Jet mortar material based on quinary cementing material and preparation method thereof
By mixing alkali slag, calcium carbide slag with slag with cement and fly ash, five-membered cementitious material is formed, and spray molding technology is used to solve the early strength problems of industrial waste treatment and spray concrete, and the compressive strength and resistance are improved The folding strength realizes the recycling of waste and environmental protection.
Patent Information
- Application Number
- CN202411152225.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
Smart Images

Figure CN119038936A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of building materials, and in particular to a spray mortar material based on five-component cementitious materials and a preparation method thereof. Background Art
[0002] Slag is an industrial byproduct produced during the ironmaking process in a blast furnace. When fly ash replaces cement in equal amounts, the performance of concrete can be optimized. Alkali slag and carbide slag are solid wastes produced in the two core industrial processes of producing soda ash by the ammonia-soda process and producing acetylene by hydrolysis of carbide. Untreated alkali slag and carbide slag solutions may cause the soil to enter a salinized state after a long period of accumulation. The accumulation will lead to the accumulation of harmful trace elements. Long-term infiltration may pollute groundwater resources, and the resulting environmental pollution will greatly endanger the local residents' domestic water and the surrounding ecosystem. As for how to deal with these waste resources, the current main method of "on-site landfill" will not only have an adverse impact on the environment, but also affect the survival of humans, animals and plants.
[0003] Shotcrete is a construction technology that uses a sprayer to spray concrete or cement slurry at high speed onto the target surface. It is characterized by fast construction speed, low cost, and adaptability to complex construction conditions. It is mainly used for support and repair projects, such as underground tunnel lining, dam protective layer, rock wall reinforcement, seismic reinforcement of buildings, etc. Due to its special application, higher requirements are placed on the early strength and setting time of shotcrete.
[0004] Compared with ordinary Portland cement, solid waste-based cementitious materials have finer fineness, higher activity, and lower cost, which is conducive to the recycling of resources. Solid waste-based cementitious materials just meet the requirements of shotcrete for early strength and setting time, which not only improves the working performance and mechanical properties of shotcrete, but also reduces the consumption of natural resources and energy, thereby reducing the project cost performance.
[0005] Therefore, studying how to properly treat and utilize industrial solid waste and apply it to shotcrete will promote environmental protection and the technological development of shotcrete. Summary of the invention
[0006] In view of the problems existing in the prior art, the present invention provides a method for preparing a spray mortar material based on a five-component cementitious material and a spray mortar material, wherein a modified mixture is prepared by mixing alkali slag, carbide slag and slag, and the five-component cementitious material is prepared by mixing with cement and fly ash, and the five-component cementitious material is further processed and sprayed to prepare a spray mortar material based on the five-component cementitious material by spraying, wherein the alkali slag and carbide slag are used as alkali activators to perform alkali excitation treatment on the slag, thereby enhancing the activity of the slag, and secondly the spraying molding method helps the rapid solidification of the mortar material.
[0007] The first aspect of the present invention provides a method for preparing a spray mortar material based on a five-component cementitious material, and the specific steps are as follows:
[0008] S1, preparing alkali slag powder and carbide slag powder: respectively standing the alkali slag slurry and carbide slag slurry for 5-7 days, removing the upper clear liquid and stirring the sediment layer to a wet base state, placing the wet base alkali slag slurry and carbide slag slurry in a drying oven at 60-80° C. for drying, then grinding the dried alkali slag and carbide slag respectively, and sieving with a 200-300 mesh sieve to obtain alkali slag powder and carbide slag powder;
[0009] S2, modification treatment of slag by alkali slag powder and carbide slag powder: the alkali slag powder, the carbide slag powder and the slag of equal mass are mixed evenly, and then put into a horizontal ball mill for dry grinding. After the mixed dry grinding for 30-40 minutes, the mixture is covered with a plastic wrap and allowed to stand for aging for 24-36 hours to obtain a modified alkali slag-carbide slag-slag mixture. The operating frequency of the horizontal ball mill is set to 40-60 Hz, and the speed is set to 250-300 r / min. During the modification treatment, the alkali slag powder and the carbide slag powder are used to introduce Ca(OH)2 into the gelling system. The reaction chemical reaction of the whole system is as follows:
[0010] CaO+H2O→Ca(OH)2
[0011] Ca(OH)2+SiO2+H2O→CaO·SiO2·6-8H2O
[0012] Ca(OH)2+Al2O3+SiO2+Cl - +H2O→2CaO·2Al2O3·4SiO2·5H2O+3CaO·Al2O3·C
[0013] aCl2·10H2O
[0014] Ca(OH)2+Al2O3+Na2O+MgO+SO3+Cl - +H2O+CO2→6MgO·Al2O3·CO2·12H2O+N
[0015] aCl + CaSO4·2H2O + CaCO3;
[0016] S3, preparing a five-component cementitious material: adding the modified alkali slag-carbide slag-slag mixture prepared in step S2, fly ash and cement in a preset mass percentage into a cement mortar mixer and stirring for 30 to 40 seconds to obtain an alkali slag-carbide slag-fly ash-slag-cement five-component cementitious material;
[0017] S4, preparing a mortar preform containing five-component cementitious materials: sequentially adding a first preset amount of machine-made sand, a second preset amount of water, a third preset amount of water-reducing agent, and a fourth preset amount of accelerating agent into a cement mortar mixer containing five-component cementitious materials of alkali slag-calcium carbide slag-fly ash-slag-cement, and stirring each material after adding each material, and finally obtaining a mortar preform containing five-component cementitious materials of alkali slag-calcium carbide slag-fly ash-slag-cement, wherein the machine-made sand, the water, the third preset amount of water-reducing agent, and the fourth preset amount of accelerating agent are added into a cement mortar mixer containing five-component cementitious materials of alkali slag-calcium carbide slag-fly ash-slag-cement. , the mass ratio of the water reducing agent and the quick-setting agent to the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement is 2-4: 0.3-0.5: 0.01-0.02: 0.05-0.07: 1; the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement includes 10-20% alkali slag, 0-10% carbide slag, 0-20% fly ash, 0-20% slag and 50-70% cement in mass percentage;
[0018] S5. Preparation of spray mortar material by spraying and curing: a mortar sprayer is used to spray and cure the mortar preform of the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement prepared in step S4.
