Preparation method of silicon carbide ceramic

Nanocrystals are formed in situ in silicon carbide ceramics through magnetic stirring and rotary evaporation technology. Combined with discharge plasma sintering, the problem of nano-scale raw materials aggregation affects density, and the preparation of silicon carbide ceramics with high purity and high density is achieved, which simplifies the Process and reduce costs.

CN119039004AActive Publication Date: 2024-11-29BEIJING INST OF TECH TANGSHAN RES INST +1

Patent Information

Application Number
CN202411155108.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

During the sintering process, silicon carbide ceramics are easily agglomerated due to the agglomeration of nano-scale raw materials, and the existing fine crystal strengthening methods are complex and easy to introduce impurities. How to achieve in-situ self-generating nanocrystals while maintaining denseness.

Method used

Magnetic stirring and rotary evaporation technology are used to prepare dry powders, combined with discharge plasma sintering, nano silicon carbide is directly formed in situ in the micron-scale spherical silicon carbide matrix, simplifying the process and reducing impurity contamination.

Benefits of technology

Nanocrystal reinforcement under high purity and high density is achieved, the preparation process is simplified, production costs are reduced, and the high-temperature performance of silicon carbide ceramics is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039004A_ABST
    Figure CN119039004A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of silicon carbide ceramic. The method comprises the following steps: 1) preparing a main raw material, wherein the main raw material comprises the following components: micron-sized alpha-silicon carbide spherical powder and polycarbosilane powder accounting for 2.5%-10% by mass of silicon carbide; 2) slurry preparation: adding polycarbosilane powder into a butyl ether solvent, preparing a polycarbosilane solution under magnetic stirring, then adding silicon carbide powder into the polycarbosilane solution, and continuing magnetic stirring to obtain mixed slurry; (3) rotary evaporation drying: carrying out rotary evaporation drying on the mixed slurry obtained in the step (2) to prepare ceramic powder; and 4) spark plasma sintering: performing spark plasma sintering on the ceramic powder obtained in the step (3) to obtain the silicon carbide ceramic. The compact silicon carbide ceramic with good performance can be obtained through direct sintering in-situ self-generation of nano silicon carbide crystal grains. The process is simple in step, short in flow, convenient to operate, capable of effectively reducing the cost and suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of preparation of silicon carbide ceramics, and in particular relates to a method for directly sintering in-situ self-generated nanocrystals to achieve fine-grained strengthened silicon carbide ceramics. Background Art

[0002] Silicon carbide (SiC) has few lattice defects due to its crystal structure and the highly covalent nature of Si-C bonds, and has excellent high-temperature strength, high wear resistance, corrosion resistance, and good electrical and thermal conductivity. Therefore, silicon carbide is widely used in aerospace, defense armor, semiconductors, nuclear industry and other fields. However, the strong covalent bonding and low diffusion coefficient of silicon carbide make it difficult to sinter. At present, the preparation of silicon carbide ceramics mainly adopts hot pressing and pressureless sintering, while spark plasma sintering has attracted much attention because it can significantly reduce the sintering temperature.

[0003] Faced with increasingly stringent performance requirements, silicon carbide ceramics are in urgent need of further improving their performance. The main strengthening methods currently include second phase strengthening and fine grain strengthening. Second phase strengthening improves material properties by introducing dispersed, uniform fine particles into the silicon carbide ceramic matrix to hinder dislocation movement, but this will affect the purity of silicon carbide ceramics. Fine grain strengthening improves material properties by increasing the number of grain boundaries through grain refinement. For example, patent CN101182211 uses nano silicon carbide as the matrix raw material and adopts two-step molding and sintering technology to prepare nano silicon carbide ceramics with a grain size of 200nm.

