Asphaltene inhibitor based on modified graphene oxide as well as preparation method and application of asphaltene inhibitor
By using modified graphene oxide asphaltene inhibitors in the oil field, the polymerization of asphaltene is prevented by using fused polyaromatic rings and hydrophobic side chain structures, the problem of asphaltene deposition in the oil field is solved, and efficient and low-cost recovery is achieved Increased rate and reduced equipment maintenance costs.
Patent Information
- Application Number
- CN202411374710.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-29
AI Technical Summary
The prior art methods used to suppress asphaltene deposition in oil fields have problems such as high energy consumption, low efficiency, formation damage, poor stability and high cost, and cannot effectively solve the recovery rate reduction caused by asphaltene aggregation, flocculation and deposition. Equipment maintenance costs increase.
Using asphaltene inhibitors based on modified graphene oxide, graphite is used as raw material, and graphene oxide is prepared by Hummers method, and 6,10 diphenyldodecanol is grafted on graphite oxide through acid chloride and esterification reaction. The olefin molecules are edged, forming a modified graphene oxide asphaltene inhibitor with a fused polyaromatic ring structure and hydrophobic side chain, which uses π-π interaction and hydrophobic side chain to prevent the polymerization and deposition of asphaltene molecules.
It has achieved efficient suppression of asphaltene deposition, improved recovery rate, reduced production costs, enhanced crude oil liquidity, extended equipment service life, reduced formation blockage and corrosion risks, and is low-cost and environmentally friendly, suitable for large-scale production.
Smart Images

Figure CN119039250A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of oilfield unblocking, and particularly relates to an asphaltene inhibitor based on modified graphene oxide, and a preparation method and application thereof. Background Art
[0002] The global demand for energy is growing, and oil remains one of the most in-demand energy sources. At present, the reserves of light conventional crude oil are gradually decreasing, while the abundant heavy oil has huge potential for exploitation. Asphaltene is the core component of heavy oil, and its strong intermolecular interaction leads to its weak stability in crude oil. During crude oil extraction and refining, fluctuations in temperature, pressure and crude oil composition can easily cause asphaltene to aggregate, flocculate and precipitate, forming solid matter. This not only blocks the formation, resulting in a decrease in recovery rate, but also increases equipment maintenance costs, seriously affecting economic benefits. In recent years, asphaltene deposition has been common in oil fields. In order to improve recovery and reduce production costs, it is crucial to inhibit asphaltene deposition.
[0003] At present, the methods to solve asphaltene deposition mainly include physical removal, heat treatment, microbial method and chemical removal. Physical removal methods include scraping of sucker rods, scraping of steel wires and strong negative pressure unblocking. Although physical removal is simple to operate, it has problems such as high energy consumption and low efficiency. Moreover, it can only be removed after the blockage occurs, which cannot solve the problem from the source and only treats the symptoms but not the root cause. Thermal treatment is to increase the solubility of sediments and disperse them in the oil phase by injecting fluids (steam or hot water / gas / oil), setting up downhole heaters, adding exothermic agents, etc. However, as the temperature decreases, solid sediments may reappear, and the unblocking effect is limited by the capacity of the equipment, which will also cause formation damage. The microbial method is to use anaerobic / aerobic bacteria to treat asphaltene sediments through biodegradation, converting them into light hydrocarbons, thereby achieving the purpose of unblocking. However, microorganisms are generally less stable under high temperature and high salt, and the microbial action process is slow, difficult to control, and prone to corrosion. Chemical removal is one of the most common ways to unblock. Generally, asphaltene inhibitors are added to form a good dispersion in the oil through their strong adsorption with asphaltene. Although some progress has been made in the research on asphaltene inhibitors, there are still problems such as high cost and unsatisfactory effect. Therefore, there is an urgent need to develop efficient and low-cost asphaltene inhibitors.
[0004] The existing physical removal methods have high energy consumption and low efficiency, the heat treatment method may cause solid sediments to reappear and damage the formation, the microbial method has poor stability, slow action process and easy corrosion, and the asphaltene inhibitors in the chemical removal method are expensive and have unsatisfactory effects. Therefore, it is urgent to find an asphaltene inhibitor based on modified graphene oxide and its preparation method and application to inhibit asphaltene deposition efficiently and at low cost, improve recovery and reduce production costs. Summary of the invention
[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide an asphaltene inhibitor based on modified graphene oxide and its preparation method and application, so as to solve the technical problems of asphaltene aggregation, flocculation and deposition caused by temperature and pressure fluctuations and changes in crude oil composition during crude oil extraction and refining. These phenomena can lead to blockage of oil well formations, blockage of oil pipelines and corrosion of equipment, thereby reducing recovery rate and production efficiency. The present invention aims to reduce the relevant risks in crude oil production and transportation by inhibiting the agglomeration and deposition of asphaltene particles, and improve the stability and economy of oil extraction and refining processes.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions: The present invention discloses a method for preparing an asphaltene inhibitor based on modified graphene oxide, comprising the following steps: S1: Graphite, NaNO3 and concentrated H2SO4 were stirred and mixed evenly, KMnO4 was slowly added, and low-temperature reaction, medium-temperature reaction and high-temperature reaction were carried out in sequence, and then distilled water and H2O2 were added until bright yellow, and after centrifugation, filtration, washing and drying, the mixture was dissolved in distilled water, and after ultrasonication and freeze-drying, intermediate I was obtained; S2: adding intermediate I to the first solvent, mixing and stirring to react, then adding phosphorus oxychloride to carry out chlorination reaction, and after the reaction is completed, removing the solvent by reduced pressure distillation to obtain intermediate II; S3: The intermediate II, 6,10-diphenyl dodecanol and the second solvent are stirred and mixed uniformly, and after esterification reaction, the mixture is allowed to stand, filtered, washed and dried to obtain an asphaltene inhibitor based on modified graphene oxide.