[0019] Preferably, step S5 specifically includes the following sub-steps:
[0020] S51, lubricating the mortar pipe of the mortar spraying machine with cement slurry, and then pouring the mortar prefabricated body of the alkali slag-carbide slag-fly ash-slag-cement five-element cementitious material into the injection mortar pump of the mortar spraying machine;
[0021] S52. Adjust the nozzle of the spray gun to form an angle of 40° to 50° with the spray surface of the spray plate, start the mortar sprayer, and the spray mortar pump of the mortar sprayer continuously mixes the mortar preform of the alkali slag-calcium carbide slag-fly ash-slag-cement five-component cementitious material at a rotation speed of 80 to 100 revolutions per minute for 30 to 60 seconds, and then drives the mortar preform of the alkali slag-calcium carbide slag-fly ash-slag-cement five-component cementitious material into the mortar pipeline by air pressure, and sprays the formed spray mortar flow onto the spray plate through the nozzle of the spray gun, and solidifies to form the spray mortar material of the alkali slag-calcium carbide slag-fly ash-slag-cement five-component cementitious material.
[0022] Preferably, in step S4, after adding a first preset amount of machine-made sand, stir at a low speed for 30 to 60 seconds, after adding a second preset amount of water, stir at a low speed for 60 to 90 seconds, after adding a third preset amount of water reducer, stir at a low speed for 30 to 60 seconds and then at a high speed for 30 to 60 seconds, and after adding a fourth preset amount of accelerator, stir at a high speed for 30 to 40 seconds, wherein the rotation speed of the low-speed stirring is 40 to 70 r / min, and the rotation speed of the high-speed stirring is 100 to 150 r / min.
[0023] Preferably, the moisture content of the sedimentary layers of the alkali slag slurry and carbide slag slurry in the wet-based state is 40% to 60%, the drying time of the alkali slag slurry in the wet-based state is 5-7 days, and the drying time of the carbide slag slurry in the wet-based state is 2-3 days.
[0024] Preferably, the specific surface area of the slag is 330 to 370 m 2 / kg, the medium particle size of the specific surface area of the slag is 17-21μm, the cement is PO 42.5 silicate cement, the particle size of the machine-made sand is 0.16-4.75mm, the fineness modulus of the machine-made sand is 2.4-2.8, the mud content of the machine-made sand is ≤1%, the water reducer is a polycarboxylic acid type water reducer and the water reduction rate is ≥15%, the initial setting time of the accelerator is ≤5min and the final setting time is ≤15min, the solid content of the accelerator is 35-45%, and the size of the spray plate is ≥450mm×450mm×120mm.
[0025] Preferably, the alkali residue used in step S1 is prepared from soda ash by an ammonia-soda process, and the reaction process is as follows:
[0026] CaCO3 high temperature CaO+CO2↑
[0027] CaO+H2O=Ca(OH)2
[0028] NaCl+NH3+CO2+H2O=NaHCO3+NH4Cl
[0029] 2NH4Cl+Ca(OH)2=2NH3↑+CaCl2+2H2O
[0030] 2NaHCO3 high temperature Na2CO3+CO2↑+H2O;
[0031] The carbide slag used in step S1 is alkaline waste slag produced in the process of obtaining acetylene gas by hydrolyzing carbide, and the reaction process is as follows:
[0032] CaC2+2H2O=C2H2+Ca(OH)2.
[0033] Preferably, the grinding process in step S1 uses a high-speed crusher with a rotation speed of 25000-30000 r / min, and the cement mortar mixer in step S3 is a planetary cement mortar mixer.
[0034] The second aspect of the present invention provides a method for preparing a spray mortar material based on a five-component cementitious material, wherein the spray mortar material includes a first preset amount of machine-made sand, a second preset amount of water, a third preset amount of a water reducer, a fourth preset amount of an accelerator, and a five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement. The mass ratio of the first preset amount of machine-made sand to the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement is 2 to 4, the mass ratio of the second preset amount of water to the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement is 0.3 to 0.5, the third preset amount of the water reducer is 1 to 2% of the mass of the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement, and the fourth preset amount of the accelerator is 5 to 7% of the mass of the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement.
[0035] Preferably, the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement includes 10-20% alkali slag, 0-10% carbide slag, 0-20% fly ash, 0-20% slag and 50-70% cement in mass percentage.
[0036] Preferably, the sprayed mortar material is subjected to a compressive strength test, and the specific processing process is: the cured spray plate sample is cut and formed into a triple test mold of 40mm×40mm×160mm, and then cured in a standard curing box with a temperature of 20±2℃ and a humidity greater than 95% for 1 day, 7 days and 28 days, and then the compressive strength and flexural strength tests are respectively performed.
[0037] Compared with the prior art, the present invention has the following advantages:
[0038] 1. The spray mortar material based on the five-component cementitious material of the present invention has higher compressive strength than the existing spray mortar material. The 1d compressive strength of the spray mortar specimen of the present invention is as high as 15MPa, and the flexural strength is 3.9MPa; the 28d compressive strength is as high as 52MPa, and the flexural strength is 8.8MPa; the initial setting time is as short as 3min, and the final setting time is as short as 4min30s, which not only shortens the setting time of the spray mortar specimen, but also greatly improves the macro strength of the spray mortar specimen;
[0039] 2. The spray mortar material based on the five-component cementitious material of the present invention reduces the amount of cement by adding alkali slag, carbide slag and slag, and utilizes fly ash to improve the workability of the mortar specimen based on the cementitious material system. The added alkali slag and carbide slag make the whole system alkaline and thus stimulate the hydration reaction between fly ash, slag and cement. Through test analysis, it can be known that the 28d hydration products are mainly hydrated calcium silicate gel and hydrated calcium chloroaluminate crystals. Their joint action and mutual overlap provide a source of strength for the cementitious system.