[0004] Polycarbosilane is often introduced into materials as a precursor of silicon carbide ceramics, and nano-scale silicon carbide can be prepared after thermal crosslinking and pyrolysis. During the cracking process of polycarbosilane, when the temperature is greater than 200°C, organic macromolecules undergo condensation reactions and release gases; when the temperature is greater than 800°C, all organic macromolecules are converted into amorphous inorganic substances, and when the temperature is greater than 1400°C, amorphous inorganic substances are crystallized and converted into silicon carbide nanocrystals. For example, patent CN101774810 mixes polycarbosilane and α-SiC micropowder, and prepares a surface-modified silicon carbide powder of β-SiC nanocrystals coated with non-spherical α-SiC micropowder by high-temperature cracking. However, in the above-mentioned fine-grain strengthening method, the nano-scale raw material powder is easy to agglomerate, which affects the uniformity of the organization. The method of preparing modified powder by cracking and coating the precursor first, and then sintering the powder to prepare bulk silicon carbide ceramics increases the complexity of the process and is prone to introducing impurities.

[0005] In the manufacturing process of composite materials, the method of generating and growing reinforcing materials directly in the matrix is ​​called in-situ self-generation method, which can effectively avoid the introduction of impurities. The ceramic precursor polycarbosilane is mixed with the raw material powder and then directly sintered. On the one hand, the nanocrystals generated by the in-situ self-generation method can achieve fine grain strengthening, and on the other hand, it can also reduce the impurity pollution in the two-step process of pyrolysis of the precursor to prepare the modified powder and then sintering the modified powder. However, the cracking of polycarbosilane at high temperature will release a large amount of gas, which seriously affects the density of the sintered material. This is also the reason why the ceramic precursor must first be cracked at high temperature to prepare the powder when preparing silicon carbide ceramics. Therefore, how to ensure the in-situ self-generation of nanocrystals while maintaining the density of the bulk material is an urgent problem to be solved. Summary of the invention

[0006] The present invention provides a method for preparing silicon carbide ceramics, wherein the mixed powder is first magnetically stirred, then rotary evaporated to directly obtain a dry mixed powder, and finally the mixed powder is directly sintered, and nano silicon carbide is in situ formed in a micron-sized spherical silicon carbide matrix by an in-situ self-generation method, and a dense bulk ceramic is obtained. Nanocrystals can further improve the toughness of silicon carbide, and direct sintering ensures the high purity of the prepared silicon carbide ceramics. A silicon carbide ceramic is provided by the preparation method, and the performance of the silicon carbide ceramic can meet general process requirements.

[0007] On the one hand, the present invention provides a method for preparing silicon carbide ceramics, which mainly includes the following process steps:

[0008] Step (1) Configuration of main raw materials: The main raw materials include the following components: micron-grade α-silicon carbide spherical powder, polycarbosilane powder accounting for 2.5%-10% of the mass ratio of silicon carbide powder, the particle size range of the silicon carbide spherical powder is 40-70 μm, the purity is greater than 99%, the molecular weight of polycarbosilane is 1100-1400, and it is a mixture of colorless blocks and powders at room temperature. The reason for using spherical silicon carbide powder is that the spherical powder has good fluidity during the sintering process, and the gaps between the spherical powders are conducive to gas discharge, which helps to promote densification and sintering.

[0009] Step (2) slurry preparation: weighed polycarbosilane is placed in a flat-bottom flask, and then a magnetic stirring bar is placed in the flat-bottom flask. The material of the magnetic stirring bar is polytetrafluoroethylene / magnetic steel material, and the size of the magnetic stirring bar is a cylinder of Ø8mm×40mm.

[0010] Pour butyl ether organic solvent into the flat-bottom flask, and then place the flat-bottom flask containing polycarbosilane, magnetic stirring bar and butyl ether on a magnetic stirring device. The magnetic stirring speed is 450-800r / min, and the stirring time is 30-60min, until the polycarbosilane is completely dissolved and the solution is transparent without suspension and precipitation.

[0011] The weighed silicon carbide spherical powder is added to the mixed polycarbosilane solution, and the stirring speed is increased to 800-1500 r / min for 3-6 hours to obtain a mixed slurry.