[0007] Preferably, in step S1, the mass ratio of graphite, NaNO3, concentrated H2SO4 and KMnO4 is 1:(1-1.2):(40-42):(2-3).
[0008] Preferably, in step S1, the temperature of the low-temperature reaction is 0-5°C, and the reaction time is 2-3h; the temperature of the medium-temperature reaction is 35-40°C, and the reaction time is 2-3h; the temperature of the high-temperature reaction is 85-90°C, and the reaction time is 1-2h; and the amount of distilled water added is 60-80wt% of the total mass of the system.
[0009] Preferably, in step S2, the first solvent is any one of DMF, acetonitrile and tetrahydrofuran; and the mass ratio of the intermediate I, phosphorus oxychloride and the first solvent is 1: (0.1-0.2): (20-30).
[0010] Preferably, in step S2, the acyl chlorination reaction temperature is 15-25° C., and the reaction time is 2-5 h.
[0011] Preferably, in step S3, the second solvent is any one of dichloromethane, chloroform and tetrachloromethane; the mass ratio of intermediate II, 6,10-diphenyldodecanol and the second solvent is 1: (0.3-0.6): (20-30).
[0012] Preferably, in step S3, the temperature of the esterification reaction is 40-60° C., the reaction time is 3-6 hours, and the standing time is 24 hours.
[0013] The present invention also discloses an asphaltene inhibitor based on modified graphene oxide, which is prepared by the above preparation method. At 30° C., the dispersion stability is 86.6% to 92.8%; at 60° C., the dispersion stability is 88.7% to 96.6%.
[0014] Preferably, the general structural formula of the asphaltene inhibitor based on modified graphene oxide is: .
[0015] The present invention also discloses the use of the asphaltene inhibitor based on modified graphene oxide prepared by the preparation method as a scale inhibitor in an oil field, and the water separation rate of the scale inhibitor is 19.5% to 22.8%.
[0016] Compared with the prior art, the present invention has the following beneficial effects: The invention provides a method for preparing an asphaltene inhibitor based on modified graphene oxide. The method uses graphite as a raw material, firstly uses the Hummers method to prepare graphene oxide, and then uses acyl chloride reaction and esterification reaction to graft 6,10 diphenyl dodecanol on the edge of the graphene oxide molecule to obtain a modified graphene oxide asphaltene inhibitor having both a central fused polyaromatic ring structure and an edge hydrophobic side chain. There is a strong π-π interaction between the fused polyaromatic ring structure and the asphaltene. After the modified graphene oxide inhibitor is adsorbed on the asphaltene, a large number of hydrophobic side chains around it can effectively increase the steric hindrance between the asphaltene, form intervals between the asphaltene molecules, and improve the effect of inhibiting asphaltene deposition. The graphite selected by the invention is natural biomass, which is low in cost and environmentally friendly; the reaction mechanism is clear, the reaction process is easy to control, and it is suitable for large-scale production. The 6,10 diphenyl dodecanol modified graphene oxide of the invention can be used as a new type of asphaltene inhibitor for oilfield wellbore scale inhibition. Its mechanism of action is to inhibit the mutual attraction and association between asphaltene molecules, thereby achieving the effect of inhibiting their coagulation. The central condensed ring structure of the modified graphene oxide asphaltene inhibitor can be strongly anchored on the asphaltene surface under the action of π-π, hydrogen bonding and hydrophobicity, and has the ability to adsorb at multiple points on the asphaltene surface, which is conducive to forming a higher adsorption fastness. The hydrophobic chain at the edge can provide a steric hindrance effect between asphaltene molecules, effectively preventing the agglomeration of asphaltene molecules at the physical level, inhibiting their aggregation tendency, and then exerting the excellent dispersing inhibition effect of the inhibitor. Through the above effects, the inhibitor successfully prevents further aggregation between asphaltene molecules and effectively controls the aggregation tendency of asphaltene.
[0017] The invention also discloses an asphaltene inhibitor based on modified graphene oxide prepared by the above-mentioned preparation method. The asphaltene inhibitor based on modified graphene oxide can effectively inhibit asphaltene deposition. Through specific acyl chloride reaction and esterification reaction, 6,10 diphenyl dodecanol is grafted on the edge of graphene oxide molecules. The formed modified graphene oxide inhibitor can generate strong π-π interaction with asphaltene molecules, and provide steric hindrance through hydrophobic side chains, effectively preventing further polymerization and deposition of asphaltene molecules. The recovery rate can be improved. The addition of the inhibitor can significantly reduce the blockage of asphaltene in the formation, thereby improving the fluidity and recovery rate of crude oil and increasing the economic benefits of the oil field. The cost can be reduced. The selected graphite raw material is natural biomass, which is low in cost and easy to obtain. The reaction process is simple and easy to control, suitable for large-scale production, and helps to reduce the production cost of the inhibitor and the overall operating cost of the oil field. Environmentally friendly, graphite as a raw material is easily degradable and environmentally friendly, the entire preparation process and the use of the product meet environmental protection requirements, and help to reduce the negative impact of oil field exploitation on the environment. Good stability: The modified graphene oxide inhibitor has stable chemical properties and can maintain effective inhibition under different temperature and pressure conditions, reducing asphaltene deposition problems caused by fluctuating conditions.