[0040] 3. The spraying mortar material based on five-component cementitious materials of the present invention comprises alkali slag, carbide slag, slag and fly ash as raw materials. Solid waste-based cementitious materials are used to replace cement in the production of sprayed concrete, thereby reducing the production of silicate cement clinker and making full use of industrial waste residues. At the same time, industrial waste resources can be recycled, waste can be treated with waste, a circular economy can be developed, and environmental pollution can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 It is a flow chart of the preparation method of the spray mortar material based on the five-component cementitious material of the present invention;
[0042] Figure 2 The microscopic morphology of the first part of the 28d hardened slurry of the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement prepared in Example 7 of the present invention is magnified 5000 times;
[0043] Figure 3 The microscopic morphology of the second part of the 28d hardened slurry of the alkali slag-carbide slag-fly ash-slag-cement five-component cementitious material prepared in Example 7 of the present invention is magnified 5000 times;
[0044] Figure 4 The microscopic morphology of the third part of the 28d hardened slurry of the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement prepared in Example 7 of the present invention is magnified 5000 times;
[0045] Figure 5 The X-ray diffraction spectrum of the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement prepared in Example 7 of the present invention with a curing age of 28 days;
[0046] Figure 6 The energy spectrum analysis exploration point location diagram of the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement prepared in Example 7 of the present invention;
[0047] Figure 7 An X-ray energy dispersion spectrum analysis diagram of the detection point 1 of the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement prepared in Example 7 of the present invention;
[0048] Figure 8This is the X-ray energy dispersion spectrum analysis of the probe point 2 of the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement prepared in Example 7 of the present invention. DETAILED DESCRIPTION
[0049] In order to fully describe the technical content, objectives and effects of the present invention, the following will be described in detail with reference to the accompanying drawings.
[0050] The present invention provides a method for preparing a spray mortar material based on a five-component cementitious material. Figure 1 As shown, the specific steps are as follows:
[0051] S1. Let the alkali residue slurry and carbide slag slurry stand for 5-7 days respectively, then remove the upper clear liquid and fully stir the sedimentation layer to a wet base state, put the wet base alkali residue slurry into a drying oven at 60-80°C for drying for 5-7 days, put the wet base carbide slag slurry into a drying oven at 60-80°C for drying for 2-3 days to obtain dry alkali residue and carbide slag, then use a high-speed crusher with a rotation speed of 25000-30000r / min to grind the dried alkali residue and carbide slag for 20-40min, sieve the ground alkali residue and carbide slag with a 200-mesh sieve to obtain alkali residue powder and carbide slag powder, put the alkali residue powder and carbide slag powder into different vacuum sealed bags respectively, and store them in a dry environment for standby use.
[0052] The wet base state is that the moisture content of the sedimentary layer of alkali slag slurry and carbide slag slurry is maintained at 40% to 60%.
[0053] S2, the alkali slag powder prepared in S1 is mixed with carbide slag powder and slag in a mass ratio of 1:1:1 and placed in a horizontal ball mill. The operating frequency of the horizontal ball mill is 40-60Hz, and the speed of the horizontal ball mill is 250r / min. After the mixed dry grinding for 30 minutes, it is covered with plastic wrap and left to age for 24 hours to obtain a modified alkali slag-carbide slag-slag mixture. After aging for 24 hours, the impurities in the alkali slag and carbide slag will dissolve and the precipitation process will tend to equilibrium, and most of the precipitation will be effectively solidified. In this process, the alkali slag and carbide slag are mainly used to introduce Ca(OH)2 into the gelling system. The main reaction chemical equation of the whole system is as follows:
[0054] CaO+H2O→Ca(OH)2
[0055] Ca(OH)2+SiO2+H2O→CaO·SiO2·6-8H2O
[0056] Ca(OH)2+Al2O3+SiO2+Cl - +H2O→2CaO·2Al2O3·4SiO2·5H2O+3CaO·Al2O3·C
[0057] aCl2·10H2O
[0058] Ca(OH)2+Al2O3+Na2O+MgO+SO3+Cl - +H2O+CO2→6MgO·Al2O3·CO2·12H2O+NaCl+CaSO4·2H2O+CaCO3.
[0059] In addition, during the dry grinding process, alkali slag and carbide slag are used as alkaline activators. The alkali slag, carbide slag and slag are evenly mixed and further refined. Through physical activation, that is, refining the particle size of the alkali slag and carbide slag, their hydration activity is further improved to accelerate the hydration rate of the slag, which can achieve the purpose of improving the coagulation and hardening properties of the cementitious material and is more conducive to promoting the hydration reaction of alkali slag, carbide slag and slag.
[0060] S3. Add the alkali slag powder, carbide slag powder, fly ash, slag and cement prepared in S1 into a mortar mixer at a preset mass percentage and stir for 30 to 40 seconds to obtain a five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement.
[0061] The specific surface area of the fly ash selected in step S3 is 310-340m 2 / kg, and the specific surface area of fly ash has a medium particle size of 21-25 μm; the specific surface area of slag is 330-370 m 2 / kg, and the median particle size of the slag specific surface area is 17 to 21 μm.
[0062] S4. Add a first preset amount of machine-made sand into a mortar mixer and stir for 30 to 60 seconds. Add a second preset amount of water into the mortar mixer and stir for 60 to 90 seconds to obtain a mortar mixture of alkali slag-carbide slag-fly ash-slag-cement five-component cementitious material. Add a third preset amount of water reducer into the mortar mixer and stir the mortar mixture of alkali slag-carbide slag-fly ash-slag-cement five-component cementitious material according to a set stirring program. The stirring program is firstly stirring at a low speed of 40 to 70 r / min for 30 to 60 seconds, and then stirring at a high speed of 100 to 150 r / min for 30 to 60 seconds. After the stirring program is completed, add a fourth preset amount of accelerator into the mortar mixer and stir for 30 to 40 seconds to obtain a mortar preform of alkali slag-carbide slag-fly ash-slag-cement five-component cementitious material.
