Metal catalyst, catalyst composition and application thereof
By introducing heteroaryl Ar with a specific structure into pyridine-amine hafnium catalyst and optimizing ligand design, the problems of insufficient heat resistance and catalytic activity of pyridine-amine hafnium catalyst under high temperature conditions were solved, realizing the preparation of polyolefins with high molecular weight and narrow molecular weight distribution and high α-olefin insertion rate, thus expanding the application potential of the catalyst.
Patent Information
- Application Number
- CN202411142015.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-20
AI Technical Summary
Existing pyridine-amine-based hafnium catalysts suffer from insufficient heat resistance and catalytic activity under high-temperature conditions. The catalytic polymers have low molecular weights and wide molecular weight distributions, low α-olefin insertion rates in the copolymers, and the catalyst structures are simple and lack scalability.
By introducing heteroaryl Ar with specific structures into metal catalysts, pyridine amine ligands are designed, and the ligand structure of the catalyst is optimized to improve its heat resistance and catalytic activity, especially exhibiting excellent performance under high temperature conditions. Metal catalysts are also prepared by reacting pyridine imine Schiff base compounds with heterocyclic metal compounds.
This method enables the catalytic preparation of polyolefins with high molecular weight and narrow molecular weight distribution at high temperatures, and significantly improves the insertion rate of α-olefins in olefin copolymers. The catalyst is easy to extend in structure and has broad prospects for industrial applications.
Smart Images

Figure CN119039494A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of olefin polymerization catalysis, and specifically relates to a metal catalyst, a catalyst composition and application thereof. Background Art
[0002] In the field of olefin polymerization, catalysts play a vital role. Their performance directly affects many key parameters of the polymer products, such as microstructure, molecular weight and stereoselectivity, and thus directly determines their performance. The discovery and use of metallocene catalysts began in the early 1950s, but the development was slow and has not received enough attention. The discovery of methylaluminoxane (MAO) in 1980 greatly improved the performance of metallocenes, so it has received widespread attention and also opened up researchers' pursuit of single-core catalysts. Metallocene catalysts can catalyze the preparation of various types of polyolefin products with high activity, including ethylene-propylene copolymers, ethylene and α-olefin copolymers, and polypropylene with different stereoregularities. However, metallocene catalysts are generally difficult to synthesize, with low yields and high costs. Therefore, various catalyst systems that do not contain metallocene have aroused widespread research interest, and a variety of catalytic systems with excellent performance have emerged.
[0003] In recent years, the pyridylamine hafnium catalyst developed by Dow has attracted attention in the industry for its excellent catalytic activity and heat resistance. The typical structure of the pyridylamine hafnium catalyst is Where X is a monovalent ligand group, and R is a methyl group, a phenyl group, a tert-butyl group, and a simple substituted group thereof; the catalyst can catalyze the polymerization of ethylene to obtain linear polyethylene, and catalyze the polymerization of propylene to obtain highly isotactic polypropylene. At the same time, the catalyst also shows good catalytic copolymerization performance, and can catalyze the copolymerization of ethylene and α-olefins to prepare polyolefin elastomers (POE); it can be used in combination with the FI-Zr catalyst developed by Mitsui Company to prepare olefin multi-block copolymers (OBC) with the assistance of a chain shuttling agent, and has been successfully industrialized. In addition, the pyridylamine-based hafnium catalyst also has good functional group tolerance and has been used to catalyze the copolymerization of ethylene or propylene with various monomers with functional groups.
[0004] Although pyridinylamine-based hafnium catalysts have achieved commercial success, their performance still has room for further improvement, such as poor heat resistance, obviously insufficient performance under high temperature conditions, low molecular weight of polymers obtained by catalytic polymerization, wide molecular weight distribution, and reduced insertion rate of copolymers. To this end, the academic and industrial communities have been exploring new catalyst design ideas and optimizing their structures, including focusing on their skeleton structures, aromatic amine groups, naphthalene rings, and reduced Schiff base groups, especially the first two. However, the improvement in catalytic performance is not obvious enough, and the structure of the catalyst is still relatively simple and lacks scalability. In addition, the industry has also proposed a bimetallic core catalyst based on pyridinylamine ligands. Although the heat resistance is improved compared to the mononuclear catalyst, the catalyst is not easy to purify, the molecular weight of the polymer obtained by catalysis is low, the molecular weight distribution is wide, and the insertion rate of α-olefin in ethylene and α-olefin copolymers is still low.
[0005] Based on this, it is an urgent problem to be solved in this field to develop a catalyst with high high-temperature catalytic activity that can catalyze the production of polyolefins with large molecular weight and narrow molecular weight distribution, while increasing the insertion rate of α-olefins in the copolymer products. Summary of the invention
[0006] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a metal catalyst, a catalyst composition and applications thereof. By designing the ligand molecular structure, the metal catalyst has excellent heat resistance and catalytic activity, especially high catalytic activity under high temperature conditions, and can catalyze the production of polyolefins with large molecular weight and narrow molecular weight distribution, and significantly improve the α-olefin insertion rate in olefin copolymers.
[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a metal catalyst having a structure as shown in Formula I:
[0009]
[0010] In formula I, the structure of Ar is -* represents the attachment site of the group; the dotted arc represents the conjugated double bond in the five-membered ring, that is, the structure of Ar is
[0011] D1, D2, and D3 are each independently selected from O, S, N, NR A1 or CR A2 Any of the following, not all of which are CR A2 .
[0012] D4 is selected from N or CR A3 Any one of .
[0013] RA1 , R A2 , R A3 , R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 , R 11 Each is independently selected from any one of hydrogen, halogen, substituted or unsubstituted C1-C30 straight or branched alkyl, substituted or unsubstituted C1-C30 alkoxy, substituted or unsubstituted C3-C30 cycloalkyl, substituted or unsubstituted C6-C30 aryl, substituted or unsubstituted C3-C30 heteroaryl, C1-C30 alkylsilyl and C1-C30 alkoxysilyl.
[0014] R A2 , R A3 Any two adjacent groups in R1, R2, R3, R4, R5, R6, R7, R8, and R9 are not connected or are connected to form a ring through a chemical bond.
[0015] In the present invention, “R A2 , R A3 , R1, R2, R3, R4, R5, R6, R7, R8, and R9 are each independently not connected to the adjacent ring structure" means that the aforementioned groups are only connected to the C atom through a single bond; "R A2 , R A3 "Any two adjacent groups among R1, R2, R3, R4, R5, R6, R7, R8 and R9 are connected to form a ring through a chemical bond" means that any two adjacent groups among the aforementioned groups are connected through a chemical bond to form a fused ring structure. When the same description is involved below, they all have the same meaning and will not be repeated one by one.
[0016] In formula I, X1 and X2 are each independently selected from any one of halogen, C1-C30 straight or branched alkyl, C6-C30 aryl, C7-C30 arylalkyl, C1-C30 alkylamino, and C6-C30 arylamino.
[0017] In formula I, M is selected from any one of the Group IVB metals.
[0018] The substituted substituents are each independently selected from at least one of halogen, unsubstituted or R'-substituted C1-C10 straight or branched alkyl, unsubstituted or R'-substituted C1-C10 alkoxy, and unsubstituted or R'-substituted C2-C10 alkenyl; R' is each independently selected from at least one of halogen and C6-C12 aryl.
[0019] In the present invention, the "substituted or unsubstituted" group may be substituted with one substituent or with multiple substituents. When there are multiple (at least 2) substituents, they may be the same or different substituents. When the same expressions are mentioned below, they have the same meaning. Unless otherwise specified, the selection range of the substituted substituents is as shown above and will not be repeated.
[0020] The molecular structure of the metal catalyst provided by the present invention is shown in Formula I. A heteroaryl Ar with a specific structure is introduced on the amine group and the pyridine bridging carbon atom. Through the structural design of the pyridine amine ligand, especially the introduction of the heteroaryl Ar at a specific site, the metal catalyst has significantly improved heat resistance and excellent catalytic activity on the basis of inheriting the advantages of the traditional pyridine amine hafnium catalyst, especially good high-temperature catalytic performance, can catalytically prepare polyolefins with high molecular weight and narrow molecular weight distribution, and effectively improves the insertion rate of α-olefins in olefin copolymers; in addition, the metal catalyst has good modifiability, is easy to expand and improve the structure, and has broad industrial application prospects.
[0021] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the objectives and beneficial effects of the present invention can be better achieved and realized.
[0022] In the present invention, the halogen includes fluorine, chlorine, bromine and iodine.
[0023] In the present invention, the C1-C30 straight chain or branched alkyl group can be a straight chain or branched alkyl group of C1, C2, C3, C4, C5, C6, C7, C8, C9, C10, C11, C12, C13, C14, C15, C16, C17, C18, C20, C22, C24, C25, C26, C28, etc., preferably a C1-C20 straight chain or branched alkyl group, further preferably a C1-C10 straight chain or branched alkyl group, illustratively including but not limited to: methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, 2-methylbutyl, n-pentyl, isopentyl, neopentyl, n-hexyl, neohexyl, 2-ethylhexyl, n-octyl, n-heptyl, n-nonyl, n-decyl, etc.
[0024] In the present invention, the C1-C30 alkoxy group can be a straight chain or branched chain alkoxy group of C1, C2, C3, C4, C5, C6, C7, C8, C9, C10, C11, C12, C13, C14, C15, C16, C17, C18, C20, C22, C24, C25, C26, C28, etc., preferably a C1-C20 alkoxy group, and more preferably a C1-C10 alkoxy group. A specific example is a monovalent group formed by connecting the above straight chain or branched chain alkyl group to O.
[0025] In the present invention, the C3-C30 cycloalkyl group can be a cycloalkyl group of C4, C5, C6, C7, C8, C9, C10, C11, C12, C13, C14, C15, C16, C17, C18, C20, C22, C24, C25, C26 or C28, including a monocyclic alkyl group or a polycyclic alkyl group, preferably a C3-C20 cycloalkyl group, further preferably a C3-C10 cycloalkyl group, illustratively including but not limited to: cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, adamantyl, etc.
[0026] In the present invention, the C6-C30 aromatic groups can be aromatic groups of C6, C9, C10, C12, C14, C16, C18, C20, C22, C24, C26 or C28, and C6-C20 aromatic groups are further preferred, including monocyclic aromatic groups and condensed-ring aromatic groups, illustratively including but not limited to phenyl, biphenyl, terphenyl, naphthyl, anthracenyl, phenanthryl, etc.