[0018] The present invention also discloses the use of the asphaltene inhibitor based on modified graphene oxide prepared by the above preparation method as a scale inhibitor in oil fields. Through the unique molecular structure design, the inhibitor forms a strong interaction with the asphaltene molecules, effectively disperses the asphaltene, and significantly reduces the risk of formation blockage. The addition of the inhibitor reduces the fluid resistance caused by asphaltene deposition, making the crude oil flow smoother and improving the extraction and transportation efficiency of the oil field. By inhibiting asphaltene deposition, the blockage and corrosion inside the equipment are reduced, thereby extending the service life of the equipment and reducing the maintenance cost and the loss caused by downtime. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 A synthetic route map of the modified graphene oxide asphaltene inhibitor disclosed in the present invention; Figure 2 Schematic diagram of the inhibition mechanism of the modified graphene oxide asphaltene inhibitor disclosed in the present invention; Figure 3 This is an infrared spectrum of the modified graphene oxide asphaltene inhibitor prepared in Example 5 disclosed in the present invention. DETAILED DESCRIPTION
[0020] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0021] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0022] Unless otherwise specified, all technical and scientific terms used herein have the common meanings understood by those skilled in the art for the present invention. In case of conflict, the definitions in this specification shall prevail.
[0023] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0024] In this article, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0025] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0026] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0027] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0028] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0029] The present invention is further described in detail below in conjunction with the accompanying drawings: Based on the analysis of the molecular structure of asphaltene, the present invention grafts 6,10 diphenyl dodecanol onto the edge of graphene oxide molecules through acyl chlorination reaction and esterification reaction, so that the modified graphene oxide has both a central fused polyaromatic ring structure and an edge hydrophobic side chain, and there is a strong π-π interaction between the fused polyaromatic ring structure and the asphaltene. After the modified graphene oxide inhibitor is adsorbed on the asphaltene, a large number of hydrophobic side chains around it can effectively increase the steric hindrance between the asphaltene, form intervals between the asphaltene molecules, and improve the effect of inhibiting asphaltene deposition.
[0030] The present invention discloses a method for preparing an asphaltene inhibitor based on modified graphene oxide, comprising the following steps: S1: Add graphite, NaNO3 and concentrated H2SO4 to a dry three-necked flask, stir and mix evenly, react for 0.5-1h, then slowly add KMnO4 to the mixed solution under an ice bath, and carry out low-temperature reaction, medium-temperature reaction and high-temperature reaction in sequence. After the reaction is completed, add distilled water and H2O2 until the color of the solution changes to bright yellow, centrifuge, filter, wash and dry to obtain the first product, then dissolve the first product in distilled water, and obtain intermediate I after ultrasonic treatment and freeze-drying; S2: adding intermediate I to the first solvent, stirring and mixing evenly, then adding phosphorus oxychloride and stirring at a certain temperature for a certain period of time to react with chlorination. After the reaction is completed, removing the solvent by reduced pressure distillation to obtain intermediate II; S3: The intermediate II, 6,10-diphenyl dodecanol and the second solvent are mixed evenly, and the esterification reaction is stirred at a certain temperature for a certain time. After the reaction is completed, the mixture is allowed to stand for 24 hours, and then filtered, washed and dried to obtain an asphaltene inhibitor based on modified graphene oxide.
[0031] As an optional solution, in S1, the mass ratio of graphite, NaNO3, concentrated H2SO4 and KMnO4 is 1: (1~1.2): (40~42): (2~3). The temperature of the low-temperature reaction is 0~5℃, and the reaction time is 2~3h; the temperature of the medium-temperature reaction is 35~40℃, and the reaction time is 2~3h; the temperature of the high-temperature reaction is 85~90℃, and the reaction time is 1~2h; the amount of distilled water added is 60~80wt% of the total mass of the system.
[0032] As an optional scheme, in S2, the first solvent is one of DMF, acetonitrile and tetrahydrofuran; the mass ratio of intermediate I, phosphorus oxychloride and the first solvent is 1: (0.1-0.2): (20-30). The acyl chlorination reaction temperature is 15-25°C, and the reaction time is 2-5h.
[0033] As an optional solution, in S3, the second solvent is any one of dichloromethane, trichloromethane and tetrachloromethane; the mass ratio of intermediate II, 6,10-diphenyl dodecanol and the second solvent is 1: (0.3-0.6): (20-30). The esterification reaction temperature is 40-60°C, and the reaction time is 3-6h.
[0034] The present invention provides an asphaltene inhibitor based on modified graphene oxide, and the general structural formula of the asphaltene inhibitor based on modified graphene oxide is as follows: .