[0063] In addition, fly ash provides fluidity for the cementitious system, the water reducer precipitates water for the system, and the accelerator makes the system solidify quickly. Since the main components of slag, fly ash and cement are the same, solid waste such as slag and fly ash are used to replace cement. The reaction equations of S3 and S4 are the same as the above steps.
[0064] Specifically, the particle size of the machine-made sand used in step S4 is 0.16-4.75 mm, the fineness modulus is 2.4-2.8, the mud content is ≤1%, the water reducer is a polycarboxylic acid type water reducer, and the water reduction rate of the water reducer is greater than or equal to 15%; the initial setting time of the accelerator is ≤5 min, the final setting time is ≤15 min, and the solid content is 35-45%.
[0065] S5. Use a mortar sprayer to spray and solidify the mortar preform of the five-component cementitious material of alkali slag-calcium carbide slag-fly ash-slag-cement. The test mold size of the spray plate is 450mm×450mm×120mm. Lubricate the mortar pipe of the mortar sprayer with cement slurry, and then pour the mortar preform of the five-component cementitious material of alkali slag-calcium carbide slag-fly ash-slag-cement prepared in S4 into the spray mortar pump of the mortar sprayer. Start the mortar sprayer, and the spray mortar pump spirally rotates at a speed of 80 to 100 revolutions per minute to continuously mix the mortar preform of the five-component cementitious material of alkali slag-calcium carbide slag-fly ash-slag-cement for 30 to 60 seconds. The mortar material of alkali slag-calcium carbide slag-fly ash-slag-cement five-element cementitious material driven by air pressure will pass through the mortar pipe and reach the spray gun mouth of the spray machine. The spray gun mouth forms a 45° angle with the large plate spraying surface, and the formed spray mortar flow is sprayed onto the spray plate, and then quickly solidifies and hardens to form the spray mortar material of alkali slag-calcium carbide slag-fly ash-slag-cement five-element cementitious material. Subsequently, the sprayed large plate test mold is cut into the required test piece size and formed in a triple test mold of 40mm×40mm×160mm, and cured in a standard curing box with a temperature of (20±2)℃ and a humidity of more than 95% to 1d, 7d, and 28d.
[0066] The following is a further description of a method for preparing a spray mortar material based on a five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement in combination with an embodiment of the present invention:
[0067] The alkali slag and carbide slag slurry are allowed to stand for 5-7 days, then the upper clear liquid is removed and the sedimentation layer is fully stirred to a wet base state, the alkali slag slurry in the wet base state is placed in a drying oven at 60-80°C for drying for 5-7 days, and the carbide slag slurry in the wet base state is placed in a drying oven at 60-80°C for drying for 2-3 days to obtain dry alkali slag and carbide slag, and then the dried alkali slag and carbide slag are ground by a high-speed crusher, and the ground alkali slag and carbide slag are sieved with a 200-mesh sieve to obtain alkali slag powder and carbide slag powder, the alkali slag powder and carbide slag powder are respectively placed in different vacuum sealed bags and stored in a dry environment for use, and the high-speed crusher is 25000-30000r / min.
[0068] Example 1: Weigh 0.53kg of alkali slag powder, 0.075kg of carbide slag powder, 0.15kg of fly ash, 0.45kg of slag and 0.60kg of cement, add them into a mortar mixer and stir for 30s, then add 9kg of machine-made sand and stir for 45s, then add 1.26kg of water and stir for 75s, then add 0.042kg of water reducer into the mortar mixer, first stir at a low speed of 70r / min for 60s, then stir at a high speed of 150r / min for 60s, finally add 0.18kg of accelerator and stir for 30s to obtain a mortar preform of alkali slag-carbide slag-fly ash-slag-cement five-element cementitious material, and finally obtain mortar specimens with a size of 40mm×40mm×160mm by spray large plate forming. The mortar specimens are cured under standard conditions for 1d, 7d and 28d, which are recorded as sample 1.
[0069] Example 2: Weigh 0.53kg of alkali slag powder, 0.075kg of carbide slag powder, 0.30kg of fly ash, 0.30kg of slag and 0.60kg of cement, add them into a mortar mixer and stir for 30s, then add 9kg of machine-made sand and stir for 45s, then add 1.26kg of water and stir for 75s, then add 0.042kg of water reducer into the mortar mixer, first stir at a low speed of 70r / min for 60s, then stir at a high speed of 150r / min for 60s, finally add 0.18kg of accelerator and stir for 30s to obtain a mortar preform of alkali slag-carbide slag-fly ash-slag-cement five-element cementitious material, and finally obtain mortar specimens with a size of 40mm×40mm×160mm by spray large plate forming. The mortar specimens are cured under standard conditions for 1d, 7d and 28d, which are recorded as sample 2.
[0070] Example 3: Weigh 0.53kg of alkali slag powder, 0.075kg of carbide slag powder, 0.45kg of fly ash, 0.15kg of slag and 0.60kg of cement, add them into a mortar mixer and stir for 30s, then add 9kg of machine-made sand and stir for 45s, then add 1.26kg of water and stir for 75s, then add 0.042kg of water reducer into the mortar mixer, first stir at a low speed of 70r / min for 60s, then stir at a high speed of 150r / min for 60s, finally add 0.18kg of accelerator and stir for 30s to obtain a mortar preform of alkali slag-carbide slag-fly ash-slag-cement five-element cementitious material, and finally obtain mortar specimens with a size of 40mm×40mm×160mm by spray large plate forming. The mortar specimens are cured under standard conditions for 1d, 7d and 28d, which are recorded as sample 3.