[0027] In the present invention, the C3-C30 heteroaryl group can be a heteroaryl group of C3, C4, C5, C6, C9, C10, C12, C14, C16, C18, C20, C22, C24, C26 or C28, preferably a C3-C20 heteroaryl group, wherein the heteroatom can be N, O, S, etc.; including a monocyclic heteroaryl group or a condensed ring heteroaryl group, illustratively including but not limited to: pyridyl, pyrimidinyl, pyrazinyl, pyridazinyl, triazine, furanyl, thienyl, pyrrolyl, quinolyl, isoquinolyl, quinoxalinyl, quinazolinyl, benzofuranyl, benzothienyl, indolyl, dibenzofuranyl, dibenzothienyl, carbazolyl, N-phenylcarbazolyl, etc.
[0028] In the present invention, the C1-C30 alkylsilyl groups may be alkylsilyl groups of C3, C4, C5, C6, C7, C8, C9, C10, C11, C12, C13, C14, C15, C16, C17, C18, C20, C22, C24, C25, C26, C28, etc., which are monovalent groups in which at least one hydrogen in -SiH3 is replaced by the above-mentioned straight-chain or branched alkyl groups.
[0029] In the present invention, the C1-C30 alkoxysilyl groups can all be alkoxysilyl groups of C3, C4, C5, C6, C7, C8, C9, C10, C11, C12, C13, C14, C15, C16, C17, C18, C20, C22, C24, C25, C26, C28, etc., which are monovalent groups in which at least one hydrogen in -SiH3 is replaced by the above-mentioned alkoxy group.
[0030] In the present invention, the C7-C30 aryl alkyl group can be an aryl alkyl group of C8, C9, C10, C11, C12, C13, C14, C15, C16, C17, C18, C20, C22, C24, C25, C26, C28, etc., and a specific example is a monovalent group formed by connecting the above aryl groups to a straight-chain or branched alkyl group, and a typical example is benzyl (phenylmethyl).
[0031] In the present invention, the C1-C30 alkylamino group can be an alkylamino group of C3, C4, C5, C6, C7, C8, C9, C10, C11, C12, C13, C14, C15, C16, C17, C18, C20, C22, C24, C25, C26, C28, etc., which is a monovalent group in which at least one hydrogen in -NH2 is replaced by the above-mentioned straight-chain or branched alkyl group.
[0032] In the present invention, the C6-C30 arylamino group can be an arylamino group of C6, C9, C10, C12, C14, C16, C18, C20, C22, C24, C26 or C28, which is a monovalent group in which at least one hydrogen in -NH2 is replaced by the above aryl group.
[0033] In the present invention, the C1-C10 straight chain or branched alkyl group can be a straight chain or branched alkyl group of C1, C2, C3, C4, C5, C6, C7, C8, C9, C10, illustratively including but not limited to: methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, 2-methylbutyl, n-pentyl, isopentyl, neopentyl, n-hexyl, neohexyl, 2-ethylhexyl, n-octyl, n-heptyl, n-nonyl, n-decyl, etc.
[0034] In the present invention, the C1-C10 alkoxy groups can be straight-chain or branched alkoxy groups of C1, C2, C3, C4, C5, C6, C7, C8, C9, or C10, and specific examples include monovalent groups formed by connecting the above straight-chain or branched alkyl groups to O.
[0035] In the present invention, the C2-C10 alkenyl groups may be straight or branched alkenyl groups of C2, C3, C4, C5, C6, C7, C8, C9, or C10, containing at least one C=C, including but not limited to vinyl, propenyl, allyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, butadienyl, pentadienyl, and the like.
[0036] In the present invention, the C6-C12 aryl groups may be aryl groups of C6, C9, C10, C12, etc., illustratively including but not limited to phenyl, biphenyl, naphthyl, etc.
[0037] Preferably, any two adjacent groups among R1, R2, R3, R4, R5, R6, R7, R8, and R9 are not connected or are connected by a chemical bond to form a ring Cy1; the ring Cy1 is selected from substituted or unsubstituted C3-C20 (for example, C3, C4, C5, C6, C7, C8, C9, C10, C11, C12, C13, C14, C15, C16, C17 or C18, etc.) alicyclic, substituted or unsubstituted C6-C20 (for example, C6, C9, C10, C12, C14 , C16, C18, etc.) aromatic ring, substituted or unsubstituted C3-C20 (for example, C3, C4, C5, C6, C7, C8, C9, C10, C11, C12, C13, C14, C15, C16, C17 or C18, etc.) heteroaromatic ring, further preferably substituted or unsubstituted C3-C8 alicyclic ring, substituted or unsubstituted C6-C10 aromatic ring, substituted or unsubstituted C3-C8 heteroaromatic ring; the heteroatoms in the heteroaromatic ring include at least one of O, S or N.
[0038] Preferably, any two adjacent groups among R1, R2, R3, R4, R5, R6, R7, R8 and R9 are not connected or are connected by a chemical bond to form a benzene ring.
[0039] Preferably, the metal catalyst has a structure as shown in Formula II:
[0040]
[0041] In Formula II, Ar, R1, R2, R3, R4, R5, R 10 , R 11 , X1, X2, and M have the same defined ranges as in Formula I.
[0042] Preferably, R1 and R5 are each independently selected from any one of C1-C10 (e.g., C2, C3, C4, C5, C6, C7, C8, C9, etc.) straight chain or branched chain alkyl groups, more preferably C1-C6 straight chain or branched chain alkyl groups, and even more preferably isopropyl.
[0043] As a preferred technical solution of the present invention, the R 11 Any one selected from hydrogen or a simple less hindered group, such as hydrogen, C1-C10 (e.g. C2, C3, C4, C5, C6, C7, C8, C9, etc.) straight chain or branched alkyl, C6-C20 (e.g. C6, C9, C10, C12, C14, C16, C18, etc.) aryl, more preferably hydrogen, methyl, ethyl, n-propyl, n-butyl, tert-butyl, phenyl, more preferably hydrogen.
[0044] As a preferred technical solution of the present invention, the R2, R4, R10 Each is independently selected from any one of hydrogen, halogen, substituted or unsubstituted C1-C10 (for example, C2, C3, C4, C5, C6, C7, C8 or C9, etc.) straight chain or branched alkyl, substituted or unsubstituted C1-C10 (for example, C2, C3, C4, C5, C6, C7, C8 or C9, etc.) alkoxy, substituted or unsubstituted C6-C20 (for example, C6, C9, C10, C12, C14, C16 or C18, etc.) aryl.
[0045] Preferably, R2, R4, R 10 and R 11 For hydrogen.
[0046] Preferably, the metal catalyst has a structure as shown in Formula III:
[0047]
[0048] Wherein, Ar, R3, X1, X2, and M have the same defined ranges as in Formula I.
[0049] Preferably, R3 is selected from any one of hydrogen, halogen, C1-C10 (e.g., C2, C3, C4, C5, C6, C7, C8, C9, etc.) straight chain or branched alkyl, C1-C10 (e.g., C2, C3, C4, C5, C6, C7, C8, C9, etc.) alkoxy, further preferably any one of hydrogen, halogen, C1-C6 straight chain or branched alkyl, C1-C6 alkoxy, further preferably hydrogen, fluorine, chlorine, methyl or methoxy.
[0050] Preferably, in Ar, 1-3 (e.g., 1, 2 or 3) of D1, D2, D3 and D4 are O, S, N, NR A1 , the rest are CR A2 or CR A3 , R A2 , R A3 Any two adjacent groups in the above-mentioned are not connected or are connected to form a ring by a chemical bond; thereby, Ar is any one of the following substituted or unsubstituted groups: pyrrolyl, furyl, thienyl, oxazolyl, isoxazolyl, thiazolyl, isothiazolyl, pyrazolyl, imidazolyl, indolyl, benzothienyl, benzofuranyl, triazolyl, etc.
[0051] Preferably, the structure of Ar is -* represents the attachment site of the group;
[0052] D1 is selected from O, S or NR A1 Any of the following;
[0053] R A1Any one selected from hydrogen, halogen, substituted or unsubstituted C1-C30 straight or branched alkyl, substituted or unsubstituted C1-C30 alkoxy, substituted or unsubstituted C3-C30 cycloalkyl, substituted or unsubstituted C6-C30 aryl, substituted or unsubstituted C3-C30 heteroaryl, C1-C30 alkylsilyl, C1-C30 alkoxysilyl, further preferably hydrogen, substituted or unsubstituted C1-C10 (e.g., C2, C3, C4, C5, C6, C7, C8, C9, etc.) straight or branched alkyl, substituted or unsubstituted C6-C20 (e.g., C6, C9, C10, C12, C14, C16, C18, etc.) aryl, further preferably hydrogen, C1-C6 straight or branched alkyl, phenyl, biphenyl, naphthyl.
[0054] R A Each is independently selected from any one of halogen, substituted or unsubstituted C1-C30 straight or branched alkyl, substituted or unsubstituted C1-C30 alkoxy, substituted or unsubstituted C3-C30 cycloalkyl, substituted or unsubstituted C6-C30 aryl, substituted or unsubstituted C3-C30 heteroaryl, C1-C30 alkylsilyl, and C1-C30 alkoxysilyl; any two adjacent R A They are not connected to each other or are connected to form a ring through chemical bonds.
[0055] The substituted substituents are each independently selected from at least one of halogen, unsubstituted or R'-substituted C1-C10 straight or branched alkyl, unsubstituted or R'-substituted alkoxy, and unsubstituted or R'-substituted C2-C10 alkenyl; R' is each independently selected from at least one of halogen and C6-C12 aryl.
[0056] n represents a substituent R A The number of R is selected from an integer of 0-4, for example, 0, 1, 2, 3 or 4; when n≥2, multiple (at least 2) R A are the same or different groups.
