material, which can ensure that the density reaches 1.4-1.8g˙cm -3 Within the specified range, the specific gravity is relatively light, while the flexural strength and compressive strength can reach a high level.
[0122] As shown in Table 1, the density and strength of the reef base materials in Examples 7, 10-12 and Comparative Examples 6-10 are different due to the different ratios of sand and fine sand in the aggregate. Among them, the mass ratio of sand and fine sand in the aggregate is controlled at 30wt%-60wt%: 40wt%-70wt%, which can ensure that the density of the reef base material is 1.4-1.8g˙cm -3Within the range, further controlling the ratio within the range of 40wt%-60wt%:40wt%-60wt%, can effectively improve the flexural strength and compressive strength of the reef foundation material, and the overall effect is better.
[0123] As shown in Table 1, the density and strength of Examples 7, 14-16 and Comparative Examples 14-15 are different due to the different proportions of cement, slag powder and fly ash in the cementitious material. When the proportions of cement, slag powder and fly ash in the cementitious material are in the range of 20wt%-40wt%, 30wt%-60wt% and 20wt%-30wt%, the density of the reef foundation material is 1.4-1.8g˙cm -3 The flexural strength is above 13MPa and the compressive strength is above 15MPa. However, no cement component is added to the cementitious materials of Comparative Examples 11-12, which leads to a serious decrease in the flexural strength and compressive strength of the reef-based materials, and the density of the prepared reef-based materials is less than 1.4g˙cm -3 , its specific gravity is too light and it is easy to float, which cannot meet the needs of marine applications.
[0124] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. It is particularly pointed out that for those skilled in the art, any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of protection of the present invention.
Claims
1. A lightweight porous ecological reef-based material, characterized in that: It includes a cementitious material, an alkali activator, an aggregate, a foaming material, an additive and water; the cementitious material includes 20wt%-40wt% cement, 30wt%-60wt% slag powder and 20wt%-40wt% fly ash; the aggregate includes 30wt%-60wt% sand and gravel and 40wt%-70wt% fine sand; the alkali activator is 4-8wt% of the mass of the cementitious material; the mass ratio of the cementitious material to the aggregate is (3-4):2; the foaming material is formed by stirring and foaming a cement foaming agent and water, and the volume of the foaming material is 10vt%-20vt% of the total volume of the reef foundation material; the water is 45wt%-60wt% of the mass of the cementitious material.
2. A lightweight porous ecological reef-based material as claimed in claim 1, characterized in that: The reef foundation material also includes glass fiber, and the glass fiber accounts for 0.5wt%-4wt% of the mass of the aggregate.
3. A lightweight porous ecological reef-based material as claimed in claim 1 or 2, characterized in that: It also includes construction waste powder and shell powder, wherein the shell powder is attached to the surface of the artificial reef base; the construction waste powder accounts for 5wt%-15wt% of the mass of the cementitious material, and the shell powder accounts for 2wt%-5wt% of the mass of the cementitious material.
4. A lightweight porous ecological reef-based material as claimed in claim 3, characterized in that: The construction waste powder and shell powder are independent of each other and have a mesh size of 100-200 meshes.
5. A lightweight porous ecological reef-based material as claimed in claim 1 or 2, characterized in that: The auxiliary agent is an accelerating agent and / or an early strength agent; the auxiliary agent accounts for 4-8wt% of the cement mass.
6. A lightweight porous ecological reef-based material as claimed in claim 5, characterized in that: The quick-setting agent and early-strength agent are each independent and are carbonate and / or sulfate.
7. A lightweight porous ecological reef-based material as claimed in claim 1 or 2, characterized in that: The mass ratio of the cement foaming agent to water in the foaming material is 1:28-32.
8. A lightweight porous ecological reef-based material as claimed in claim 1 or 2, characterized in that: Satisfy at least one of the following a)-g): a) The cement is PO42.5 ordinary Portland cement; b) the slag powder is S95 specification Shougang slag powder; c) The fly ash is Grade II or above; d) the alkaline activator is at least one of silicates, aluminates, phosphates, sulfates and carbonates containing alkaline elements; e) the length of the glass fiber is 1 cm-3 cm; f) The size of the sand and gravel is 1cm-3cm; g) The cement foaming agent is a polymer foaming agent and / or an animal or plant foaming agent.
9. A method for preparing a lightweight porous ecological reef-based material according to any one of claims 2 to 8, characterized in that: The following steps are involved: (1) mixing cementitious material, alkali activator, additive, glass fiber, aggregate, and construction waste powder to form a mixture; (2) mixing a cement foaming agent with water to form foam under the action of a foaming device to obtain a foaming material; (3) adding water and foaming material to the mixture and stirring to obtain a foaming slurry; (4) applying the shell powder evenly on the inner surface of the mold, pouring the foaming slurry into the mold, smoothing it and evenly sprinkling the shell powder on the surface; (5) Curing the material in the mold, and after it is shaped, watering and curing it every day to obtain a lightweight and porous ecological reef base.
10. The method for preparing a lightweight porous ecological reef-based material according to claim 9, characterized in that: In step (5), curing is carried out at a temperature not lower than 10° C. for 7 to 14 days.
Citation Information
Cited By
Foam concrete material for artificial fish reef and preparation method thereof
CN122355652A