[0071] Example 4: Weigh 0.45kg of alkali slag powder, 0.15kg of carbide slag powder, 0.15kg of fly ash, 0.45kg of slag and 0.60kg of cement, add them into a mortar mixer and stir for 30s, then add 9kg of machine-made sand and stir for 45s, then add 1.26kg of water and stir for 75s, then add 0.042kg of water reducer into the mortar mixer, first stir at a low speed of 70r / min for 60s, then stir at a high speed of 150r / min for 60s, finally add 0.18kg of accelerator and stir for 30s to obtain a mortar preform of alkali slag-carbide slag-fly ash-slag-cement five-element cementitious material, and finally obtain mortar specimens with a size of 40mm×40mm×160mm by spray large plate forming. The mortar specimens are cured under standard conditions for 1d, 7d and 28d, which are recorded as sample 4.
[0072] Example 5: Weigh 0.45kg of alkali slag powder, 0.15kg of carbide slag powder, 0.30kg of fly ash, 0.30kg of slag and 0.60kg of cement, add them into a mortar mixer and stir for 30s, then add 9kg of machine-made sand and stir for 45s, then add 1.26kg of water and stir for 75s, then add 0.042kg of water reducer into the mortar mixer, first stir at a low speed of 70r / min for 60s, then stir at a high speed of 150r / min for 60s, finally add 0.18kg of accelerator and stir for 30s to obtain a mortar preform of alkali slag-carbide slag-fly ash-slag-cement five-element cementitious material, and finally obtain mortar specimens with a size of 40mm×40mm×160mm by spray large plate forming. The mortar specimens are cured under standard conditions for 1d, 7d and 28d, which are recorded as sample 5.
[0073] Example 6: Weigh 0.45kg of alkali slag powder, 0.15kg of carbide slag powder, 0.45kg of fly ash, 0.15kg of slag and 0.60kg of cement, add them into a mortar mixer and stir for 30s, then add 9kg of machine-made sand and stir for 45s, then add 1.26kg of water and stir for 75s, then add 0.042kg of water reducer into the mortar mixer, first stir at a low speed of 70r / min for 60s, then stir at a high speed of 150r / min for 60s, finally add 0.18kg of accelerator and stir for 30s to obtain a mortar preform of alkali slag-carbide slag-fly ash-slag-cement five-element cementitious material, and finally obtain mortar specimens with a size of 40mm×40mm×160mm by spray large plate forming. The mortar specimens are cured under standard conditions for 1d, 7d and 28d, which are recorded as sample 6.
[0074] Example 7: Weigh 0.30kg of alkali slag powder, 0.30kg of carbide slag powder, 0.15kg of fly ash, 0.45kg of slag and 0.60kg of cement, add them into a mortar mixer and stir for 30s, then add 9kg of machine-made sand and stir for 45s, then add 1.26kg of water and stir for 75s, then add 0.042kg of water reducer into the mortar mixer, first stir at a low speed of 70r / min for 60s, then stir at a high speed of 150r / min for 60s, finally add 0.18kg of accelerator and stir for 30s to obtain a mortar preform of alkali slag-carbide slag-fly ash-slag-cement five-element cementitious material, and finally obtain mortar specimens with a size of 40mm×40mm×160mm by spray large plate forming. The mortar specimens are cured under standard conditions for 1d, 7d and 28d, which are recorded as sample 7.
[0075] Example 8: Weigh 0.30kg of alkali slag powder, 0.30kg of carbide slag powder, 0.30kg of fly ash, 0.30kg of slag and 0.60kg of cement, add them into a mortar mixer and stir for 30s, then add 9kg of machine-made sand and stir for 45s, then add 1.26kg of water and stir for 75s, then add 0.042kg of water reducer into the mortar mixer, first stir at a low speed of 70r / min for 60s, then stir at a high speed of 150r / min for 60s, finally add 0.18kg of accelerator and stir for 30s to obtain a mortar preform of alkali slag-carbide slag-fly ash-slag-cement five-element cementitious material, and finally obtain mortar specimens with a size of 40mm×40mm×160mm by spray large plate forming. The mortar specimens are cured under standard conditions for 1d, 7d and 28d, which are recorded as sample 8.
[0076] Example 9: Weigh 0.30kg of alkali slag powder, 0.30kg of carbide slag powder, 0.45kg of fly ash, 0.15kg of slag and 0.60kg of cement, add them into a mortar mixer and stir for 30s, then add 9kg of machine-made sand and stir for 45s, then add 1.26kg of water and stir for 75s, then add 0.042kg of water reducer into the mortar mixer, first stir at a low speed of 70r / min for 60s, then stir at a high speed of 150r / min for 60s, finally add 0.18kg of quick-setting agent and stir for 30s to obtain a mortar preform of alkali slag-carbide slag-fly ash-slag-cement five-element cementitious material, and finally obtain mortar specimens with a size of 40mm×40mm×160mm by spray large plate forming. The mortar specimens are cured under standard conditions for 1d, 7d and 28d, which are recorded as sample 9.
[0077] Comparative Example 1: Weigh 0.53kg of alkali slag powder, 0.075kg of carbide slag powder, 0.60kg of slag powder and 1.8kg of cement, add them into a mortar mixer and stir for 30s, then add 9kg of machine-made sand and stir for 45s, then add 1.26kg of water and stir for 75s, then add 0.042kg of water reducer into the mortar mixer, first stir at a low speed of 70r / min for 60s, then stir at a high speed of 150r / min for 60s, finally add 0.18kg of accelerator and stir for 30s to obtain a mortar preform of alkali slag-carbide slag-fly ash-slag-cement five-element cementitious material, and finally obtain mortar specimens with a size of 40mm×40mm×160mm by spray large plate forming. The mortar specimens are cured under standard conditions for 1d, 7d and 28d, which are recorded as sample 10.