[0057] Preferably, the R Aeach independently selected from halogen, substituted or unsubstituted C1-C10 (e.g. C2, C3, C4, C5, C6, C7, C8, C9, etc.) straight or branched alkyl, substituted or unsubstituted C1-C10 (e.g. C2, C3, C4, C5, C6, C7, C8, C9, etc.) alkoxy, substituted or unsubstituted C3-C10 (e.g. C4, C5, C6, C7, C8, C9, etc.) cycloalkyl, substituted or unsubstituted C6-C20 (e.g. C6, C9, C10, Any one of C12, C14, C15, C16 or C18) aryl, substituted or unsubstituted C3-C20 (e.g., C3, C4, C5, C6, C9, C10, C12, C14, C15, C16 or C18) heteroaryl, C1-C10 (e.g., C2, C3, C4, C5, C6, C7, C8, C9, etc.) alkylsilyl, C1-C10 (e.g., C2, C3, C4, C5, C6, C7, C8, C9, etc.) alkoxysilyl;
[0058] Preferably, any two adjacent R A are not connected or connected by chemical bonds to form a ring Cy2; the ring Cy2 is selected from a substituted or unsubstituted C3-C20 (e.g., C3, C4, C5, C6, C7, C8, C9, C10, C11, C12, C13, C14, C15, C16, C17 or C18, etc.) alicyclic ring, a substituted or unsubstituted C6-C20 (e.g., C6, C9, C10, C12, C14, C16, C18, etc.) aromatic ring, a substituted or unsubstituted C The present invention relates to any one of C3-C20 (for example, C3, C4, C5, C6, C7, C8, C9, C10, C11, C12, C13, C14, C15, C16, C17 or C18) heteroaromatic rings, and further preferably any one of substituted or unsubstituted C3-C8 alicyclic rings, substituted or unsubstituted C6-C10 aromatic rings, and substituted or unsubstituted C3-C8 heteroaromatic rings; the heteroatoms in the heteroaromatic rings include at least one of O, S or N.
[0059] Further preferably, any two adjacent R A They are not connected or connected to form benzene rings through chemical bonds.
[0060] Preferably, Ar is selected from any one of the following groups:
[0061]
[0062] Among them, R A4 , R A5 , R A6Each is independently selected from any one of hydrogen, halogen, substituted or unsubstituted C1-C30 straight or branched alkyl, substituted or unsubstituted C1-C30 alkoxy, substituted or unsubstituted C3-C30 cycloalkyl, substituted or unsubstituted C6-C30 aryl, substituted or unsubstituted C3-C30 heteroaryl, C1-C30 alkylsilyl, and C1-C30 alkoxysilyl, and is more preferably hydrogen, halogen, substituted or Any one of unsubstituted C1-C10 (e.g., C2, C3, C4, C5, C6, C7, C8, C9, etc.) straight chain or branched alkyl, substituted or unsubstituted C1-C10 (e.g., C2, C3, C4, C5, C6, C7, C8, C9, etc.) alkoxy, substituted or unsubstituted C6-C20 (e.g., C6, C9, C10, C12, C14, C16, C18, etc.) aryl.
[0063] Preferably, R A4 , R A5 , R A6 The substituents substituted in the above-mentioned are each independently selected from halogen, unsubstituted or R'-substituted C1-C10 (e.g., C2, C3, C4, C5, C6, C7, C8, C9, etc.) straight or branched alkyl, unsubstituted or R'-substituted C1-C10 (e.g., C2, C3, C4, C5, C6, C7, C8, C9, etc.) alkoxy, unsubstituted or R'-substituted C2-C10 (e.g., C3, C4, C5, C6, C7, C8, C9, etc.) R' is independently selected from at least one of halogen, C6-C12 (such as C6, C9, C10, C12, etc.) aryl; further preferably, the substituted substituents are independently selected from any one of halogen (fluorine, chlorine, bromine, iodine), unsubstituted or halogenated C1-C6 straight or branched alkyl, unsubstituted or halogenated C1-C6 alkoxy, unsubstituted or halogenated C2-C6 alkenyl, di(phenyl)alkenyl.
[0064] Further preferably, Ar is selected from any one of the following groups:
[0065]
[0066] Wherein, -* represents the attachment site of the group.
[0067] R A1Each is independently selected from any one of hydrogen, substituted or unsubstituted C1-C10 (e.g., C2, C3, C4, C5, C6, C7, C8, C9, etc.) straight chain or branched alkyl, substituted or unsubstituted C6-C20 (e.g., C6, C9, C10, C12, C14, C16, C18, etc.) aryl, further preferably any one of hydrogen, C1-C6 straight chain or branched alkyl, phenyl, biphenyl, naphthyl, further preferably hydrogen, methyl, ethyl, propyl, isopropyl, n-butyl, tert-butyl, isobutyl or phenyl.
[0068] R A4 , R A5 Each is independently selected from any one of hydrogen, halogen, substituted or unsubstituted C1-C10 (e.g. C2, C3, C4, C5, C6, C7, C8, C9, etc.) straight chain or branched alkyl, substituted or unsubstituted C1-C10 (e.g. C2, C3, C4, C5, C6, C7, C8, C9, etc.) alkoxy, substituted or unsubstituted C6-C20 (e.g. C6, C9, C10, C12, C14, C16, C18, etc.) aryl.
[0069] Preferably, R A4 , R A5 The substituents substituted in the above-mentioned are each independently selected from halogen, unsubstituted or R'-substituted C1-C10 (e.g., C2, C3, C4, C5, C6, C7, C8, C9, etc.) straight or branched alkyl, unsubstituted or R'-substituted C1-C10 (e.g., C2, C3, C4, C5, C6, C7, C8, C9, etc.) alkoxy, unsubstituted or R'-substituted C2-C10 (e.g., C3, C4, C5, C6, C7, C8, C9, etc.) R' is independently selected from at least one of halogen, C6-C12 (such as C6, C9, C10, C12, etc.) aryl; further preferably, the substituted substituents are independently selected from any one of halogen (fluorine, chlorine, bromine, iodine), unsubstituted or halogenated C1-C6 straight or branched alkyl, unsubstituted or halogenated C1-C6 alkoxy, unsubstituted or halogenated C2-C6 alkenyl, di(phenyl)alkenyl.
[0070] More preferably, R A4 , R A5 Each is independently selected from hydrogen, halogen, unsubstituted or halogenated C1-C6 (e.g. C2, C3, C4, C5, C6, etc.) straight or branched alkyl, unsubstituted or halogenated C1-C6 (e.g. C2, C3, C4, C5, C6, etc.) alkoxy, phenyl, Any one of; Ph represents phenyl, -* represents the connection site of the group.
[0071] Preferably, the M is selected from any one of titanium, zirconium and hafnium, and hafnium is more preferably selected.
[0072] Preferably, the metal catalyst has any one of the following structures:
[0073]
[0074]
[0075] Preferably, X1 and X2 are each independently selected from any one of halogen (fluorine, chlorine, bromine, iodine), C1-C10 (e.g., C2, C3, C4, C5, C6, C7, C8, C9, etc.) straight chain or branched alkyl, benzyl, C1-C10 (e.g., C2, C3, C4, C5, C6, C7, C8, C9, etc.) alkylamino, C6-C20 (e.g., C6, C9, C10, C12, C14, C16, C18, etc.) arylamino, and more preferably any one of halogen, methyl, benzyl, and dimethylamino.
[0076] In a second aspect, the present invention provides a method for preparing the metal catalyst as described in the first aspect, the preparation method comprising the following steps:
[0077] (1) A heterocyclic metal compound of the structure represented by formula A reacts with a pyridine imine Schiff base compound of the structure represented by formula B to obtain a pyridine amine ligand of the structure represented by formula C. The reaction formula is as follows:
[0078]
[0079] Among them, Ar, R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 , R 11 , X1, X2 and M have the same defined ranges as in Formula I;
[0080] Y is selected from any one of Li or Mg-Hal, and Hal is selected from any one of halogens;
[0081] (2) After the pyridylamine ligand undergoes a first reaction with a hydrogen abstraction reagent, it undergoes a second reaction with a metal M source to obtain the metal catalyst having a structure as shown in Formula I.
[0082] Preferably, the preparation method of the heterocyclic metal compound comprises: reacting a heterocyclic compound of a structure represented by formula AS with a lithium reagent or metal magnesium to obtain the heterocyclic metal compound of a structure represented by formula A, and the reaction formula is as follows:
[0083]
[0084] Among them, Y2 is selected from any one of hydrogen or halogen, and more preferably hydrogen or bromine.
[0085] As a preferred technical solution of the present invention, the heterocyclic metal compound of the structure shown in formula A can be a lithium salt obtained by reacting a heterocyclic compound of the structure shown in formula AS with a lithium reagent (such as metallic lithium, alkyl lithium, lithium amide) (Y in formula A is Li); or, the heterocyclic metal compound of the structure shown in formula A can be a Grignard reagent obtained by reacting a heterocyclic compound of the structure shown in formula AS with metallic magnesium (Y in formula A is Mg-Hal, Hal is a halogen).
[0086] Preferably, the preparation method of the heterocyclic metal compound comprises: subjecting the heterocyclic compound with the structure shown in Formula AS to a halogen-lithium exchange reaction with a lithium reagent to obtain the heterocyclic metal compound with the structure shown in Formula A.
[0087] Preferably, the temperature of the halogen-lithium exchange reaction is <0°C, for example, it can be -90°C, -85°C, -80°C, -78°C, -75°C, -70°C, -60°C, -50°C, -40°C, -30°C, -25°C, -10°C, -5°C or -2°C, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0088] Preferably, the alkyl lithium includes any one of n-butyl lithium, methyl lithium, and tert-butyl lithium, or a combination of at least two of them.
[0089] Preferably, the lithium amide comprises lithium bis(trimethylsilyl)amide.
[0090] In addition, the Ar (five-membered ring) contains halogen, that is, R A2 , R A3 , R A4 , R A5 , R A6 and R A When at least one of the halogens is halogen, preferably bromine, after the heterocyclic metal compound of the structure represented by formula A in step (1) reacts with the pyridine imine Schiff base compound of the structure represented by formula B, bromine is retained and can be used for coupling reaction with other organic compounds to achieve further derivatization of the ligand. The organic compound is any one of an organoboron compound, an organotin compound, an organomagnesium compound, an organozinc compound, an organoaluminum compound, an organosilicon compound, an organothalium compound, and a double bond-containing compound, preferably an organoboron compound or an organozinc compound.
[0091] In the present invention, the pyridine imine Schiff base compound of the structure shown in formula B can be prepared by referring to the method disclosed in the prior art. As a preferred technical solution of the present invention, it can be prepared by referring to the multi-step reaction disclosed in CN100381475C. Specifically, the pyridine compound of the structure shown in formula B-1 and the aromatic amine compound of the structure shown in formula B-2 are subjected to Schiff base condensation reaction under acidic conditions, and then subjected to Suzuki coupling reaction with the aromatic boronic acid compound of the structure shown in formula B-3 to obtain the compound; the reaction formula is as follows:
[0092]
[0093] As another preferred technical solution of the present invention, the pyridine imine Schiff base compound of the structure shown in formula B can be obtained by subjecting the compound of the structure shown in formula B-S2 and the aromatic amine compound of the structure shown in formula B-2 to a Schiff base condensation reaction under acidic conditions, and the reaction formula is as follows:
[0094]
[0095] Preferably, the compound of the structure shown in formula B-S2 can be purchased or obtained by Suzuki coupling reaction, and the reaction formula is as follows:
[0096]
[0097] Wherein, Hal2 is selected from any one of the halogens, for example, it can be Br.