[0035] The present invention provides an application of an asphaltene inhibitor based on modified graphene oxide prepared according to the above-mentioned preparation method as a scale inhibitor in the field of oil fields. The inhibitor can significantly improve the inhibitory effect. The inhibitor can strongly interact with asphaltene molecules through its unique molecular structure, i.e., the fused polyaromatic ring structure at the center and the hydrophobic side chain at the edge to form a stable dispersion system, thereby significantly improving the effect of inhibiting asphaltene deposition and reducing the risk of formation blockage. The fluidity of crude oil can be enhanced. The addition of the inhibitor helps to maintain the fluidity of crude oil, reduce the increase in fluid resistance caused by asphaltene deposition, make crude oil easier to be mined and transported, and thus improve the production efficiency of the oil field. The service life of equipment can be extended: by effectively inhibiting the deposition of asphaltene, the inhibitor can reduce the blockage and corrosion inside the equipment, thereby extending the service life of related equipment and reducing maintenance costs and downtime. By improving the recovery rate, reducing maintenance costs, extending the life of equipment and reducing losses caused by shutdowns, the application of the inhibitor can significantly improve the economic benefits of the oil field and bring considerable returns to oil field operators.
[0036] The present invention will be further described below in conjunction with specific embodiments: Example 1 A method for preparing an asphaltene inhibitor based on modified graphene oxide comprises the following steps: S1: Add graphite, NaNO3, and concentrated H2SO4 in a mass ratio of 1:1:40 to a dry three-necked flask, stir and mix evenly, then slowly add KMnO4 twice the mass of graphite in an ice bath, stir and react at low temperature for 2 hours at 0°C, then heat to 35°C for medium temperature reaction for 2 hours, and finally heat to 85°C for high temperature reaction for 1 hour. After the reaction is completed, add distilled water and H2O2 with a mass of 60wt% of the total mass of the current system to the current system until the color of the solution turns bright yellow, centrifuge, filter, wash and dry to obtain the first product, then dissolve the first product in distilled water, and obtain intermediate I after ultrasonic treatment and freeze drying; S2: Add 1 g of intermediate I to 20 g of DMF, stir and mix evenly, then add 0.1 g of phosphorus oxychloride and stir at 15°C for 2 h for acyl chloride reaction. After the reaction is completed, remove the solvent by vacuum distillation to obtain intermediate II; S3: The intermediate II, 6,10-diphenyldodecanol and dichloromethane in a mass ratio of 1:0.3:20 were mixed evenly, and the esterification reaction was stirred at 40°C for 3 hours. After the reaction was completed, it was allowed to stand for 24 hours. After filtration, washing and drying, an asphaltene inhibitor based on modified graphene oxide was obtained.
[0037] Embodiment 2: A method for preparing an asphaltene inhibitor based on modified graphene oxide comprises the following steps: S1: Add graphite, NaNO3, and concentrated H2SO4 in a mass ratio of 1:1.2:42 to a dry three-necked flask, stir and mix evenly, then slowly add KMnO4 with a mass three times that of graphite in an ice bath, stir and react at low temperature for 3 hours at 5°C, then heat to 40°C for medium temperature reaction for 3 hours, and finally heat to 90°C for high temperature reaction for 2 hours. After the reaction is completed, add distilled water and H2O2 with a mass of 80wt% of the total mass of the current system to the current system until the color of the solution turns bright yellow, centrifuge, filter, wash and dry to obtain the first product, then dissolve the first product in distilled water, and obtain intermediate I after ultrasonic treatment and freeze drying; S2: 1 g of intermediate I was added to 30 g of acetonitrile, and the mixture was stirred to be uniform. Then, 0.2 g of phosphorus oxychloride was added and stirred at 25°C for 5 h for acyl chloride reaction. After the reaction was completed, the solvent was removed by distillation under reduced pressure to obtain intermediate II; S3: The intermediate II, 6,10-diphenyldodecanol and chloroform in a mass ratio of 1:0.6:30 were mixed evenly, and the esterification reaction was stirred at 60°C for 6 hours. After the reaction was completed, it was allowed to stand for 24 hours. After filtration, washing and drying, an asphaltene inhibitor based on modified graphene oxide was obtained.
[0038] Embodiment 3: A method for preparing an asphaltene inhibitor based on modified graphene oxide comprises the following steps: S1: Add graphite, NaNO3, and concentrated H2SO4 in a mass ratio of 1:1.1:41 to a dry three-necked flask, stir and mix evenly, then slowly add KMnO4 with a mass 2.5 times that of graphite in an ice bath, stir and react at low temperature for 2.5 hours at 2°C, then heat to 37°C for medium temperature reaction for 2.5 hours, and finally heat to 88°C for high temperature reaction for 1.5 hours. After the reaction is completed, add distilled water and H2O2 with a mass of 70wt% of the total mass of the current system to the current system until the color of the solution turns bright yellow, centrifuge, filter, wash and dry to obtain the first product, then dissolve the first product in distilled water, and obtain intermediate I after ultrasonic treatment and freeze drying; S2: Add 1 g of intermediate I to 25 g of tetrahydrofuran, stir and mix well, then add 0.15 g of phosphorus oxychloride and stir at 20°C for 3 h for acyl chloride reaction. After the reaction is completed, remove the solvent by distillation under reduced pressure to obtain intermediate II; S3: Intermediate II, 6,10-diphenyldodecanol and tetrachloromethane in a mass ratio of 1:0.4:25 were mixed evenly, and the mixture was stirred for esterification reaction at 50°C for 4.5 hours. After the reaction was completed, the mixture was allowed to stand for 24 hours, and an asphaltene inhibitor based on modified graphene oxide was obtained by filtration, washing and drying.