[0078] Comparative Example 2: Weigh 0.30kg of alkali slag powder, 0.30kg of carbide slag powder, 0.60kg of slag and 1.8kg of cement, add them into a mortar mixer and stir for 30s, then add 9kg of machine-made sand and stir for 45s, then add 1.26kg of water and stir for 75s, then add 0.042kg of water reducer into the mortar mixer, first stir at a low speed of 70r / min for 60s, then stir at a high speed of 150r / min for 60s, finally add 0.18kg of accelerator and stir for 30s to obtain a mortar preform of alkali slag-carbide slag-fly ash-slag-cement five-element cementitious material, and finally obtain mortar specimens with a size of 40mm×40mm×160mm by spray large plate forming method. The mortar specimens are cured under standard conditions for 1d, 7d and 28d, which are recorded as sample 11.
[0079] The initial setting time and final setting time of the sprayed mortar in Examples 1 to 9 were tested using a cement mortar setting time measuring instrument, and the test results are shown in Table 1; the compressive strength and flexural strength were tested using a hydraulic universal testing machine and an electric flexural testing machine, and the test results are shown in Table 2; the XRD test used a D / MAX-2500 / PC type X-ray diffractometer, a Cu target, a tube voltage of 200kV, a tube current of 40mA, a diffraction angle scanning range set to 10° to 80°, and a scanning rate of 1° / min. The SEM-EDS test used a TESCAN-VEGA3 scanning electron microscope to observe the microscopic morphology of the hardened slurry, and used the EDS spectrometer it carried to determine the microscopic material composition of the specimen.
[0080] Table 1 Initial setting time and final setting time index test results of the sprayed mortar specimens of the five-component cementitious material of alkali slag-calcium carbide slag-fly ash-slag-cement in Examples 1 to 9
[0081]
[0082] Table 1
[0083] Table 2 shows the index test results of the spraying mortar specimens of the five-component cementitious materials of alkali slag-calcium carbide slag-fly ash-slag-cement in Examples 1 to 9 and the spraying mortar specimens of the four-component cementitious materials of alkali slag-calcium carbide slag-slag-cement in Comparative Example 1 and Comparative Example 2.
[0084]
[0085]
[0086] Table 2
[0087] As shown in Table 1, for different slag-cement precursors, with the increase of fly ash content, the initial setting time and final setting time of the mortar specimens of the five-element cementitious material of alkali slag-carbide slag-fly ash-slag-cement are improved. It can be concluded that the increase of fly ash content has an inhibitory effect on the coagulation of cement mortar. This is because the coagulation time of mortar specimens is related to the hydration reaction rate of the cementitious system. The activity of slag-cement precursors gradually decreases due to the addition of fly ash, and the hydration reaction rate gradually decreases. Correspondingly, the hydration products also gradually decrease, which leads to a longer coagulation and hardening time of mortar specimens. With the increase of carbide slag content, the coagulation of mortar specimens is promoted. With the addition of more and more carbide slag, the hydration reaction rate becomes faster, and more hydration products are generated, resulting in a shortened coagulation time of the system. And from the results, it can be seen that for slag-cement precursors with different ratios, the optimal content of carbide slag is 10%, at which time the coagulation time of mortar specimens is less than that of other content.
[0088] It can be seen from the test results in Table 2 that after fly ash replaces part of the slag and is added into the slag-cement precursor, its strength is reduced. As more and more fly ash is added, the compressive strength and flexural strength both decrease to a certain extent. When the fly ash content is 2.5, 5, and 10%, respectively, the 28d compressive strength in Examples 4 to 6 decreases from 40.73MPa to 38.67 and 34.43MPa, respectively, down by 5.1 and 15.5%, respectively. The 28d flexural strength decreases from 6.72MPa to 6.22 and 5.59MPa, respectively, down by 7.4 and 16.8%, respectively. This is because the activity of fly ash is lower than that of slag. After replacing the highly active slag, the hydration rate of the entire cementitious system slowly slows down, and the generated hydration products also decrease, which to a large extent leads to a decrease in the compressive strength and flexural strength of the mortar specimens. After carbide slag replaced alkali slag and was added to the slag-cement precursor, compared with Examples 1, 4, and 7, the 28d compressive strength increased from 40.73MPa to 41.53 and 52.37MPa, respectively, up 2.0 and 28.6%, respectively, and the 28d flexural strength increased from 6.72MPa to 7.76 and 8.78MPa, respectively, up 15.5 and 30.7%, respectively, which greatly improved the compressive strength and flexural strength. When the mass ratio of the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement was 1:1:0.5:1.5:6, the mortar The compressive strength and flexural strength of the specimens both reached peak values, and the cementitious system reached its optimal state at this time. Unlike the quaternary alkali slag-carbide slag-slag-cement cementitious material, the fly ash activity in the quinary alkali slag-carbide slag-fly ash-slag-cement cementitious material is relatively low. At this time, the amount of carbide slag added is more than that of the quaternary material, which will increase the Ca(OH)2 crystals in the system, requiring more Ca(OH)2 mass to react with fly ash, and then generating more calcium silicate hydrate gelling and calcium chloroaluminate hydrate, making the compressive strength of the cementitious system as high as 52MPa and the flexural strength as high as 8.8MPa.
[0089] The alkali slag-carbide slag-fly ash-slag-cement five-component cementitious material prepared in Example 7 was subjected to vacuum evacuation and gold spraying treatment, and the microscopic morphology of the hardened slurry of the four-component cementitious material was observed using a scanning electron microscope. The microscopic morphology of the hardened slurry of the alkali slag-carbide slag-fly ash-slag-cement five-component cementitious material prepared in Example 7 at 28 days of age was obtained at a magnification of 5000 times as shown in the figure. Figures 2 to 4 As shown by Figure 2 , Figure 3 as well as Figure 4It can be seen that the alkali slag-carbide slag-fly ash-slag-cement five-element cementitious material prepared in Example 7 has an overall dense microstructure, a relatively flat surface and few cracks, which is the main reason for the highest compressive strength and flexural strength. It also proves that the carbide slag promotes the hydration reaction of the entire cementitious system; the alkali slag contains a large amount of soluble chloride, which will generate conventional flocculent calcium silicate hydrate (CAH, CASH), and the entire cementitious system contains a large number of hexagonal plate-like crystals and needle-rod-like crystal structures. These crystal structures should be hydrated calcium chloroaluminate (3CaO·Al2O3·CaCl2·10H2O), and they overlap each other to fill the tiny cracks in the system, making the structure tighter. The two crystal structure hydration products jointly form the skeleton of the system, ensuring its highest strength.