[0098] Preferably, the temperature of the reaction in step (1) is ≤50°C, for example, it can be -90°C, -85°C, -80°C, -78°C, -75°C, -70°C, -60°C, -50°C, -40°C, -30°C, -25°C, -10°C, -5°C, 0°C, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 38°C, 40°C, 45°C or 48°C, as well as specific values between the above points. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific points included in the range; further preferably, -10°C to room temperature.
[0099] Preferably, the reaction time of step (1) is 0.5-24 h, for example, it can be 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 12 h, 14 h, 15 h, 16 h, 18 h, 20 h or 22 h, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0100] Preferably, the hydrogen abstraction reagent includes any one or a combination of at least two of potassium hydride, sodium hydride, lithium hydride, lithium bistrimethylsilylamide, sodium bistrimethylsilylamide, lithium diisopropylamide, and C1-C6 (e.g., C2, C3, C4, C5, etc.) alkyl lithiums, and further preferably any one or a combination of at least two of sodium hydride, potassium hydride, and C1-C6 alkyl lithiums.
[0101] Preferably, the temperature of the first reaction in step (2) is ≤25°C, for example, it can be -80°C, -78°C, -75°C, -70°C, -60°C, -50°C, -40°C, -30°C, -25°C, -10°C, -5°C, 0°C, 5°C, 10°C, 15°C, 20°C or 22°C, as well as specific values between the above points. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively enumerates the specific points included in the range; room temperature is further preferred.
[0102] Preferably, the time of the first reaction in step (2) is 0.1-12 h, for example, it can be 0.5 h, 0.8 h, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h, 6 h, 7 h, 8 h, 9 h, 10 h or 11 h, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the said range.
[0103] Preferably, the metal M source includes a metal M salt, such as any one of Group IVB metal halides, amino compounds, alkyl compounds, alkylamino compounds, aryl compounds, benzyl compounds, or a combination of at least two thereof.
[0104] Preferably, the metal M source illustratively includes but is not limited to: titanium tetrachloride, zirconium tetrachloride, hafnium tetrachloride, bis(dimethylamino)titanium dichloride, bis(diethylamino)zirconium dichloride, tetrakis(dimethylamino)hafnium.
[0105] Exemplarily, the method of the second reaction includes: the hydrogen abstraction product of the pyridineamine ligand directly reacts with a metal M source to obtain the heterocyclic metal compound with the structure shown in formula A; or, the hydrogen abstraction product of the pyridineamine ligand reacts with a halide of a Group IVB metal and then undergoes an alkylation reaction to obtain the heterocyclic metal compound with the structure shown in formula A.
[0106] Preferably, the temperature of the second reaction in step (2) is 50-150°C, for example, it can be 55°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C or 145°C, as well as specific values between the above points. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific points included in the range, and 100-145°C is further preferred.
[0107] Preferably, the time of the second reaction in step (2) is 1-12 h, for example, it can be 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h, 6 h, 8 h, 10 h or 11 h, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively enumerates the specific point values included in the range, and 2-6 h is further preferred.
[0108] Preferably, the alkylating agent used in the alkylation reaction comprises at least one of an alkyl Grignard reagent and an alkyl aluminum, more preferably an alkyl Grignard reagent, and more preferably methyl magnesium bromide (MeMgBr).
[0109] Preferably, the temperature of the alkylation reaction is ≤50°C, for example, it can be -10°C, -5°C, 0°C, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 38°C, 40°C, 45°C or 48°C, as well as specific values between the above points. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively enumerates the specific points included in the range, and room temperature is further preferred.
[0110] Preferably, the alkylation reaction time is 0.1-24 h, for example, it can be 0.5 h, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h, 6 h, 8 h, 10 h, 12 h, 14 h, 15 h, 16 h, 18 h, 20 h or 22 h, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively enumerates the specific point values included in the range.
[0111] In a third aspect, the present invention provides a catalyst composition, the catalyst composition comprising a main catalyst and a co-catalyst, the main catalyst comprising at least one of the metal catalysts described in the first aspect.
[0112] Preferably, the co-catalyst comprises any one of an alkyl aluminum compound, an organic aluminum oxide compound, and a boron salt, or a combination of at least two thereof.
[0113] Preferably, the alkyl aluminum compound includes any one of trimethyl aluminum, triethyl aluminum, triisobutyl aluminum, tri-n-hexylaluminum, trioctylaluminum, or a combination of at least two thereof.
[0114] Preferably, the organic aluminum oxide compound includes any one of methylaluminoxane, ethylaluminoxane, isobutylaluminoxane, and alkylaluminum-modified methylaluminoxane, or a combination of at least two thereof.
[0115] Preferably, the boron salt includes any one of tris(pentafluorophenyl)boron, triphenylcarbonium tetra(pentafluorophenyl)boron, tetra(pentafluorophenyl)boric acid-methyldi-(octadecyl)ammonium salt, and N,N-dimethylanilinium tetra(pentafluorophenyl)borate, or a combination of at least two thereof.
[0116] As a preferred technical solution of the present invention, the co-catalyst includes a boron salt, and an alkyl aluminum compound can be used as an impurity scavenger.
[0117] Preferably, the molar ratio of the metal Al in the co-catalyst to the metal M in the main catalyst is (10-5000):1, for example, it can be 20:1, 50:1, 80:1, 100:1, 200:1, 300:1, 500:1, 600:1, 800:1, 1000:1, 1500:1, 2000:1, 2500:1, 3000:1, 3500:1, 4000:1, 4500:1 or 4800:1, further preferably (30-1000):1, and even more preferably (40-100):1.
[0118] Preferably, the molar ratio of the B element in the co-catalyst to the metal M in the main catalyst is (1-2):1, for example, it can be 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1 or 1.9:1, etc., and more preferably (1-1.5):1.
[0119] In a fourth aspect, the present invention provides a use of the metal catalyst as described in the first aspect and the catalyst composition as described in the third aspect in catalyzing olefin polymerization.
[0120] Preferably, the olefin polymerization includes olefin homopolymerization or ethylene / α-olefin copolymerization.
[0121] Wherein, the olefin homopolymerization comprises homopolymerization of any one of ethylene and α-olefins, and the α-olefins comprise propylene, 1-butene, 1-hexene, 1-octene, 4-methyl-1-pentene, C10-C30 (e.g., C11, C12, C13, C14, C15, C16, C17, C18, C19, C20, C22, C23, C24, C25, C26, C28, etc.) linear α-olefins, C10-C30 (e.g., C11, C12, C13, C14, C15, C16, C17, C18, C19, C20, C22, C23, C24, C25, C26, C28, etc.) branched α-olefins, any one of the aforementioned α-olefins with double bonds, functional groups containing nitrogen, oxygen, boron, aluminum, phosphorus, and halogen, or a combination of at least two thereof.
[0122] In a fifth aspect, the present invention provides a method for preparing a polyolefin, the method comprising: polymerizing an olefin monomer in the presence of a catalyst to obtain the polyolefin;
[0123] The catalyst comprises at least one of the metal catalyst described in the first aspect and the catalyst composition described in the third aspect.
[0124] Preferably, the olefin monomer comprises ethylene and / or α-olefin.
[0125] Preferably, the α-olefin includes any one or a combination of at least two of propylene, 1-butene, 1-hexene, 1-octene, 4-methyl-1-pentene, C10-C30 (e.g., C11, C12, C13, C14, C15, C16, C17, C18, C19, C20, C22, C23, C24, C25, C26, C28, etc.) linear α-olefins, and C10-C30 (e.g., C11, C12, C13, C14, C15, C16, C17, C18, C19, C20, C22, C23, C24, C25, C26, C28, etc.) branched α-olefins.
[0126] Preferably, the α-olefin further comprises any one or a combination of at least two of the aforementioned α-olefins having a double bond, or a functional group containing nitrogen, oxygen, boron, aluminum, phosphorus, or halogen.
[0127] Preferably, the polymerization reaction is carried out in the presence of an organic solvent.
[0128] Preferably, the organic solvent comprises any one or a combination of at least two of an alkane solvent, a halogenated alkane solvent, a cycloalkane solvent, and an aromatic solvent, and more preferably any one or a combination of at least two of Isopar E, n-hexane, heptane, toluene, and xylene.
[0129] Preferably, the polymerization reaction temperature is 0-200°C, for example, it can be 5°C, 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C or 190°C, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively enumerates the specific point values included in the range, and 100-160°C is further preferred.
[0130] Preferably, the polymerization reaction pressure is 0.1-10 MPa, for example, it can be 0.2 MPa, 0.5 MPa, 0.8 MPa, 1 MPa, 1.5 MPa, 2 MPa, 2.5 MPa, 3 MPa, 3.5 MPa, 4 MPa, 4.5 MPa, 5 MPa, 5.5 MPa, 6 MPa, 7 MPa, 8 MPa or 9 MPa, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range, and 0.5-5 MPa is further preferred.
[0131] As a preferred technical solution of the present invention, the metal catalyst is used to catalyze the homopolymerization reaction of olefin monomers, has excellent catalytic activity and thermal stability, and the obtained olefin homopolymer has a high molecular weight, a narrow molecular weight distribution, and exhibits the characteristics of high linearity and high melting point.
[0132] Preferably, the metal catalyst (catalyst composition) of the present invention is used to catalyze the preparation of polyethylene at a high temperature (≥110° C.), so that the molecular weight of the polyethylene is high and the weight average molecular weight (M w ) can be 18.4×10 4 g / mol, and the molecular weight distribution is narrow, the molecular weight distribution index (PDI) ≤ 2.6; catalytic activity ≥ 10 7 g / mol·h, especially the catalytic activity at 130℃≥10 7 g / mol·h.
[0133] As another preferred technical solution of the present invention, the metal catalyst is used to catalyze the copolymerization reaction of ethylene and α-olefin, has excellent catalytic activity and thermal stability, and the copolymerization product has a high α-olefin insertion rate and has the properties of a polyolefin elastomer.