[0012] Step (3) Rotary evaporation and drying: Place the flask containing the mixed slurry obtained in step (2) in a rotary evaporator and perform rotary evaporation and drying by heating in an oil bath.

[0013] The rotary evaporation drying environment is in a negative pressure state, the rotary evaporation drying temperature is 130-150°C, the flask rotation speed is 50-100r / min, and the drying time is 1-2h to prepare the ceramic powder. What is directly obtained after rotary evaporation is dry ceramic powder, not a block. The rotary evaporation drying temperature is the boiling point of butyl ether (141°C) and does not reach the softening point of polycarbosilane (180-230°C). What is directly obtained after rotary evaporation is dry ceramic powder.

[0014] Step (4) Spark plasma sintering: The ceramic powder obtained in step (3) is loaded into a graphite mold, and then the graphite mold is placed in a spark plasma sintering device, first heated to 800°C at a heating rate of 100-150°C / min, and kept at this temperature for 2-5 minutes, which helps the powder particles to flow and rearrange and promotes gas discharge.

[0015] The temperature was continued to rise to 1200°C at a heating rate of 100-150°C / min.

[0016] While increasing the sintering pressure to 50 MPa, continue to increase the temperature to 1600 ° C at a heating rate of 50-100 ° C / min, and ensure that the pressure loading is completed before reaching 1600 ° C. At this stage, the simultaneous pressurization and heating are conducive to initial densification and sintering.

[0017] When the temperature rises to 1600℃, continue to pressurize and heat up. While increasing the sintering pressure to 70-80MPa, continue to heat up to 1750-1800℃ at a heating rate of 50-100℃ / min. It should be ensured that the pressure loading is completed before reaching the set temperature. The insulation time is 1-10min. At this stage, the simultaneous pressurization and heating are conducive to the final densification and sintering. After sintering, cool with the furnace to obtain silicon carbide samples.

[0018] On the other hand, the present invention also provides silicon carbide ceramics prepared by the preparation method.

[0019] The beneficial effects of the present invention include:

[0020] The method for preparing silicon carbide ceramics provided by the present invention does not require the addition of additional sintering aids, nor does it require thermal crosslinking and curing. After rotary evaporation, the powder can be directly used for sintering, and the main product after the ceramic precursor is cracked is silicon carbide, which not only ensures the purity but also improves the high-temperature performance of the silicon carbide ceramic.

[0021] The present invention provides a method for preparing silicon carbide ceramics, which adopts an in-situ self-generation method to in-situ form nano silicon carbide grains in a micron-sized spherical silicon carbide matrix and directly sinter to prepare a dense bulk ceramic.

[0022] The present invention provides a method for preparing silicon carbide ceramics, which uses the high pressure and rapid temperature rise of spark plasma sintering to suppress the growth of grains, and obtains silicon carbide ceramics with multi-level grain size distribution, solving the problem of poor ceramic density caused by gas generated by the decomposition of polycarbosilane. This method for preparing silicon carbide ceramics has the advantages of short process and simple operation, and can effectively reduce the production cost of silicon carbide ceramics. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 A process engineering diagram of a method for preparing silicon carbide ceramics in an embodiment

[0024] Figure 2 A microscopic morphology of spherical silicon carbide in a method for preparing silicon carbide ceramics in an embodiment

[0025] Figure 3 The XRD pattern of spherical silicon carbide in a method for preparing silicon carbide ceramics in the embodiment is shown in FIG.

[0026] Figure 4 FTIR spectrum of polycarbosilane of a method for preparing silicon carbide ceramics in the embodiment

[0027] Figure 5 A fracture morphology of a silicon carbide ceramic sample obtained by adding 2.5 wt% polycarbosilane in a method for preparing silicon carbide ceramic in an embodiment

[0028] Figure 6 A fracture morphology of a silicon carbide ceramic sample obtained by adding 5 wt% polycarbosilane in a method for preparing silicon carbide ceramic in an embodiment DETAILED DESCRIPTION

[0029] The present invention is further described below in conjunction with the accompanying drawings and specific examples. It should be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values ​​​​exemplified below.