[0039] Embodiment 4: A method for preparing an asphaltene inhibitor based on modified graphene oxide comprises the following steps: S1: Add graphite, NaNO3, and concentrated H2SO4 in a mass ratio of 1:1.2:40 to a dry three-necked flask, stir and mix evenly, then slowly add KMnO4 with a mass three times that of graphite in an ice bath, stir and react at low temperature for 3 hours at 3°C, then heat to 38°C for medium temperature reaction for 2 hours, and finally heat to 89°C for high temperature reaction for 1 hour. After the reaction is completed, add distilled water and H2O2 with a mass of 65wt% of the total mass of the current system to the current system until the color of the solution turns bright yellow, centrifuge, filter, wash and dry to obtain the first product, then dissolve the first product in distilled water, and obtain intermediate I after ultrasonic treatment and freeze drying; S2: 1 g of intermediate I was added to 22 g of DMF, and the mixture was stirred to be uniform. Then, 0.12 g of phosphorus oxychloride was added and stirred at 18°C for 4 h for acyl chloride reaction. After the reaction was completed, the solvent was removed by distillation under reduced pressure to obtain intermediate II; S3: The intermediate II, 6,10-diphenyldodecanol and dichloromethane in a mass ratio of 1:0.5:22 were mixed evenly, and the esterification reaction was stirred at 45°C for 5 hours. After the reaction was completed, it was allowed to stand for 24 hours. After filtration, washing and drying, an asphaltene inhibitor based on modified graphene oxide was obtained.
[0040] Embodiment 5: A method for preparing an asphaltene inhibitor based on modified graphene oxide comprises the following steps: S1: Add graphite, NaNO3, and concentrated H2SO4 in a mass ratio of 1:1:41 to a dry three-necked flask, stir and mix evenly, then slowly add KMnO4 twice the mass of graphite in an ice bath, stir and react at low temperature for 2.5 hours at 1°C, then heat to 36°C for medium temperature reaction for 3 hours, and finally heat to 87°C for high temperature reaction for 1.5 hours. After the reaction is completed, add distilled water and H2O2 with a mass of 75wt% of the total mass of the current system to the current system until the color of the solution turns bright yellow, centrifuge, filter, wash and dry to obtain the first product, then dissolve the first product in distilled water, and obtain intermediate I after ultrasonic treatment and freeze drying; S2: 1 g of intermediate I was added to 21 g of acetonitrile, and the mixture was stirred to be uniform. Then, 0.1 g of phosphorus oxychloride was added and stirred at 17°C for 2.5 h for acyl chloride reaction. After the reaction was completed, the solvent was removed by distillation under reduced pressure to obtain intermediate II; S3: The intermediate II, 6,10-diphenyldodecanol and chloroform in a mass ratio of 1:0.35:21 were mixed evenly, and the esterification reaction was stirred at 42°C for 4 hours. After the reaction was completed, the mixture was allowed to stand for 24 hours, and an asphaltene inhibitor based on modified graphene oxide was obtained by filtration, washing and drying.
[0041] Embodiment 6: A method for preparing an asphaltene inhibitor based on modified graphene oxide comprises the following steps: S1: Add graphite, NaNO3, and concentrated H2SO4 in a mass ratio of 1:1.1:42 to a dry three-necked flask, stir and mix evenly, then slowly add KMnO4 with a mass 2.8 times that of graphite in an ice bath, stir and react at low temperature for 3 hours at 4°C, then heat to 39°C for medium temperature reaction for 2.5 hours, and finally heat to 90°C for high temperature reaction for 2 hours. After the reaction is completed, add distilled water and H2O2 with a mass of 70wt% of the total mass of the current system to the current system until the color of the solution turns bright yellow, centrifuge, filter, wash and dry to obtain the first product, then dissolve the first product in distilled water, and obtain intermediate I after ultrasonic treatment and freeze drying; S2: 1 g of intermediate I was added to 23 g of tetrahydrofuran, and the mixture was stirred to be uniform. Then, 0.18 g of phosphorus oxychloride was added and the mixture was stirred at 22°C for 4.5 h for acyl chloride reaction. After the reaction was completed, the solvent was removed by distillation under reduced pressure to obtain intermediate II; S3: Intermediate II, 6,10-diphenyldodecanol and tetrachloromethane in a mass ratio of 1:0.45:23 were mixed evenly, and the esterification reaction was stirred at 55°C for 5.5 hours. After the reaction was completed, it was allowed to stand for 24 hours. After filtration, washing and drying, an asphaltene inhibitor based on modified graphene oxide was obtained.