[0134] Preferably, the metal catalyst of the present invention is used to catalyze the preparation of ethylene-octene copolymer at high temperature (e.g., 130° C.), and the obtained ethylene-octene copolymer has a high molecular weight and a weight average molecular weight (M w )≥4.2×10 4 g / mol,M w It can be 4.2×10 4 -5.3×10 4 g / mol, narrow molecular weight distribution, PDI ≤ 2.7, insertion rate of 1-octene monomer ≥ 32.5wt%, can be 32.5-53.9wt%. Catalytic activity > 1.7×10 7 g / mol·h.
[0135] Compared with the prior art, the present invention has the following beneficial effects:
[0136] (1) The metal catalyst provided by the present invention has a structure as shown in Formula I, and a heteroaryl group Ar with a specific structure is introduced on the amine group and the pyridine bridging carbon atom. Through the structural design of the ligand, the metal catalyst has excellent heat resistance and catalytic activity, especially good high-temperature catalytic performance, and can catalytically prepare olefin polymers with high molecular weight and narrow molecular weight distribution, and significantly improve the insertion rate of α-olefin monomers in olefin copolymers; in addition, the metal catalyst is easy to expand its structure and has broad industrial application prospects.
[0137] (2) The metal catalyst provided by the present invention is used to catalyze ethylene homopolymerization, has excellent high-temperature catalytic performance, and can obtain polyethylene with high molecular weight and narrow molecular weight distribution. The metal catalyst is used to catalyze ethylene-octene copolymerization, has excellent catalytic performance and high catalytic activity, and can obtain ethylene-octene copolymer with high molecular weight, narrow molecular weight distribution, high octene insertion rate and excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0138] Figure 1 The H NMR spectrum of the ligand L1 provided in Preparation Example 2;
[0139] Figure 2 The H NMR spectrum of the ligand L5 provided in Preparation Example 6;
[0140] Figure 3 The H NMR spectrum of the metal catalyst Cat 1 provided in Example 1;
[0141] Figure 4 The nuclear magnetic hydrogen spectrum of the metal catalyst Cat 2 provided in Example 2;
[0142] Figure 5 This is the H-NMR spectrum of the metal catalyst Cat 5 provided in Example 5. DETAILED DESCRIPTION
[0143] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0144] In the following specific embodiments of the present invention, the materials, reagents, etc. used can all be conventional commercially available raw materials obtained from commercial channels.
[0145] In a specific embodiment, the metal catalyst is a Hf (hafnium) catalyst, which can be prepared by the following synthesis route:
[0146]
[0147] (1) synthesizing a naphthyl-containing pyridine imine Schiff base compound according to a known route;
[0148] (2) A heterocyclic metal compound (lithium salt or Grignard reagent) is added to a solution of a pyridine imine Schiff base compound (the solvent may be an ether solvent, such as tetrahydrofuran and / or diethyl ether) and monitored by thin layer chromatography (TLC). Generally, the pyridine imine Schiff base compound can be completely converted by overnight reaction. Sometimes, additional heterocyclic metal compounds are required, and finally the pyridine imine Schiff base compound can be completely converted. In this step, the target ligand can be obtained without column chromatography.
[0149] (3) The obtained ligand is dissolved in a solvent (such as toluene), hydrogen is abstracted with n-butyllithium n-BuLi, and then mixed with HfX4 (X represents a halogen, such as HfCl4), refluxed in the solvent, and then treated with a Grignard reagent to obtain the target metal catalyst.
[0150] The specific preparation method of the metal catalyst of the present invention will be described in detail below with multiple preparation examples and embodiments, but the preparation method of the present invention is not limited to these preparation examples and embodiments.
[0151] In the preparation examples and embodiments of the present invention, nuclear magnetic resonance spectroscopy ( 1 The product structure was characterized and confirmed by H NMR, and the deuterated solvent used was one of deuterated benzene (benzene-d6), deuterated dimethyl sulfoxide (DMSO-d6), and deuterated chloroform (CDCl3).
[0152] Preparation Example 1: Synthesis of Pyridineimine Schiff Base 6-(1-naphthyl)-2-((2,6-diisopropylphenyl)imino)pyridine (Compound A)
[0153]
[0154] 23.3 g (100 mmol) of compound 1 and 26.56 g (150 mmol) of compound 2 were dissolved in 100 mL of dry toluene. 20 mg of p-toluenesulfonic acid PTSA was added to the solution. The solution was heated to 90°C and reacted for 10 h to form a gray solution. The solution was restored to room temperature, toluene was concentrated, 50 mL of anhydrous ethanol was added and stirred for 2 h to form a slurry. 36 g of solid was obtained by filtration with a yield of 90%.
[0155] Structural characterization: 1 H NMR (500MHz, benzene-d6): δ8.63(s,1H),8.36(dd,J=7.7,1.2Hz,1H),8.30–8.22(m,1H),7.76–7.64(m,2H),7.58(d d,J=7.2,1.3Hz,1H),7.32–7.23(m,4H),7.22–7.07(m,4H),3.22(hept,J=6.9Hz,2H),1.18(d,J=6.9Hz,12H).
[0156] Preparation Example 2: Synthesis of 2-(N-(2,6-diisopropylphenylamino)-2-benzofuranylmethyl)-6-(1-naphthyl)-pyridine (ligand L1)
[0157]
[0158] Under nitrogen protection, 0.6g (5.08mmol) of benzofuran was dissolved in 20mL of dry anhydrous tetrahydrofuran (THF). Subsequently, the system was cooled to -78°C, and 3.2mL (5.08mmol) of n-butyl lithium (n-BuLi) was added dropwise at this temperature. After the addition was completed, the solution showed a bright yellow color and maintained at this temperature for 10min under continuous stirring. Subsequently, the system was gradually warmed to room temperature and continued to stir for 30min. The system was cooled to -78°C again. At this time, another 20mL dry anhydrous THF solution containing 1.99g (5.08mmol) of compound A was taken and slowly added dropwise to the previous benzofuran lithium salt solution at low temperature. During the addition, the color of the reaction solution became significantly darker. Subsequently, the system was warmed to room temperature again and stirred all night. TLC monitored the reaction progress. After the reaction was completed, 20mL of water was added to quench the reaction, and then 40mL of ethyl acetate (EA) was used for three extractions. The organic phases were combined, dried over anhydrous sodium sulfate, and then concentrated. Purification was performed by silica gel column chromatography (petroleum ether PE:EA=50:1) to obtain 1.3 g of product L1 with a yield of 50%.
[0159] The H NMR spectrum of ligand L1 is shown in Figure 1 As shown, 1 H NMR (500MHz, DMSO-d6): δ8.07–7.95(m,4H),7.70–7.56(m,5H),7.53–7.45(m,2H) ),7.27(td,J=8.2,7.7,1.5Hz,1H),7.24–7.18(m,1H),7.12(ddd,J=8.3,6.8,1. 4Hz,1H),7.04–6.93(m,3H),6.88(s,1H),5.50(d,J=10.5Hz,1H),5.17(d,J=10. 5Hz, 1H), 3.25 (hept, J = 6.8Hz, 2H), 0.99 (d, J = 6.7Hz, 6H), 0.95 (d, J = 6.7Hz, 6H).
[0160] Preparation Example 3: Synthesis of 2-(N-(2,6-diisopropylphenylamino)-2-benzothienylmethyl)-6-(1-naphthyl)-pyridine (ligand L2)
[0161]
[0162] Under nitrogen protection, 0.7g (5.22mmol) of benzothiophene was dissolved in 20mL of dry anhydrous tetrahydrofuran. The system was cooled to -78°C, and 3.3mL (5.22mmol) of n-butyl lithium was added dropwise at this temperature. After the addition was completed, the solution turned yellow and maintained at this temperature for 10min under continuous stirring. Then, the system was warmed to room temperature and continued to stir for 30min. After that, the system was cooled to -78°C again. At this time, another 20mL dry anhydrous THF solution containing 2.05g (5.22mmol) of compound A was taken and slowly added dropwise to the previous benzothiophene lithium salt solution under low temperature conditions. As the addition process proceeded, the color of the reaction solution gradually deepened. Subsequently, the system was warmed to room temperature again and stirred all night, and TLC (PE: EA = 5: 1) monitoring showed that the reaction was complete. 20mL of water was added to quench the reaction, and then 40mL of EA was used for three extractions. After the organic phases were combined, they were dried over anhydrous sodium sulfate, and then the solvent was concentrated. Finally, the product was purified by silica gel column chromatography (PE:EA=50:1) to obtain 1.18 g of product with a yield of 43%.
[0163] 1 H NMR (400MHz, benzene-d6): δ8.33(d,J=8.3Hz,1H),7.69-7.60(m,3H),7.50(d,J=8.0Hz,1H),7.44(d,J=7.9Hz,1H),7.29(dd,J=8.3,7.1Hz,1H),7.24- 6.99(m,10H),6.83(dd,J=7.5,1.3Hz,1H),5.72(d,J=9.7Hz,1H),5.38(d,J=9.9Hz,1H),3.53(sept,J=6.8Hz,2H),1.07(dd,J=8.0,6.8Hz,12H).
[0164] Preparation Example 4: Synthesis of 2-(N-(2,6-diisopropylphenylamino)-3-benzothienylmethyl)-6-(1-naphthyl)-pyridine (ligand L3)
[0165]
[0166] 0.97g (4.55mmol) of 3-bromobenzothiophene was dissolved in 20mL of ether and placed in a 100mL reaction bottle in a glove box. At -78°C, 2mL (2.4M, 4.77mmol) of n-butyl lithium was slowly added dropwise and the temperature was maintained for 1h. 1.5g (3.82mmol) of compound A was dissolved in ether and added dropwise to the above lithium salt solution. The temperature was slowly raised to -50°C for 0.5h, then raised to -20°C for 0.5h, and finally reacted at room temperature for 12h. The reaction progress was monitored by TLC to ensure that compound A was completely reacted. Water was added to quench the reaction, the aqueous phase was separated, the organic phase was extracted with ethyl acetate, dried and concentrated. The product was separated by column chromatography, using petroleum ether and ethyl acetate (PE:EA=100:1) as eluents to obtain a total of 1.1g of ligand L3 with a yield of 55%.
[0167] 1 H NMR (500MHz, CDCl3): δ7.95–7.81(m,3H),7.75–7.71(m,2H),7.64(dd,J=8.6,1.1Hz,1H ),7.52(q,J=3.7Hz,2H),7.47–7.38(m,3H),7.31(ddd,J=14.7,6.8,1.1Hz,2H),7.21(dd d,J=8.1,7.0,1.1Hz,1H),7.11(ddd,J=8.4,6.7,1.4Hz,1H),7.04(s,3H),5.53(d,J=9.1 Hz, 1H), 4.61 (d, J = 9.2Hz, 1H), 3.00 (sept, J = 6.9Hz, 2H), 0.97 (dd, J = 27.5, 6.8Hz, 12H).