[0030] Example 1

[0031] Step (1) Preparation of main raw materials: The main raw materials include the following components: weigh 10 grams of micron-grade α-silicon carbide spherical powder and 0.25 grams of polycarbosilane powder, the particle size range of the silicon carbide spherical powder is 40 μm, the purity is greater than 99%, and the molecular weight of polycarbosilane is 1200.

[0032] Step (2) Slurry preparation: polycarbosilane is placed in a flat-bottom flask, and a magnetic stirrer is added. The material of the magnetic stirrer is polytetrafluoroethylene / magnetic steel material, and the size of the magnetic stirrer is a cylinder of Ø8mm×40mm.

[0033] Pour 50 ml of butyl ether organic solvent into the flat-bottom flask, and then place the flat-bottom flask containing polycarbosilane, magnetic stirring bar and butyl ether on the magnetic stirring equipment. The magnetic stirring speed is 450 r / min and the stirring time is 30 min. The polycarbosilane is completely dissolved and the solution is transparent without suspension and precipitation.

[0034] The weighed silicon carbide spherical powder was added to the mixed polycarbosilane solution, and the stirring speed was increased to 800 r / min for 3 h to obtain a mixed slurry.

[0035] Step (3) Rotary evaporation and drying: Place the flask containing the mixed slurry obtained in step (2) in a rotary evaporator and perform rotary evaporation and drying by heating in an oil bath.

[0036] Under negative pressure, the rotary evaporation drying temperature is 140°C, the flask rotation speed is 50r / min, and the drying time is 2h to prepare ceramic powder. What is directly obtained after rotary evaporation is dry ceramic powder, not a block.

[0037] Step (4) Spark plasma sintering: The ceramic powder obtained in step (3) is placed in a graphite mold, and then the graphite mold is placed in a spark plasma sintering device, first heated to 800°C at a heating rate of 100°C / min, and kept at this temperature for 3 minutes, which helps the powder flow and promotes gas discharge.

[0038] The temperature was further increased to 1200°C at a heating rate of 100°C / min.

[0039] While increasing the sintering pressure to 50 MPa, continue to increase the temperature to 1600°C at a heating rate of 50°C / min. It should be ensured that the pressure loading is completed before the temperature reaches 1600°C. At this stage, the simultaneous pressurization and heating are conducive to initial densification and sintering.

[0040] When the temperature reaches 1600℃, continue to pressurize and heat up. While increasing the sintering pressure to 80MPa, continue to heat up to 1750℃ at a heating rate of 50℃ / min. It should be ensured that the pressure loading is completed before the temperature reaches 1750℃, and the holding time is 5min. At this stage, the simultaneous pressurization and heating are conducive to the final densification and sintering. After sintering, it is cooled in the furnace to obtain a silicon carbide sample.

[0041] The fracture morphology of the silicon carbide sample sintered in this embodiment is shown in FIG. Figure 5 As shown in the figure, nano-crystals can be observed, indicating that in-situ self-generation of silicon carbide has been achieved, that is, nano-crystals generated by in-situ cracking of the precursor polycarbosilane. The three-point bending strength test showed that the bending strength of the sample was 443MPa. The above data show that dense silicon carbide ceramics with good performance have been successfully prepared by direct sintering.

[0042] Example 2

[0043] Configuration of main raw materials: The main raw materials include the following components: weigh 10 grams of micron-grade α-silicon carbide spherical powder, 0.5 grams of polycarbosilane powder, the particle size range of the silicon carbide spherical powder is 40 μm, the purity is greater than 99%, and the molecular weight of polycarbosilane is 1200.

[0044] Step (2) is the same as in Example 1.

[0045] Step (3) is the same as in Example 1.

[0046] Step (4) is the same as in Example 1.