[0042] Embodiment 7: A method for preparing an asphaltene inhibitor based on modified graphene oxide comprises the following steps: S1: Add graphite, NaNO3, and concentrated H2SO4 in a mass ratio of 1:1.15:40 to a dry three-necked flask, stir and mix evenly, then slowly add KMnO4 with a mass 2.7 times that of graphite in an ice bath, stir and react at low temperature for 2.5 hours at 3°C, then heat to 38°C for medium temperature reaction for 3 hours, and finally heat to 88°C for high temperature reaction for 1.5 hours. After the reaction is completed, add distilled water and H2O2 with a mass of 65wt% of the total mass of the current system to the current system until the color of the solution turns bright yellow, centrifuge, filter, wash and dry to obtain the first product, then dissolve the first product in distilled water, and obtain intermediate I after ultrasonic treatment and freeze drying; S2: 1 g of intermediate I was added to 24 g of acetonitrile, and the mixture was stirred to be uniform. Then, 0.14 g of phosphorus oxychloride was added and stirred at 20°C for 3 h for acyl chloride reaction. After the reaction was completed, the solvent was removed by distillation under reduced pressure to obtain intermediate II; S3: The intermediate II, 6,10-diphenyldodecanol and dichloromethane in a mass ratio of 1:0.38:24 were mixed evenly, and the esterification reaction was stirred at 48°C for 4 hours. After the reaction was completed, it was allowed to stand for 24 hours, and an asphaltene inhibitor based on modified graphene oxide was obtained by filtration, washing and drying.
[0043] Embodiment 8: A method for preparing an asphaltene inhibitor based on modified graphene oxide comprises the following steps: S1: Add graphite, NaNO3, and concentrated H2SO4 in a mass ratio of 1:1.05:40 to a dry three-necked flask, stir and mix evenly, then slowly add KMnO4 with a mass 2.2 times that of graphite in an ice bath, stir and react at low temperature for 3 hours at 2°C, then heat to 35°C for medium temperature reaction for 2.5 hours, and finally heat to 87°C for high temperature reaction for 1 hour. After the reaction is completed, add distilled water and H2O2 with a mass of 70wt% of the total mass of the current system to the current system until the color of the solution turns bright yellow, centrifuge, filter, wash and dry to obtain the first product, then dissolve the first product in distilled water, and obtain intermediate I after ultrasonic treatment and freeze drying; S2: 1 g of intermediate I was added to 22 g of tetrahydrofuran, and the mixture was stirred to be uniform. Then, 0.12 g of phosphorus oxychloride was added and stirred at 18°C for 4.5 h for acyl chloride reaction. After the reaction was completed, the solvent was removed by distillation under reduced pressure to obtain intermediate II; S3: The intermediate II, 6,10-diphenyldodecanol and tetrachloromethane in a mass ratio of 1:0.4:22 were mixed evenly, and the esterification reaction was stirred at 50°C for 5 hours. After the reaction was completed, it was allowed to stand for 24 hours, and an asphaltene inhibitor based on modified graphene oxide was obtained by filtration, washing and drying.
[0044] Embodiment 9: A method for preparing an asphaltene inhibitor based on modified graphene oxide comprises the following steps: S1: Add graphite, NaNO3, and concentrated H2SO4 in a mass ratio of 1:1.2:42 to a dry three-necked flask, stir and mix evenly, then slowly add KMnO4 with a mass three times that of graphite in an ice bath, stir and react at low temperature for 3 hours at 4°C, then heat to 40°C for medium temperature reaction for 3 hours, and finally heat to 90°C for high temperature reaction for 2 hours. After the reaction is completed, add distilled water and H2O2 with a mass of 75wt% of the total mass of the current system to the current system until the color of the solution turns bright yellow, centrifuge, filter, wash and dry to obtain the first product, then dissolve the first product in distilled water, and obtain intermediate I after ultrasonic treatment and freeze drying; S2: 1 g of intermediate I was added to 26 g of DMF, and the mixture was stirred to be uniform. Then, 0.16 g of phosphorus oxychloride was added and the mixture was stirred at 23°C for 5 h for acyl chloride reaction. After the reaction was completed, the solvent was removed by distillation under reduced pressure to obtain intermediate II; S3: The intermediate II, 6,10-diphenyldodecanol and dichloromethane in a mass ratio of 1:0.5:26 were mixed evenly, and the esterification reaction was stirred at 60°C for 6 hours. After the reaction was completed, it was allowed to stand for 24 hours. After filtration, washing and drying, an asphaltene inhibitor based on modified graphene oxide was obtained.
[0045] Performance Characterization The modified graphene oxide asphaltene inhibitor prepared by the present invention can be applied to the oil field and used as a scale inhibitor.
[0046] The inhibitory effect of the modified graphene oxide asphaltene inhibitor prepared by the present invention is significantly better than that of the unmodified graphene oxide. The main reason is that the modified graphene oxide asphaltene inhibitor contains graphene oxide and a hydrophobic long side chain structure at the same time. The central graphene oxide has a condensed polyaromatic ring structure, and there is a π-π interaction between the asphaltene molecules, resulting in a strong adsorption fastness. The hydrophobic long side chain structure hinders the formation of a large parallel stacking structure, so that the asphaltene is stably dispersed and the appearance of organic scale is inhibited.