[0168] Preparation Example 5: Synthesis of 2-(N-(2,6-diisopropylphenylamino)-3-bromo-2-thienylmethyl)-6-(1-naphthyl)-pyridine (ligand L4)
[0169]
[0170] Weigh 1.1 g (4.54 mmol) of 2,3-dibromothiophene in a 100 mL reaction bottle and dissolve it in 20 mL of ether. At -78 ° C, add 1.9 mL (2.4 M, 4.54 mmol) of n-butyl lithium dropwise, and maintain the temperature for 1 hour. Dissolve 1.5 g (3.82 mmol) of compound A in ether and add it dropwise to the lithium salt. Then gradually increase the temperature, react at -50 ° C for 0.5 h, then increase the temperature to -20 ° C for 0.5 h, and react at room temperature for 12 h. Monitor the reaction using a TLC spot plate to ensure that there is no residual raw material. Add water to quench the reaction, extract the organic phase with ethyl acetate, dry and concentrate. The product is separated by column chromatography, using petroleum ether and ethyl acetate (PE: EA = 100: 1) as eluents to obtain a total of 31.2 g of the target product L4 with a yield of 56%.
[0171] 1 H NMR (500MHz, CDCl3): δ8.14-8.09(m,1H),7.96-7.89(m,2H),7.72(t,J=7.7Hz,1H),7.65(dd,J= 7.0,1.3Hz,1H),7.58(dd,J=8.1,7.1Hz,1H),7.53-7.46(m,2H),7.41(ddd,J=8.3,6.7,1.4Hz,1 H),7.34(dd,J=7.7,1.0Hz,1H),7.27-7.25(m,1H),7.06-6.98(m,3H),6.93(d,J=5.3Hz,1H),5. 57(s,1H),5.07(s,1H),3.12(hept,J=6.8Hz,2H),1.10(d,J=6.9Hz,6H),0.94(d,J=6.7Hz,6H).
[0172] Preparation Example 6: Synthesis of 2-(N-(2,6-diisopropylphenylamino)-3-bromo-2-benzothienylmethyl)-6-(1-naphthyl)-pyridine (ligand L5)
[0173]
[0174] 0.64 g (3 mmol) of 3-bromobenzothiophene was dissolved in 20 mL of dry anhydrous tetrahydrofuran under nitrogen atmosphere, and the mixture was cooled to -78 °C in this atmosphere. 3 mL (3 mmol) of tetrahydrofuran solution of lithium bis(trimethylsilyl)amide LiHMDS was added dropwise at this temperature. After the addition was completed, a yellow solution was formed and stirred at this temperature for 10 min. The mixture was then heated to room temperature and stirred for 30 min. The mixture was cooled to -78 °C and another 20 mL of dry anhydrous tetrahydrofuran was dissolved in 1% ethanol. 1.18 g (3 mmol) of compound A was dissolved and added dropwise to the 3-bromobenzothiophene lithium salt solution at low temperature. The color of the reaction solution turned dark, and then the temperature was raised to room temperature and stirred overnight. TLC (PE:EA=5:1) was used to monitor the progress of the reaction. After the reaction was completed, 20 mL of water was added to quench the reaction. EA (40 mL×3 times) was used for extraction. The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was concentrated. After silica gel column chromatography (PE:EA=50:1), 0.7 g of ligand L5 was obtained with a yield of 38.48%.
[0175] The H NMR spectrum of ligand L5 is shown in Figure 2 As shown, 1 H NMR (500MHz, benzene-d6): δ8.24 (d, J = 8.5 Hz, 1H), 7.72 (d, J = 8.0 Hz, 1H), 7.67-7. 63(m,2H),7.61(dd,J=7.1,1.2Hz,1H),7.40-7.22(m,4H),7.13-7.02(m,7H) ,6.95(ddd,J=8.2,7.1,1.2Hz,1H),5.95(d,J=9.0Hz,1H),5.57(d,J=9.0Hz, 1H), 3.43 (sept, J=6.8Hz, 2H), 1.10 (d, J=6.8Hz, 6H), 1.04 (d, J=6.8Hz, 6H).
[0176] Preparation Example 7: Synthesis of 2-(N-(2,6-diisopropylphenylamino)-3-(2-methoxyphenyl)-2-thienylmethyl)-6-(1-naphthyl)-pyridine (ligand L6)
[0177]
[0178] Under nitrogen atmosphere, 2-methoxyphenylboronic acid (0.15 g, 0.98 mmol), ligand L4 (0.5 g, 0.89 mmol), potassium carbonate (0.24 g, 2 eq.), tetrakis(triphenylphosphine)palladium Pd(PPh3)4 (0.05 g, 0.05 eq.) were weighed into a 250 mL reaction bottle, and 50 mL toluene, 20 mL ethanol, and 10 mL water were added. The reaction was carried out at 85°C for 12 h. The reaction was monitored by TLC, the system was concentrated, ethyl acetate was added for separation, the organic phase was dried, concentrated, and separated by column chromatography (PE:EA=50:1) to obtain 140 mg of ligand L6 with a yield of 27%.
[0179] 1 H NMR (500MHz, CDCl3): δ8.08(d,J=8.6Hz,1H),7.94-7.87(m,2H),7.61(dd,J=7.1,1.4Hz,1H),7.56( dd,J=8.1,7.1Hz,1H),7.49(ddd,J=8.1,6.7,1.2Hz,1H),7.45-7.36(m,2H),7.34-7.29(m,2H),7.1 8(ddd,J=8.9,6.7,2.5Hz,1H),7.01-6.90(m,4H),6.78-6.66(m,4H),5.34(d,J=9.8Hz,1H),4.65(d ,J=9.8Hz,1H),3.56(s,3H),3.09(sept,J=6.8Hz,2H),1.00(d,J=6.8Hz,6H),0.82(d,J=6.8Hz,6H).
[0180] Preparation Example 8: Synthesis of 2-(N-(2,6-diisopropylphenylamino)-3-phenyl-5-methyl-2-thienylmethyl)-6-(1-naphthyl)-pyridine (ligand L7)
[0181]
[0182] Under nitrogen atmosphere, weigh phenylboronic acid (6.8 g, 55.76 mmol), 2-methyl-4-bromothiophene (9 g, 50.83 mmol), potassium carbonate (7 g, 2 eq.), tetrakis(triphenylphosphine)palladium (2.93 g, 0.05 eq.) in a 500 mL reaction bottle, add 150 mL toluene, 60 mL ethanol, 30 mL water. React at 85 ° C for 12 h. Monitor the reaction by TLC, concentrate the system, extract with ethyl acetate, dry the organic phase, concentrate, and separate by column chromatography (PE: EA = 50: 1) to obtain 2-methyl-4-bromothiophene (6.6 g, yield 75%).
[0183] 1H NMR (500MHz, CDCl3): δ7.54-7.45(m,2H),7.39-7.25(m,2H),7.22-7.15(m,1H),7.11(d,J=1.5Hz,1H),6.98(s,1H),2.45(s,3H).
[0184] Ligand L7 was prepared in the same manner as ligand L2, except that an equal molar amount of 2-methyl-4-phenylthiophene was used to replace benzothiophene. The yield of ligand L7 was 42%.
[0185] 1 H NMR (500MHz, CDCl3): δ8.20(d,J=8.5Hz,1H),7.96–7.89(m,2H),7.68(dd,J=7.0,1.3Hz,1H),7 .58(td,J=7.9,4.4Hz,2H),7.52(ddd,J=8.2,6.7,1.3Hz,1H),7.48–7.37(m,3H),7.20(dd,J=5 .0,1.9Hz,2H),7.02–6.88(m,6H),6.60(d,J=1.3Hz,1H),5.39(d,J=9.1Hz,1H),4.65(d,J=9.1 Hz,1H),3.24–3.07(m,2H),2.50(d,J=1.1Hz,3H),0.93(d,J=6.8Hz,6H),0.85(d,J=6.7Hz,6H).
[0186] Example 1
[0187] Metal catalyst Cat 1, structure: The preparation method is as follows:
[0188]
[0189] Under nitrogen protection, 0.6g (1.17mmol) of ligand L1 was dissolved in toluene solvent. At 0°C, 0.77mL (1.23mmol, 1.05eq.) of n-butyl lithium was added thereto and the reaction was continued for 2h. After the solvent was drained, it was washed several times with n-hexane and then drained again. The treated product was mixed with 0.394g (1.23mol) of hafnium tetrachloride and reacted at 120°C for 5.5h. After the reaction was completed, it was cooled to room temperature, 3.3 equivalents of MeMgBr were added thereto, and the reaction was continued at room temperature overnight. The volatiles were drained and the product was extracted with toluene. The filtrate was drained and washed several times with n-hexane to obtain 0.4g of the target product with a yield of 47.5%.
[0190] The H NMR spectrum of metal catalyst Cat 1 is as follows Figure 3As shown, 1 H NMR (500MHz, benzene-d6): δ8.57(d,J=7.6Hz,1H),8.20–8.06(m,1H),7.81(d,J=7.6Hz,1H),7.75–7.65(m,1H),7.44(d,J=8.0Hz,1H),7.31 –7.26(m,3H),7.23–7.18(m,2H),7.17(d,J=1.6Hz,1H),7.12(dd,J=7.4,2.1Hz,1H),7.03(td,J=7.5,1.0Hz,1H),6.95(ddd,J=8.4,7 .2,1.4Hz,1H),6.81(t,J=7.9Hz,1H),6.53(d,J=7.6Hz,1H),6.04(s,1H),5.98(d,J=0.9Hz,1H),4.04(sept,J=6.8Hz,1H),3.28(sep t,J=6.8Hz,1H),1.41(d,J=6.8Hz,3H),1.35(d,J=6.8Hz,3H),1.16(d,J=6.8Hz,3H),1.09(s,3H),0.69(s,3H),0.51(d,J=6.7Hz,3H).
[0191] Example 2
[0192] Metal catalyst Cat 2, structure: The preparation method thereof is different from that of Example 1 only in that the ligand L1 is replaced by an equivalent amount of L2, and other materials, amounts and processes are the same as those of Example 1, to obtain a metal catalyst Cat 2.