[0090] Depend on Figure 5 It can be seen that the 3CaO·Al2O3·CaCl2·10H2O diffraction peak of the five-component cementitious material prepared in Example 7 is significantly enhanced after curing for 28 days, as shown in Figure 2 The microstructure of the gel system shown in FIG. 1 includes hexagonal plate-like crystals and needle-rod-like crystal structures; Figure 5 CaCO3 diffraction peaks can be observed in the slag. The main reasons for the existence of CaCO3 are that the CaCO3 substance in the carbide slag and the gelling system react with Ca(OH)2 and CO2 in the environment to generate; Figure 5 Mullite diffraction peaks were observed in the gel system. The main source of Mullite is fly ash. This is because some fly ash still did not participate in the hydration reaction at 28 days in the gel system. Figure 5 Quartz diffraction peaks were observed in the hydrated silicate. Quartz mainly comes from slag, which provides active silicon for the hydration reaction and promotes the hydration reaction to form amorphous calcium silicate hydrate gel.
[0091] The EDS spot test method was used to perform EDS analysis on the hardened slurry of the five-element cementitious material of alkali slag-calcium carbide slag-fly ash-slag-cement prepared in Example 7, and the element types and content analysis of the mortar material sample after curing for 28 days were detected. The EDS analysis point locations are as follows: Figure 6 The EDS spectra of EDS points 1 to 2 of the hardened slurry of the five-component cementitious material based on alkali slag-carbide slag-fly ash-slag-cement prepared in Example 7 are as shown in FIG. Figures 7-8 shown.
[0092] Depend on Figure 7 It can be seen that Figure 6 The main elements at position 1 are Ca, Si, Al, O and Cl, etc. It is determined that the hydration products here are calcium chloroaluminate hydrate and CASH gelation; Figure 8 As shown, Figure 6The main elements in position 2 are Ca, Si, Al, O and Cl, and Figure 3 The flocculent results shown by SEM are consistent, indicating that the hydration products here are also calcium chloroaluminate hydrate and CASH gel.
[0093] In summary, the mortar material provided by the present invention is based on the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement. By adding fly ash, the main components of fly ash are silicon dioxide, aluminum oxide and iron oxide, and its polymerization degree is relatively large and not easy to break and disintegrate. The alkali slag and carbide slag mainly create a strong alkaline environment for the cementitious system, so that some Si-O bonds and Al-O bonds in the fly ash are broken and Ca 2+ A small amount of hydration products are generated, such as 3CaO·Al2O3·CaCl2·10H2O, which together with CSH, CASH and other cementitious materials in the five-component cementitious materials fill the pores between the particle structures, making the structure more compact and forming a unified whole between the phases, thereby improving the compressive strength of the mortar material.
[0094] The embodiments described above are only descriptions of the preferred implementation modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing a spray mortar material based on a five-component cementitious material, characterized in that: The specific steps are as follows: S1, preparing alkali slag powder and carbide slag powder: respectively standing the alkali slag slurry and carbide slag slurry for 5-7 days, removing the upper clear liquid and stirring the sediment layer to a wet base state, placing the wet base alkali slag slurry and carbide slag slurry in a drying oven at 60-80° C. for drying, then grinding the dried alkali slag and carbide slag respectively, and sieving with a 200-300 mesh sieve to obtain alkali slag powder and carbide slag powder; S2, modification treatment of slag by alkali slag powder and carbide slag powder: the alkali slag powder, the carbide slag powder and the slag of equal mass are mixed evenly, and then put into a horizontal ball mill for dry grinding. After the mixed dry grinding for 30-40 minutes, the mixture is covered with a plastic wrap and allowed to stand for aging for 24-36 hours to obtain a modified alkali slag-carbide slag-slag mixture. The operating frequency of the horizontal ball mill is set to 40-60 Hz, and the speed is set to 250-300 r / min. During the modification treatment, the alkali slag powder and the carbide slag powder are used to introduce Ca(OH)2 into the gelling system. The reaction chemical reaction of the whole system is as follows: CaO+H2O→Ca(OH)2 Ca(OH)2+SiO2+H2O→CaO·SiO2·6-8H2O Ca(OH)2+Al2O3+SiO2+Cl - +H2O→2CaO·2Al2O3·4SiO2·5H2O+3CaO·Al2O3·C aCl2·10H2O <h2 style=";text-align:left;direction:ltr">Ca(OH)2+Al2O3+Na2O+MgO+SO3+Cl<h2 style=";text-align:left;direction:ltr"> - <h2 style=";text-align:left;direction:ltr"> +H2O+CO2→6MgO·Al2O3·CO2·12H2O+NaCl+CaSO4·2H2O+CaCO3; S3, preparing a five-component cementitious material: adding the modified alkali slag-carbide slag-slag mixture prepared in step S2, fly ash and cement in a preset mass percentage into a cement mortar mixer and stirring for 30 to 40 seconds to obtain an alkali slag-carbide slag-fly ash-slag-cement five-component cementitious material; S4, prepare a mortar preform containing five-component cementitious materials: sequentially add a first preset amount of machine-made sand, a second preset amount of water, a third preset amount of water-reducing agent and a fourth preset amount of accelerating agent into a cement mortar mixer containing five-component cementitious materials of alkali slag-calcium carbide slag-fly ash-slag-cement, and stir each material after adding one material each time, and finally obtain a mortar preform containing five-component cementitious materials of alkali slag-calcium carbide slag-fly ash-slag-cement, wherein the machine-made sand, the third preset amount of water-reducing agent and the fourth preset amount of accelerating agent are added into a cement mortar mixer containing five-component cementitious materials of alkali slag-calcium carbide slag-fly ash-slag-cement. The mass ratio of the water, the water reducing agent and the quick-setting agent to the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement is 2-4:0.3-0.5:0.01-0.02:0.05-0.07:1; the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement comprises 10-20% alkali slag, 0-10% carbide slag, 0-20% fly ash, 0-20% slag and 50-70% cement in mass percentage; S5. Preparation of spray mortar material by spraying and curing: a mortar sprayer is used to spray and cure the mortar preform of the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement prepared in step S4.