[0047] join Figure 1 This is a synthetic route map of the modified graphene oxide asphaltene inhibitor disclosed in the present invention; as can be seen from the figure, the mechanism of action of the modified graphene oxide asphaltene inhibitor disclosed in the present invention is to inhibit the mutual attraction and association between asphaltene molecules, thereby achieving the effect of inhibiting their coagulation. The central condensed ring structure of the modified graphene oxide asphaltene inhibitor can be strongly anchored on the surface of asphaltene under the effects of π-π, hydrogen bonding and hydrophobicity, and has the ability to adsorb at multiple points on the surface of asphaltene, which is conducive to forming a higher adsorption fastness. The hydrophobic chains at the edges can provide a steric hindrance effect between asphaltene molecules, effectively preventing the agglomeration of asphaltene molecules at the physical level, inhibiting their aggregation tendency, and then exerting the excellent dispersion inhibition effect of the inhibitor. Through the above effects, the inhibitor can successfully prevent further polymerization between asphaltene molecules and effectively control the coagulation tendency of asphaltene.
[0048] See also Figure 2 Schematic diagram of the inhibition mechanism of the modified graphene oxide asphaltene inhibitor disclosed in the present invention; Figure 2As shown, compared with common asphaltene inhibitors, the present invention uses natural graphite as a raw material to prepare graphene oxide, and sequentially modifies the graphene oxide by acyl chloride and 6,10-diphenyl dodecanol modification, so that the modified graphene oxide not only has a condensed polyaromatic ring structure, which can form a stable π-π interaction with the asphaltene molecules, but also has more hydrophobic side chains around it, which can effectively provide steric hindrance, increase the spacing between asphaltene molecules, and has good dispersibility and stability.
[0049] Taking Example 5 as an example, the prepared modified graphene oxide asphaltene inhibitor was characterized by infrared spectroscopy. The results are as follows: Figure 3 shown.
[0050] See also Figure 3 The infrared spectrum of the modified graphene oxide asphaltene inhibitor prepared in Example 5 disclosed in the present invention; Figure 3 It can be seen that 3300 cm - The absorption peak at ¹ corresponds to the stretching vibration of -OH; 3100 cm - The absorption peak at ¹ is the stretching vibration of the aromatic CH bond; 1735 cm - The absorption peak at ¹ is the stretching vibration of the -C=O bond; 1650 cm - The characteristic peak of the stretching vibration of the aromatic ring C=C bond appears at 1470 cm - The absorption peak at ¹ is caused by the bending vibration of the CH bond; 1150cm - The absorption peak at ¹ is the stretching vibration absorption of the C-OH bond. According to the infrared spectrum characteristics, it can be concluded that 6,10-diphenyl dodecanol has been successfully introduced into the intermediate II, indicating that the modified graphene oxide asphaltene inhibitor was successfully synthesized.
[0051] In order to characterize the effect of modified graphene oxide asphaltene inhibitor on the asphaltene dispersion inhibition effect, the asphaltene inhibitor and graphene oxide prepared in Examples 1, 2, 3, and 4 of the present invention were respectively used for dispersion stability test. The test method is: the inhibitor is dissolved in toluene at a mass ratio of 1:2 and dispersed for standby use. The heavy oil sample extracted from Changqing Oilfield has an asphaltene content of 17.1% and a density of 0.9707g / cm³. To determine its dispersion stability, 1g of heavy oil sample was taken, 13mL of n-heptane was added, and modified graphene oxide or graphene oxide with a concentration of 770 ppm was added. After stirring evenly, it was placed at different temperatures for 24h, and after centrifugation, the solid phase mass was measured to be m2. The dispersion stability calculation formula is: m1- m2 / m1. The experimental results are shown in Table 1.
[0052] Table 1 Dispersion stability test results under different temperature conditions
[0053] From the results in Table 1, it can be seen that the asphaltene inhibitors prepared in the examples of the present invention show significant advantages in terms of dispersion stability. Specifically, the dispersion stability of the asphaltene inhibitors in all examples exceeds 88%, which is significantly higher than the stability of graphene oxide. This shows that the inhibitors of the present invention have excellent effects in improving the dispersibility of asphaltene, and can not only effectively prevent the aggregation and precipitation of asphaltene, but also show excellent performance in maintaining its long-term stability.
[0054] In order to characterize the stabilizing effect of a modified graphene oxide asphaltene inhibitor on asphaltene, the stability of the modified graphene oxide asphaltene inhibitor prepared above was evaluated by the "water separation rate" method. Toluene was added to the above graphene oxide and the modified graphene oxide asphaltene inhibitor to prepare 8 mL of a solution with a mass concentration of 0.6 wt%, mixed evenly with 8 mL of heavy oil, added with 8 mL of distilled water, and then added to a stoppered graduated test tube and placed in a 90 ° C constant temperature box for 30 minutes, taken out and shaken evenly, and left to stand for 3 days. The volume of the water phase separated from the test tube was recorded, and the water separation rate E was calculated. d The water separation rate is calculated using the following formula, and the results are shown in Table 2: Water separation rate: Ed = V w / V×100%. Where V w is the amount of precipitated water, mL; V is the volume of the aqueous phase, mL.
[0055] Table 2 Comparison of water separation rates of inhibitors prepared in comparative examples and examples
[0056] From the results in Table 2, it can be seen that the water separation rate of the modified graphene oxide asphaltene inhibitor prepared by the present invention is significantly lower than that of graphene oxide, reaching a minimum of 19.5%, and has excellent stability, indicating that the modified graphene asphaltene inhibitor prepared by the present invention has a good inhibitory effect.