[0193]
[0194] The H NMR spectrum of the metal catalyst Cat 2 is shown in Figure 4 As shown, 1H NMR (500MHz, benzene-d6): δ8.56(d,J=7.7Hz,1H), 8.19(d,J=7.6Hz,1H), 7.81(d,J=7.7Hz,1H), 7.75–7.68(m,1H), 7.49(d,J=8.0Hz,1H),7.39(dd,J=8.0,4.9Hz,3H),7.31–7.27(m,4H),6.99(dt,J=12.4,5.6Hz,2H),6.86(t, J=7.8Hz,1H),6.67(s,1H),6.56(d,J=7.8Hz,1H),6.28(s,1H),4.27(sept,J=6.9Hz,1H),3.25(sept,J=6.8H z,1H),1.41(dd,J=10.0,6.8Hz,6H),1.16(d,J=6.7Hz,3H),1.09(s,3H),0.68(s,3H),0.52(d,J=6.7Hz,3H).
[0195] Example 3
[0196] Metal catalyst Cat 3, structure: The preparation method thereof is different from that of Example 1 only in that the ligand L1 is replaced by an equivalent amount of L3, and other materials, amounts and processes are the same as those of Example 1, to obtain a metal catalyst Cat 3.
[0197]
[0198] 1 H NMR (500MHz, benzene-d6): δ7.61(dd,J=7.1,1.2Hz,1H),7.48–7.43(m,3H),7.37(dd,J =7.6Hz,1H),7.23(d,J=8.1Hz,2H),7.14–6.98(m,3H),6.93–6.82(m,3H),6.80– 6.65(m,4H),4.23(sept,J=6.7Hz,1H),3.93(sept,J=6.8Hz,1H),1.81(d,J=6.6 Hz,3H),1.67(t,J=7.0Hz,6H),0.97(s,3H),0.33(d,J=6.8Hz,3H),-2.75(s,3H).
[0199] Example 4
[0200] Metal catalyst Cat 4, structure: The preparation method thereof is different from that of Example 1 only in that the ligand L1 is replaced by an equivalent amount of L4, and other materials, amounts and processes are the same as those of Example 1, to obtain a metal catalyst Cat 4.
[0201]
[0202] 1 H NMR (500MHz, benzene-d6): δ8.60(d,J=7.8,1H),8.13(d,J=7.8,1H),7.90-7.87(m,2H),7.76(d,J=7.5Hz,1H),7.72 –7.68(m,1H),7.68–7.65(d,J=8.1Hz,1H),7.57-7.45(m,2H),7.43-7.40(m,2H),7.16-7.00(m,1H),6.9(t,J =7.8Hz,1H),6.6(d,J=7.8Hz,1H),6.35(s,1H),3.85(sept,J=6.9Hz,1H),3.10(sept,J=6.9Hz,1H),1.35(d, J=6.9Hz,3H),1.33(d,J=6.8Hz,3H),1.17(d,J=6.8Hz,3H),1.11(s,3H),0.80(s,3H),0.54(d,J=6.8Hz,3H).
[0203] Example 5
[0204] Metal catalyst Cat 5, structure: The preparation method thereof is different from that of Example 1 only in that the ligand L1 is replaced by an equimolar amount of L5, and the other materials, amounts and processes are the same as those of Example 1, to obtain a metal catalyst Cat 5.
[0205]
[0206] The nuclear magnetic hydrogen spectrum of metal catalyst Cat 5 is as follows Figure 5 As shown, 1H NMR (500MHz, benzene-d6): δ8.56(d,J=7.7Hz,1H),8.20(d,J=7.9Hz,1H),7.81(d,J=7.6Hz,1H),7 .72(d,J=7.5Hz,1H),7.66(d,J=8.1Hz,1H),7.51(d,J=7.9Hz,1H),7.29(br,3H),7.04–6.8 0(m,6H),6.66(d,J=13.9Hz,1H),6.29(s,1H),4.22(br,1H),3.32(br,1H),1.55(d,J=6.7H z,3H),1.39(d,J=7.1Hz,3H),1.18(d,J=6.9Hz,3H),1.09(s,3H),0.70(s,3H),0.47(s,3H).
[0207] Example 6
[0208] Metal catalyst Cat 6, structure: The preparation method thereof is different from that of Example 1 only in that the ligand L1 is replaced by an equivalent amount of L6, and other materials, amounts and processes are the same as those of Example 1, to obtain a metal catalyst Cat 6.
[0209]
[0210] 1 H NMR (500MHz, benzene-d6): δ8.48(d,J=7.8,1H),8.00(d,J=7.8,1H),7.86-7.74(m,3H),7.72–7.60(m,2H) ),7.55–7.45(m,2H),7.43-7.40(m,3H),7.28–7.02(m,3H),6.96-6.90(m,2H),6.68(d,J=7.8Hz,1H ),6.40(s,1H),3.88(s,3H),3.63(sept,J=6.8Hz,1H),3.08(sept,J=6.8Hz,1H),1.40(d,J=6.9Hz, 3H),1.39(d,J=6.8Hz,3H),1.13(d,J=6.8Hz,3H),1.12(s,3H),0.65(s,3H),0.60(d,J=6.8Hz,3H).
[0211] Example 7
[0212] Metal catalyst Cat 7, structure: The preparation method thereof is different from that of Example 1 only in that the ligand L1 is replaced by an equivalent amount of L7, and other materials, amounts and processes are the same as those of Example 1, to obtain a metal catalyst Cat 7.
[0213]
[0214] 1 H NMR (500MHz, benzene-d6): δ8.62(d,J=7.8,1H),8.20(d,J=7.8,1H),7.66-7.60(m,5H),7.55(d, J=7.8Hz,2H),7.48-7.46(m,2H),7.32(d,J=7.8Hz,2H),7.30–6.99(m,5H),6.30(s,1H),3. 64(sept,J=6.8Hz,1H),3.44(sept,J=6.8Hz,1H),2.58(s,2H),1.30(d,J=6.9Hz,3H),1.2 6(d,J=6.8Hz,3H),1.25(d,J=6.8Hz,3H),1.20(s,3H),0.48(s,3H),0.38(d,J=6.8Hz,3H).
[0215] The application of the metal catalyst of the present invention in catalyzing olefin polymerization will be described in detail below with multiple application examples, but the application of the metal catalyst of the present invention is not limited to these application examples.
[0216] In the following specific embodiments of the present invention, the main testing methods for polymers are as follows:
[0217] (1) Molecular weight (weight average molecular weight M w , number average molecular weight M n ), molecular weight distribution index (PDI, M w / M n ) was obtained by high temperature gel permeation chromatography (GPC), specifically by measuring on a PL-GPC 220 gel permeation chromatography instrument at 150°C with 1,2,4-trichlorobenzene as the mobile phase.
[0218] (2) Comonomer insertion rate: measured by high temperature H NMR spectroscopy 1 The H NMR test was performed at high temperature on a Bruker AV400 nuclear magnetic resonance instrument with deuterated 1,1,2,2-tetrachloroethane as solvent at 125°C and 400 MHz.
[0219] (3) Melting temperature of polymer (T m): measured on a TA company Q2000 differential scanning calorimeter (DSC) instrument, the scanning temperature range is 40-170 ° C, the heating rate is 10 ° C / min, and the second heating temperature is taken as the melting point T m .
[0220] (4) Catalytic activity: calculated according to the following formula: Catalytic activity = polymer mass / (molar amount of metal catalyst × polymerization time).
[0221] Application Example 1
[0222] The present invention provides an application of the metal catalyst Cat 1 in ethylene homopolymerization, specifically, a method for preparing polyethylene, which is as follows:
[0223] 2 μmol of metal catalyst Cat 1 was used to catalyze the homopolymerization of ethylene, with 1.2 equivalents of boron salt triphenylcarbonium tetrakis(pentafluorophenyl)boron (CPh3) (B(C6F5)4) as an activator and 50 equivalents of triisobutylaluminum TIBA as an impurity scavenger; first, TIBA was mixed with 100 mL of solvent Isopar E in a glove box and put into a glass reactor, and then the glove box was removed and connected to an ethylene pipeline. Catalyst Cat 1 and boron salt were dissolved and mixed with toluene respectively, added to the reactor under ethylene atmosphere, the ethylene pressure was set to 8 bar, the temperature was set to 110°C, and the reaction was carried out under magnetic stirring for 5 min. After the reaction, the reaction mixture was poured into 200 mL of ethanol for precipitation, filtered, and dried to obtain 3.74 g of polymer, and the molecular weight, molecular weight distribution, melting point and catalytic activity of the polymer are shown in Table 1.
[0224] Application Example 2-6
[0225] The present invention provides an application of a metal catalyst in ethylene homopolymerization, specifically, a method for preparing polyethylene, which is different from Application Example 1 in that the metal catalyst (main catalyst) and the polymerization temperature are as shown in Table 1; the materials and parameters not shown in Table 1 are the same as those in Application Example 1; the molecular weight, molecular weight distribution, melting point and catalytic activity of the polymer are as shown in Table 1.
[0226] Comparative Example 1-2: The only difference from Application Example 1 is that the main catalyst is the catalyst CatiPr
[0227]
[0228] Table 1
[0229]
[0230] Application Example 7
[0231] The present invention provides an application of the metal catalyst Cat 1 in the copolymerization of ethylene and 1-octene, specifically, a method for preparing an ethylene-octene copolymer, which is as follows:
[0232] 2 μmol of metal catalyst Cat 1 was used to catalyze the copolymerization of ethylene and 1-octene, 1.2 equivalents of boron salt (CPh3) (B(C6F5)4) as an activator, and 100 equivalents of triisobutylaluminum TIBA as an impurity scavenger. TIBA, 100 mL of solvent Isopar E and 3 mL of 1-octene were mixed in a glove box, put into a glass reactor, and the glove box was removed to connect the ethylene pipeline. Catalyst Cat 1 and boron salt were dissolved and mixed with toluene respectively, added to the reactor under ethylene atmosphere, the ethylene pressure was set to 8 bar, the temperature was set to 130 ° C, and the reaction was carried out under magnetic stirring for 5 minutes. After the reaction, the reaction mixture was poured into 200 mL of ethanol for precipitation, filtered, and dried to obtain 4.12 g of polymer, and its test data are shown in Table 2.
[0233] Application Example 8-13
[0234] The present invention provides an application of a metal catalyst in the copolymerization of ethylene and 1-octene, specifically, a method for preparing an ethylene-octene copolymer, which differs from Application Example 7 in that the metal catalyst (main catalyst) is as shown in Table 2; the materials and parameters not shown in Table 2 are the same as those in Application Example 7; and the test data of the polymerization product are as shown in Table 2.
[0235] Comparative Example 3: The only difference from Application Example 7 is that the main catalyst is the catalyst CatiPr produced by Dow Chemical Company.