2. The method for preparing a spray mortar material based on a five-component cementitious material according to claim 1, characterized in that: Step S5 specifically includes the following sub-steps: S51, lubricating the mortar pipe of the mortar spraying machine with cement slurry, and then pouring the mortar prefabricated body of the alkali slag-carbide slag-fly ash-slag-cement five-element cementitious material into the injection mortar pump of the mortar spraying machine; S52. Adjust the nozzle of the spray gun to form an angle of 40° to 50° with the spray surface of the spray plate, start the mortar sprayer, and the spray mortar pump of the mortar sprayer continuously mixes the mortar preform of the alkali slag-calcium carbide slag-fly ash-slag-cement five-component cementitious material at a rotation speed of 80 to 100 revolutions per minute for 30 to 60 seconds, and then drives the mortar preform of the alkali slag-calcium carbide slag-fly ash-slag-cement five-component cementitious material into the mortar pipeline by air pressure, and sprays the formed spray mortar flow onto the spray plate through the nozzle of the spray gun, and solidifies to form the spray mortar material of the alkali slag-calcium carbide slag-fly ash-slag-cement five-component cementitious material.
3. The method for preparing a spray mortar material based on a five-component cementitious material according to claim 1, characterized in that: In step S4, after adding a first preset amount of machine-made sand, stir at a low speed for 30 to 60 seconds, after adding a second preset amount of water, stir at a low speed for 60 to 90 seconds, after adding a third preset amount of water reducer, stir at a low speed for 30 to 60 seconds, and then stir at a high speed for 30 to 60 seconds, after adding a fourth preset amount of accelerating setting agent, stir at a high speed for 30 to 40 seconds, wherein the rotation speed of the low-speed stirring is 40 to 70 r / min, and the rotation speed of the high-speed stirring is 100 to 150 r / min.
4. The method for preparing a spray mortar material based on a five-component cementitious material according to claim 1, characterized in that: The moisture content of the sedimentary layers of the wet-based alkali slag slurry and carbide slag slurry is 40% to 60%. The drying time of the wet-based alkali slag slurry is 5-7 days, and the drying time of the wet-based carbide slag slurry is 2-3 days.
5. The method for preparing a spray mortar material based on a five-component cementitious material according to claim 1, characterized in that: The specific surface area of the slag is 330-370m 2 / kg, the medium particle size of the specific surface area of the slag is 17-21μm, the cement is PO 42.5 silicate cement, the particle size of the machine-made sand is 0.16-4.75mm, the fineness modulus of the machine-made sand is 2.4-2.8, the mud content of the machine-made sand is ≤1%, the water reducer is a polycarboxylic acid type water reducer and the water reduction rate is ≥15%, the initial setting time of the accelerator is ≤5min and the final setting time is ≤15min, the solid content of the accelerator is 35-45%, and the size of the spray plate is ≥450mm×450mm×120mm.
6. The method for preparing a spray mortar material based on a five-component cementitious material according to claim 1, characterized in that: The alkali residue used in step S1 is produced by the ammonia-soda process to produce soda ash, and the reaction process is as follows: CaO+H2O=Ca(OH)2 NaCl+NH3+CO2+H2O=NaHCO3+NH4Cl 2NH4Cl+Ca(OH)2=2NH3↑+CaCl2+2H2O The carbide slag used in step S1 is alkaline waste slag produced in the process of obtaining acetylene gas by hydrolyzing carbide, and the reaction process is as follows: CaC2+2H2O=C2H2+Ca(OH)2.
7. The method for preparing a spray mortar material based on a five-component cementitious material according to claim 1, characterized in that: The grinding process in step S1 adopts a high-speed crusher with a rotation speed of 25000-30000 r / min, and the cement mortar mixer in step S3 is a planetary cement mortar mixer.
8. The sprayed mortar material based on five-component cementitious materials prepared by the method for preparing the sprayed mortar material based on five-component cementitious materials according to any one of claims 1 to 7, characterized in that: The sprayed mortar material includes a first preset amount of machine-made sand, a second preset amount of water, a third preset amount of water-reducing agent, a fourth preset amount of accelerating setting agent, and a five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement. The mass ratio of the first preset amount of machine-made sand to the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement is 2 to 4, the mass ratio of the second preset amount of water to the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement is 0.3 to 0.5, the third preset amount of water-reducing agent is 1 to 2% of the mass of the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement, and the fourth preset amount of accelerating setting agent is 5 to 7% of the mass of the five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement.
9. The spraying mortar material based on five-component cementitious material according to claim 8, characterized in that: The five-component cementitious material of alkali slag-carbide slag-fly ash-slag-cement comprises 10-20% of alkali slag, 0-10% of carbide slag, 0-20% of fly ash, 0-20% of slag and 50-70% of cement in mass percentage.
10. The spraying mortar material based on five-component cementitious material according to claim 8, characterized in that: The compressive strength test of the sprayed mortar material is carried out. The specific processing process is: the cured spray plate specimens are cut and formed into a triple test mold of 40mm×40mm×160mm, and then cured in a standard curing box with a temperature of 20±2°C and a humidity greater than 95% for 1 day, 7 days and 28 days, and then the compressive strength and flexural strength tests are carried out respectively.