[0057] The invention discloses an asphaltene inhibitor based on modified graphene oxide, and a preparation method and application thereof. Graphite is made into graphene oxide, added into a first solvent, stirred and mixed evenly, and then phosphorus oxychloride is added and stirred to carry out acyl chloride reaction after obtaining a mixed solution. After the acyl chloride reaction is completed, the acyl chloride graphene oxide is obtained by vacuum distillation; then 6,10 diphenyl dodecanol and a second solvent are mixed evenly, acyl chloride graphene oxide is added and stirred to carry out substitution reaction, and the asphaltene inhibitor based on modified graphene oxide is obtained by rotary evaporation, washing, centrifugation and drying. The modified graphene oxide asphaltene inhibitor comprises graphene oxide and a hydrophobic long side chain structure. Graphene oxide has a fused polyaromatic ring structure, forms a π-π interaction with asphaltene molecules, and has a strong adsorption capacity. At the same time, the hydrophobic long side chain structure hinders the formation of a large parallel stacking structure, so that the asphaltene is stably dispersed, thereby effectively preventing the formation of organic scale and improving the efficiency of the inhibitor. The graphite used in the invention has a wide range of sources, low cost, easy degradation and environmental friendliness; its reaction process is simple and easy to control, and is suitable for large-scale production.
[0058] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing an asphaltene inhibitor based on modified graphene oxide, characterized in that: The following steps are involved: S1: Graphite, NaNO3 and concentrated H2SO4 were stirred and mixed evenly, KMnO4 was slowly added, and low-temperature reaction, medium-temperature reaction and high-temperature reaction were carried out in sequence, and then distilled water and H2O2 were added until bright yellow, and after centrifugation, filtration, washing and drying, the mixture was dissolved in distilled water, and after ultrasonication and freeze-drying, intermediate I was obtained; S2: adding intermediate I to the first solvent, mixing and stirring to react, then adding phosphorus oxychloride to carry out chlorination reaction, and after the reaction is completed, removing the solvent by reduced pressure distillation to obtain intermediate II; S3: The intermediate II, 6,10-diphenyl dodecanol and the second solvent are stirred and mixed uniformly, and after esterification reaction, the mixture is allowed to stand, filtered, washed and dried to obtain an asphaltene inhibitor based on modified graphene oxide.
2. The method for preparing an asphaltene inhibitor based on modified graphene oxide according to claim 1, characterized in that: In step S1, the mass ratio of graphite, NaNO3, concentrated H2SO4 and KMnO4 is 1:(1-1.2):(40-42):(2-3).
3. The method for preparing an asphaltene inhibitor based on modified graphene oxide according to claim 1, characterized in that: In step S1, the temperature of the low-temperature reaction is 0-5°C, and the reaction time is 2-3h; the temperature of the medium-temperature reaction is 35-40°C, and the reaction time is 2-3h; the temperature of the high-temperature reaction is 85-90°C, and the reaction time is 1-2h; the amount of distilled water added is 60-80wt% of the total mass of the system.
4. The method for preparing an asphaltene inhibitor based on modified graphene oxide according to claim 1, characterized in that: In step S2, the first solvent is any one of DMF, acetonitrile and tetrahydrofuran; the mass ratio of the intermediate I, phosphorus oxychloride and the first solvent is 1: (0.1-0.2): (20-30).
5. The method for preparing an asphaltene inhibitor based on modified graphene oxide according to claim 1, characterized in that: In step S2, the acyl chlorination reaction temperature is 15-25° C., and the reaction time is 2-5 h.
6. The method for preparing an asphaltene inhibitor based on modified graphene oxide according to claim 1, characterized in that: In step S3, the second solvent is any one of dichloromethane, chloroform and tetrachloromethane; the mass ratio of the intermediate II, 6,10-diphenyldodecanol and the second solvent is 1: (0.3-0.6): (20-30).
7. The method for preparing an asphaltene inhibitor based on modified graphene oxide according to claim 1, characterized in that: In step S3, the temperature of the esterification reaction is 40-60° C., the reaction time is 3-6 hours, and the standing time is 24 hours.
8. An asphaltene inhibitor based on modified graphene oxide, characterized in that: The method is prepared by the preparation method according to any one of claims 1 to 9, characterized in that the dispersion stability is 86.6% to 92.8% at 30°C; and the dispersion stability is 88.7% to 96.6% at 60°C.
9. The asphaltene inhibitor based on modified graphene oxide according to claim 8, characterized in that: The general structural formula is: 。 10. Use of the asphaltene inhibitor based on modified graphene oxide obtained by the preparation method according to any one of claims 1 to 8 as a scale inhibitor in an oil field, characterized in that: The water separation rate is 19.5%~22.8%.
Citation Information
Patent Citations
Composition as well as preparation method and application thereof
CN114106802A
Adsorbing or sensing method for anionic materials
KR1020170069062A
Preparation method of solid inhibitors of compound action for prevention of asphaltene-tarry-paraffin deposits and hydrating
RU2346021C1
Preparation method of solid inhibitor to prevent asphaltene-resin-paraffin deposits
RU2503703C1
Inhibition of asphaltene precipitation
WO2015175432A1