[0236] Table 2
[0237]
[0238] According to the data in Table 1 and Table 2, the non-metallocene catalyst provided by the present invention has excellent thermal stability, and can obtain olefin polymers with large molecular weight, narrow molecular weight distribution and high comonomer insertion rate in the reaction of catalyzing ethylene polymerization and copolymerization of ethylene and 1-octene. In particular, under high temperature reaction conditions, the catalytic activity, molecular weight, molecular weight distribution and insertion rate of the metal catalyst provided by the present invention are significantly better than those of the existing hafnium pyridylamine catalyst. Moreover, the heterocycle in the metal catalyst of the present invention has good modifiability, which is conducive to further improvement of the catalyst structure and has good application value.
[0239] The applicant declares that the present invention illustrates the metal catalyst, catalyst composition and application of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A metal catalyst, It is characterized in that The metal catalyst has a structure as shown in Formula I: Among them, the structure of Ar is represents the attachment site of the group, and the dashed arc represents the conjugated double bond; D 1 , D 2 , D 3 Each independently selected from O, S, N, NR A1 or CR A2 Any of the following, not all of which are CR A2 ; D 4 Select from N or CR A3 Any of the following; R A1 , R A2 , R A3 , R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , R 10 , R 11 Each is independently selected from any one of hydrogen, halogen, substituted or unsubstituted C1-C30 straight or branched alkyl, substituted or unsubstituted C1-C30 alkoxy, substituted or unsubstituted C3-C30 cycloalkyl, substituted or unsubstituted C6-C30 aryl, substituted or unsubstituted C3-C30 heteroaryl, C1-C30 alkylsilyl, and C1-C30 alkoxysilyl; R A2 , R A3 , R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 Any two adjacent groups are not connected or connected to form a ring through a chemical bond; X 1 , X 2 Each is independently selected from any one of halogen, C1-C30 straight or branched alkyl, C6-C30 aryl, C7-C30 arylalkyl, C1-C30 alkylamino, and C6-C30 arylamino; M is selected from any one of Group IVB metals; The substituted substituents are each independently selected from at least one of halogen, unsubstituted or R'-substituted C1-C10 straight or branched alkyl, unsubstituted or R'-substituted C1-C10 alkoxy, and unsubstituted or R'-substituted C2-C10 alkenyl; R' is each independently selected from at least one of halogen and C6-C12 aryl.
2. The metal catalyst according to claim 1, It is characterized in that The metal catalyst has a structure as shown in Formula II: Among them, Ar, R 1 , R 2 , R 3 , R 4 , R 5 , R 10 , R 11 , X 1 , X 2 , M have the same defined ranges as in Formula I.
3. The metal catalyst according to claim 1 or 2, It is characterized in that The R 1 , R 5 Each independently selected from any one of C1-C10 straight chain or branched chain alkyl, more preferably C1-C6 straight chain or branched chain alkyl; Preferably, the R 2 , R 4 , R 10 and R 11 is hydrogen; Preferably, the metal catalyst has a structure as shown in Formula III: Among them, Ar, R 3 , X 1 , X 2 , M has the same defined range as in Formula I; Preferably, the R 3 Any one selected from hydrogen, halogen, C1-C10 straight or branched alkyl, C1-C10 alkoxy.
4. The metal catalyst according to any one of claims 1 to 3, It is characterized in that The structure of Ar is The attachment site of the representative group; D 1 Selected from O, S or NR A1 Any of the following; R A1 Any one selected from hydrogen, halogen, substituted or unsubstituted C1-C30 straight or branched alkyl, substituted or unsubstituted C1-C30 alkoxy, substituted or unsubstituted C3-C30 cycloalkyl, substituted or unsubstituted C6-C30 aryl, substituted or unsubstituted C3-C30 heteroaryl, C1-C30 alkylsilyl, C1-C30 alkoxysilyl, further preferably any one selected from hydrogen, substituted or unsubstituted C1-C10 straight or branched alkyl, substituted or unsubstituted C6-C20 aryl; R A Each is independently selected from any one of halogen, substituted or unsubstituted C1-C30 straight or branched alkyl, substituted or unsubstituted C1-C30 alkoxy, substituted or unsubstituted C3-C30 cycloalkyl, substituted or unsubstituted C6-C30 aryl, substituted or unsubstituted C3-C30 heteroaryl, C1-C30 alkylsilyl, and C1-C30 alkoxysilyl; any two adjacent R A They are not connected to each other or connected to form a ring through chemical bonds; The substituted substituents are each independently selected from at least one of halogen, unsubstituted or R'-substituted C1-C10 straight or branched alkyl, unsubstituted or R'-substituted alkoxy, and unsubstituted or R'-substituted C2-C10 alkenyl; R' is each independently selected from at least one of halogen and C6-C12 aryl; n is an integer selected from 0 to 4; Preferably, Ar is selected from any one of the following groups: Among them, R A4 , R A5 , R A6 Each is independently selected from any one of hydrogen, halogen, substituted or unsubstituted C1-C30 straight or branched alkyl, substituted or unsubstituted C1-C30 alkoxy, substituted or unsubstituted C3-C30 cycloalkyl, substituted or unsubstituted C6-C30 aryl, substituted or unsubstituted C3-C30 heteroaryl, C1-C30 alkylsilyl, and C1-C30 alkoxysilyl, and is further preferably any one of hydrogen, halogen, substituted or unsubstituted C1-C10 straight or branched alkyl, substituted or unsubstituted C1-C10 alkoxy, and substituted or unsubstituted C6-C20 aryl; Further preferably, Ar is selected from any one of the following groups: in, The attachment site of the representative group; R A1 Each is independently selected from any one of hydrogen, substituted or unsubstituted C1-C10 straight or branched alkyl, and substituted or unsubstituted C6-C20 aryl; R A4 , R A5 Each is independently selected from any one of hydrogen, halogen, substituted or unsubstituted C1-C10 straight or branched alkyl, substituted or unsubstituted C1-C10 alkoxy, substituted or unsubstituted C6-C20 aryl, more preferably hydrogen, halogen, unsubstituted or halogenated C1-C6 straight or branched alkyl, unsubstituted or halogenated C1-C6 alkoxy, phenyl, Any one of .
5. The metal catalyst according to any one of claims 1 to 4, It is characterized in that The M is selected from any one of titanium, zirconium and hafnium, and hafnium is more preferred; Preferably, the metal catalyst has any one of the following structures: Preferably, the X 1 , X 2 Each is independently selected from any one of halogen, C1-C10 straight or branched alkyl, benzyl, C1-C10 alkylamino, and C6-C20 arylamino, and more preferably any one of halogen, methyl, benzyl, and dimethylamino.
6. A method for preparing the metal catalyst according to any one of claims 1 to 5, It is characterized in that The preparation method comprises the following steps: (1) A heterocyclic metal compound of the structure represented by formula A reacts with a pyridine imine Schiff base compound of the structure represented by formula B to obtain a pyridine amine ligand of the structure represented by formula C. The reaction formula is as follows: Among them, Ar, R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , R 10 , R 11 , X 1 , X 2 and M have the same defined ranges as in Formula I; Y is selected from any one of Li or Mg-Hal, and Hal is selected from any one of halogens; (2) After the pyridylamine ligand undergoes a first reaction with a hydrogen abstraction reagent, it undergoes a second reaction with a metal M source to obtain the metal catalyst having a structure as shown in Formula I.
7. The preparation method according to claim 6, It is characterized in that The preparation method of the heterocyclic metal compound comprises: reacting a heterocyclic compound having a structure shown in Formula AS with a lithium reagent or metal magnesium to obtain the heterocyclic metal compound having a structure shown in Formula A, and the reaction formula is as follows: Among them, Y 2 Any one selected from hydrogen or halogen; Preferably, the hydrogen abstraction reagent includes any one of potassium hydride, sodium hydride, lithium hydride, lithium bistrimethylsilylamide, sodium bistrimethylsilylamide, lithium diisopropylamide, and C1-C6 alkyl lithium, or a combination of at least two thereof.
8. A catalyst composition, It is characterized in that The catalyst composition comprises a main catalyst and a co-catalyst, wherein the main catalyst comprises at least one of the metal catalysts according to any one of claims 1 to 5; Preferably, the co-catalyst comprises any one or a combination of at least two of an alkyl aluminum compound, an organic aluminum oxide compound, and a boron salt; Preferably, the alkyl aluminum compound includes any one of trimethyl aluminum, triethyl aluminum, triisobutyl aluminum, tri-n-hexyl aluminum, and trioctyl aluminum, or a combination of at least two thereof; Preferably, the organoaluminum oxide compound comprises any one or a combination of at least two of methylaluminoxane, ethylaluminoxane, isobutylaluminoxane, and alkylaluminum-modified methylaluminoxane; Preferably, the boron salt includes any one of tris(pentafluorophenyl)boron, triphenylcarbonium tetra(pentafluorophenyl)boron, tetra(pentafluorophenyl)boric acid-methyldi-(octadecyl)ammonium salt, and N,N-dimethylanilinium tetra(pentafluorophenyl)borate, or a combination of at least two thereof; Preferably, the molar ratio of the metal Al in the co-catalyst to the metal M in the main catalyst is (10-5000):1, more preferably (50-1000):1; Preferably, the molar ratio of the B element in the co-catalyst to the metal M in the main catalyst is (1-2):
1.
9. Use of the metal catalyst according to any one of claims 1 to 5 and the catalyst composition according to claim 8 in catalyzing olefin polymerization; Preferably, the olefin polymerization includes olefin homopolymerization or ethylene / α-olefin copolymerization.
10. A method for preparing polyolefin, It is characterized in that The preparation method comprises: carrying out polymerization reaction of olefin monomers in the presence of a catalyst to obtain the polyolefin; The catalyst comprises at least one of the metal catalyst according to any one of claims 1 to 5 and the catalyst composition according to claim 8; Preferably, the olefin monomers include ethylene and / or α-olefins; Preferably, the polymerization reaction is carried out in the presence of an organic solvent; Preferably, the polymerization reaction temperature is 0-200°C, more preferably 100-160°C; Preferably, the polymerization reaction pressure is 0.1-10 MPa, more preferably 0.5-5 MPa.
Citation Information
Patent Citations
Catalyst composition comprising novel transition metal compound
CN107849166A
Metal catalyst as well as preparation method and application thereof
CN117777183A
Ligand compound and transition metal compound
KR1020160131707A
Method for preparing ligand compound and transition metal compound
KR1020160131708A