[0047] The fracture morphology of the silicon carbide sample sintered in this embodiment is shown in FIG. Figure 6 As shown in the figure, nano-crystals can be observed, indicating that in-situ self-generation of silicon carbide has been achieved, that is, nano-crystals are generated by in-situ cracking of the precursor polycarbosilane. The three-point bending strength test shows that the bending strength of the sample is 475MPa. The above data show that dense silicon carbide ceramics with good performance have been successfully prepared by direct sintering.

Claims

1. A method for preparing silicon carbide ceramics, characterized in that: The following steps are involved: 1) Configuration of main raw materials: The main raw materials include the following components: micron-grade α-silicon carbide spherical powder, polycarbosilane powder accounting for 2.5%-10% of silicon carbide powder by mass; 2) Slurry preparation: adding polycarbosilane powder to a butyl ether solvent to prepare a polycarbosilane solution under magnetic stirring, and then adding silicon carbide powder to the polycarbosilane solution and continuing magnetic stirring to obtain a mixed slurry; 3) Rotary evaporation drying: Rotary evaporation drying the mixed slurry obtained in step (2) to prepare ceramic powder; 4) Spark plasma sintering: The ceramic powder obtained in step (3) is subjected to spark plasma sintering to obtain silicon carbide ceramics.

2. A method for preparing silicon carbide ceramics according to claim 1, characterized in that: The particle size of the micron-grade α-silicon carbide spherical powder ranges from 40 to 70 μm, and the purity is greater than 99%.

3. A method for preparing silicon carbide ceramics according to claim 1, characterized in that: The molecular weight of polycarbosilane powder is 1100-1400, and it is a mixture of colorless blocks and powder at room temperature.

4. A method for preparing silicon carbide ceramics according to claim 1, characterized in that: The magnetic stirring speed of mixing polycarbosilane and butyl ether solvent is 450-800 r / min, the stirring time is 30-60 min, the magnetic stirring bar is made of polytetrafluoroethylene / magnetic steel, and the size of the magnetic stirring bar is a cylinder of Φ8mm×40mm.

5. A method for preparing silicon carbide ceramics according to claim 1, characterized in that: The magnetic stirring speed of mixing the silicon carbide powder and the polycarbosilane solution is 800-1500 r / min, and the stirring time is 3-6 hours.

6. A method for preparing silicon carbide ceramics according to claim 1, characterized in that: The temperature of the rotary drying is 130-150°C, the rotation speed is 50-100r / min, and the drying time is 1-2h.

7. A method for preparing silicon carbide ceramics according to claim 1, characterized in that: In step (4), during the heating process of the spark plasma sintering, the sintering temperature is less than 1200° C. and the heating rate is 100-150° C. / min; the sintering temperature is greater than 1200° C. and the heating rate is 50-100° C. / min.

8. A method for preparing silicon carbide ceramics according to claim 1, characterized in that: In step (4), the spark plasma sintering is carried out at 800° C. for 2-5 minutes.

9. A method for preparing silicon carbide ceramics according to claim 1, characterized in that: In step (4), when the spark plasma sintering temperature is raised to 1200° C., the sintering pressure is increased to 50 MPa, and the temperature is continued to be raised to 1600° C.

10. A method for preparing silicon carbide ceramics according to claim 1, characterized in that: In step (4), the spark plasma sintering, when the temperature is raised to 1600° C., the sintering pressure is increased to 70-80 MPa, and the temperature is continued to be raised to 1750-1800° C., and the holding time is 1-10 min.

11. A silicon carbide ceramic material obtained by the method according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Method for rapidly preparing MCMBs / SiC composite material through two-step sintering

    CN115724664A

  • Low-temperature sintered compact block ceramic material and preparation method thereof

    CN116947490A

  • Fibre composite ceramic with a high thermal conductivity

    US20030162647A1

  • In-situ formation of reinforcement phases in ultra high temperature ceramic composites

    US8409491B1

Cited By

  • Silicon carbide ceramic material and preparation method thereof

    CN119504275A

  • Silicon carbide ceramic material and preparation method thereof

    CN119504275B